CN102021848A CN 201010596769 CN201010596769A CN102021848A CN 102021848 A CN102021848 A CN 102021848A CN 201010596769 CN201010596769 CN 201010596769 CN 201010596769 A CN201010596769 A CN 201010596769A CN 102021848 A CN102021848 A CN 102021848A
Authority
CN
China
Prior art keywords
add
volumetric concentration
cotton textiles
lotion
look
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN 201010596769
Other languages
Chinese (zh)
Inventor
门雅静
刘显高
李秀兰
赵红玉
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
SUNVIM GROUP CO Ltd
Original Assignee
SUNVIM GROUP CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by SUNVIM GROUP CO Ltd filed Critical SUNVIM GROUP CO Ltd
Priority to CN 201010596769 priority Critical patent/CN102021848A/en
Publication of CN102021848A publication Critical patent/CN102021848A/en
Pending legal-status Critical Current

Links

Abstract

The invention discloses a method for producing color spinning cotton textiles, comprising the following steps: refining hemp fiber and cotton fiber; carrying out an acid cleaning step and a deoxidation step; adding yellow reactive dye and red reactive dye for treating for 5-10 minutes at the temperature of 40-50 DEG C based on the liquor ratio of (1:6)-10; adding 8-12g/L of anhydrous sodium sulphate into the bath lotion for treating for 5-15 minutes, adding 6-8g/L of calcined soda into the bath lotion; heating until the temperature reaches 55-60 DEG C; dyeing for 20-40 minutes; blending the dyed hemp fiber and the cotton fiber into yarns; warping, sizing and weaving the yarns into gray fabrics; and postprocessing the gray fabrics to obtain the color spinning cotton textile. The method provided by the invention is environmental-friendly; no pollution is caused; the finished product is harmless to human bodies, and has high color firmness; the prepared spinning product presents natural and fashionable color; and the woven fabric has hazy stereo effect, and is simple and reliable.

Description

A kind ofly produce the method that look spins numb cotton textiles
Technical field
The present invention relates to textile technology field, relate in particular to a kind of method that look spins numb cotton textiles of producing.
Background technology
In recent years, along with the raising of people's quality of life, pursue the environmental protection and the fashion of recovering one's original simplicity and day by day rise, Chinese fiber crops more and more are subjected to liking of consumers in general as the environmental protection ecological fiber.China-hemp fibers is rare your textile fabric of typical functions type, environment-friendly type, is acknowledged as " king of natural fabric ", has characteristics such as moisture absorption, ventilative, pleasant, heat radiation, mildew-resistant, antibacterial, radioresistance.In China, historical existing more than 8000 year of the plantation of Chinese fiber crops.The large tracts of land popularizing planting is alleviated Chinese fiber present situation in short supply effectively, and for solving the new road that the agriculture, rural areas and farmers problem is broken a high added value, its good characteristic also will bring revolutionary variation.
The production technology of existing numb cotton textiles mainly is to adopt cheese dyeing, exists following shortcoming: 1, Chinese fiber crops are different with the requirement of cotton dyeing processing in the cotton finished product dyeing course of Chinese fiber crops; 2, uneven dyeing; 3, the dyeing COLOR FASTNESS is low; The product color dimness of 4, making can't get a desired effect.
Summary of the invention
Technical problem to be solved by this invention provides that a kind of environmental protection is pollution-free, COLOR FASTNESS is high, color is natural, the production look of fashion spins the method for numb cotton textiles.
For solving the problems of the technologies described above, technical scheme of the present invention is: with china-hemp fibers and cotton fiber refining after acid pickling step and deoxygenation step, then by bath raio 1: 6~10, in the time of 40~50 ℃, after adding yellow REACTIVE DYES and red REACTIVE DYES processing 5~10min, add glauber salt, glauber salt 8~12g/L in the body lotion, handle 5~15min, add soda ash afterwards, soda ash 6~8g/L in the body lotion is warming up to 55~60 ℃ then, dyeing 20~40min, and the china-hemp fibers after will dyeing blending becomes yarn with cotton fiber; Then the yarn that described blending is become through warping, sizing, weave step and be made into grey cloth; Afterwards described grey cloth being carried out post processing obtains described look and spins numb cotton textiles.
As optimized technical scheme, described yellow REACTIVE DYES is yellow C-RG 0.12wt%, and red REACTIVE DYES is red C-2BL 0.06wt%.
As optimized technical scheme, described refining is to be 1: 6~10 by bath raio, 50~60 ℃ of temperature, in body lotion, add emulsifying agent, refining agent, handle 20~40min, add chelated dispersants, stabilizing agent, caustic soda, hydrogen peroxide again, be warming up to 85~95 ℃, handle 40~60min, remove the impurity on the fiber.
As optimized technical scheme, emulsifying agent described in the body lotion is an isomery alcohol polyoxyethylene ether, and volumetric concentration is 1.0~1.5ml/L; Described refining agent is refining agent CZ-4, and volumetric concentration is 0.5ml/L; Described chelated dispersants closes dispersant G600 for stinging, and volumetric concentration is 2~3ml/L; Described stabilizing agent is SM-90, and volumetric concentration is 3~4ml/L; Described caustic soda is a 36 ' Be ° caustic soda, and volumetric concentration is 1.0~1.6ml/L; Described hydrogen peroxide is the hydrogen peroxide of mass content 27.5%, and volumetric concentration is 6~8ml/L.
Described acid pickling step is to add citric acid in body lotion, and citric acid 0.1~0.15g/L in the body lotion handles 5~15min under 35~45 ℃ of conditions; Described deoxygenation step is to add deoxygenase JN-500 in body lotion, and deoxygenase JN-500 volumetric concentration is that 0.15~0.20ml/L handles 5~15min to reach the purpose of deoxidation under 35~45 ℃ of conditions in the body lotion.
As optimized technical scheme, blending becomes yarn to comprise step to the china-hemp fibers after described will the dyeing with cotton fiber:
The step of soaping: by bath raio 1: 6~10, add detergent LS, detergent LS0.1~0.3g/L in the body lotion, 90~100 ℃ of 5~15min that soap carry out hot water wash and cold wash more respectively;
Add soft step: use sillicon oil treatment agent DT-30, volumetric concentration is, 3ml/L, antistatic additive ElnctivKH, and volumetric concentration is 1ml/L, 40~50 ℃, handles 25~35min.
Described blending is china-hemp fibers and the cotton fiber yarn by weight proportioning blending in 45: 55, spins resultant yarn through opening picking, comb and parallel cotton fibers prior to spinning, drafting, rove, spun yarn, winder.
Described warping can be selected Switzerland's Benniger warping machines for use, its automaticity height, can be according to the tension force of the different adjustment warping of yarn count, tension force to warping is Electronic Control, simple to operate, the coiling that helps yarn can effectively reduce the warping fault, can effectively cooperate the running of high speed import loom.
Described sizing can be selected field, Tianjin coltfoal sizing for use, can carry out subregion control and adjustment of tonicity, and percentage elongation is controlled in the prescribed limit; According to the requirement of kind, dispose different drying cylinder numbers, improve and draw the yarn mode, can accomplish the flatiron oven dry of yarn two sides, filoplume is submissive.
Described weaving can be adopted many Neils Rapier looms or field, Tianjin coltfoal, Bi Jianuo loom, these equipment are that performance is the most stable in the world at present, function is the most complete, the state-of-the-art loom corollary equipment of class, is furnished with this advanced many Bills electronic jacquard machine simultaneously, can weave the colored type of 13.5in, 54in circulation, it is convenient to have colored type conversion, the characteristics that varietal adaptation is strong.The polychrome latitude mechanism of loom simultaneously can use the weft yarn of 8 kinds of different colours and material at most, has greatly enriched the kind of product, has improved production efficiency and product quality.
Described post processing be with described grey cloth through destarch, wash, add soft, oven dry and sewing and make described look and spin numb cotton textiles.
Described destarch can be used Hong Kong upright letter High Temperature High Pressure overflow dyeing machine, this equipment operation is steady, nozzle is bigger, fabric is contacted with treatment fluid fully and material loading even, the slurry of removing on the fabric preferably to be had, described destarch is to add biological destarch enzyme JN260 in body lotion, volumetric concentration is 5ml/L, bleeding agent SAS60, and volumetric concentration is 0.5ml/L, 90 ℃ of temperature are handled 25min.
Described to add soft be by bath raio 1: 6~10, adds softener NHS, softener NHS 2~4g/L neutralizing acid AC in the body lotion, and volumetric concentration is 0.6~0.8ml/L, 40 ℃ of temperature are handled 30min.
The available oscillation drying machine oven dry of described oven dry, this equipment is controlled by computer, and is added with the pre-baking oven of particular design, and the product after the oven dry is fluffy, and quality is soft and texture is arranged, and provides conditio sune qua non for making plentiful and soft product.
Described sillicon oil treatment agent DT-30 is a polysiloxane emulsion;
Described antistatic additive Elnctiv KH is carbonate compound and polymeric blends;
Described refining agent CZ-4 is that alkaline pectase is the complex of master's enzyme preparation;
Described softener NHS is the emulsion of aliphatic acid condensation product and organically-modified silicone oil;
Described stabilizing agent SM-90 is inorganic salts;
Described neutralizing acid AC is-2-butene dioic acid homopolymer and-2-hydroxyl-1,2, and the three carbonyl acid of 3-propyl group;
Described yellow C-RG is 7-(2-(formamido) amino-4-(4-(2-(2-(8-vinyl sulfonic acid base) ethyoxyl) ethyl) amino-6-fluoro-1,3,5-triazines-2-yl) amino) phenyl) azo-1,3,6-naphthalene trisulfonic acid trisodium;
Described red C-2BL is 3-amino-4-[[4-[[4-[[2-[2-(vinylsulfonyl) ethyoxyl] ethyl group] amino]-6-fluoro-1,3,5-triazines-2-yl] amino]-the 2-sulfophenyl] azo]-5-hydroxyl-2,7-naphthalenedisulfonic acid trisodium;
Described detergent LS is to methoxyl group fatty acyl amido benzene sulfonic acid sodium salt;
Described citric acid is a 2-hydroxy propane-1,2, the 3-tricarboxylic acids.
Technique scheme is a kind of produces the method that look spins numb cotton textiles owing to adopted, with china-hemp fibers and cotton fiber refining after acid pickling step and deoxygenation step, then by bath raio 1: 6~10, in the time of 40~50 ℃, after adding yellow, red REACTIVE DYES processing 5~10min, add glauber salt, glauber salt 8~12g/L in the body lotion, handle 5~15min, add soda ash afterwards, soda ash 6~8g/L in the body lotion is warming up to 55~60 ℃ then, dyeing 20~40min, and the china-hemp fibers after will dyeing blending becomes yarn with cotton fiber; Then the yarn that described blending is become through warping, sizing, weave step and be made into grey cloth; Afterwards described grey cloth being carried out post processing obtains described look and spins numb cotton textiles; Method of the present invention has been improved the cotton finished product of the Chinese fiber crops different shortcomings that require and can't produce a desired effect that the Chinese is numb and cotton dyeing is handled in dyeing course, environmental protection is pollution-free again for ingrain simultaneously, finished product does not have injury to the people, and COLOR FASTNESS height, make color nature, fashion that home textile product presents, the lining that is made into has dim stereoeffect, and is simple and reliable.
The specific embodiment
Below in conjunction with embodiment, further set forth the present invention.Should be understood that these embodiment only to be used to the present invention is described and be not used in and limit the scope of the invention.Should be understood that in addition those skilled in the art can make various changes or modifications the present invention after the content of having read the present invention's instruction, these equivalent form of values fall within the application's appended claims institute restricted portion equally.
Embodiment one:
A kind ofly produce the method that look spins numb cotton textiles, specifically comprise step:
1, refinement step: with this bobbin dyeing machine of Germany the fiber is carried out refining treatment; bath raio is 1: 6~10; 50~60 ℃ of temperature, and emulsifying agent 1#:1.0~1.5ml/L in the body lotion, refining agent CZ-4:0.5ml/L handle 10~40min; add chelated dispersants G600 2~3ml/L again; stabilizing agent SM-90 3~4ml/L, 36 ' Be ° of caustic soda 1.0~1.6ml/L, mass concentration is hydrogen peroxide 6~8ml/L of 27.5%; be warming up to 85~95 ℃, processing 40~60min.
2, acid pickling step: add citric acid, citric acid 0.1~0.15g/L in the body lotion handles 5~15min under 35~45 ℃ of conditions.
3, deoxygenation step: add deoxygenase JN-500, deoxygenase JN-500:0.15~0.20ml/L in the body lotion handles 5~15min to reach the purpose of deoxidation under 35~45 ℃ of conditions.
4, yarn dyeing step: bath raio 1: 6~10, in the time of 40~50 ℃, add the yellow C-RG0.12wt% of Huntsman REACTIVE DYES, red C-2BL 0.06wt% is behind processing 5~15min, add glauber salt, glauber salt 8~12g/L handles 5~15min in the body lotion, adds soda ash, soda ash 6~8g/L in the body lotion, be warming up to 55~60 ℃ then, dyeing 20~40min;
5, the step of soaping: bath raio 1: 6~10, add detergent LS, detergent LS:0.1~0.3g/L in the body lotion, 90~100 ℃ of 5~15min that soap carry out hot water wash and cold wash more respectively;
6, add soft step: the sillicon oil treatment agent of use: DT-30:3ml/L, antistatic additive Elnctiv KH:1ml/L in the time of 40~50 ℃, handles 25~35min.
7, spinning step: china-hemp fibers after will dye and cotton fiber mix by weight 45: 55 proportionings, pass through opening picking, comb and parallel cotton fibers prior to spinning, drafting, rove, spun yarn, winder and spin resultant yarn.
8, warping: select Switzerland's Benniger warping machines during warping for use, its automaticity height, can be according to the tension force of the different adjustment warping of yarn count, tension force to warping is Electronic Control, simple to operate, the coiling that helps yarn can effectively reduce the warping fault, can effectively cooperate the running of high speed import loom.
9, Sizing machines: with field, Tianjin coltfoal sizing.Can carry out subregion control and adjustment of tonicity, percentage elongation is controlled in the prescribed limit; According to the requirement of kind, dispose different drying cylinder numbers, improve and draw the yarn mode, can accomplish the flatiron oven dry of yarn two sides, filoplume is submissive.
10, weave: can adopt many Neils Rapier looms or field, Tianjin coltfoal, Bi Jianuo loom when weaving, these equipment are that performance is the most stable in the world at present, function is the most complete, the state-of-the-art loom corollary equipment of class, is furnished with this advanced many Bills electronic jacquard machine simultaneously, can weave the colored type of 13.5in, 54in circulation, it is convenient to have colored type conversion, the characteristics that varietal adaptation is strong.The polychrome latitude mechanism of loom simultaneously can use the weft yarn of 8 kinds of different colours and material at most, has greatly enriched the kind of product, has improved production efficiency and product quality.
11, destarch: equipment uses Hong Kong upright letter High Temperature High Pressure overflow dyeing machine, and this equipment operation is steady, and nozzle is bigger, fabric is contacted with treatment fluid fully and material loading even, the slurry of removing on the fabric preferably to be had.Technology is: in the body lotion, and biological destarch enzyme JN260:5ml/L, bleeding agent SAS60:0.5ml/L, 90 ℃ of temperature are handled 25min.
12, add soft: bath raio 1: 6~10, softener NHS:2~4g/L, neutralizing acid AC:0.6~0.8ml/L, 40 ℃ of temperature are handled 30min.
13, oven dry: with the oven dry of oscillation drying machine.This equipment is controlled by computer, and is added with the pre-baking oven of particular design, and the product after the oven dry is fluffy, and quality is soft and texture is arranged, and provides conditio sune qua non for making plentiful and soft product.
Check is made and is obtained finished product.
More than show and described basic principle of the present invention, principal character and advantage of the present invention.The technical staff of the industry should understand; the present invention is not restricted to the described embodiments; that describes in the foregoing description and the specification just illustrates principle of the present invention; without departing from the spirit and scope of the present invention; the present invention also has various changes and modifications, and these changes and improvements all fall in the claimed scope of the invention.The claimed scope of the present invention is defined by appending claims and equivalent thereof.

Claims (7)

1. produce the method that look spins numb cotton textiles for one kind, it is characterized in that: with china-hemp fibers and cotton fiber refining after acid pickling step and deoxygenation step, then by bath raio 1: 6~10, in the time of 40~50 ℃, after adding yellow REACTIVE DYES and red REACTIVE DYES processing 5~10min, add glauber salt, glauber salt 8~12g/L in the body lotion, handle 5~15min, add soda ash afterwards, soda ash 6~8g/L in the body lotion is warming up to 55~60 ℃ then, dyeing 20~40min, and the china-hemp fibers after will dyeing blending becomes yarn with cotton fiber; Then the yarn that described blending is become through warping, sizing, weave step and be made into grey cloth; Afterwards described grey cloth being carried out post processing obtains described look and spins numb cotton textiles.
2. a kind of method that look spins numb cotton textiles of producing as claimed in claim 1 is characterized in that: described yellow REACTIVE DYES is yellow C-RG 0.12wt%, and red REACTIVE DYES is red C-2BL 0.06wt%.
3. a kind of method that look spins numb cotton textiles of producing as claimed in claim 1, it is characterized in that: described refining is to be 1: 6~10 by bath raio, 50~60 ℃ of temperature, in body lotion, add emulsifying agent, refining agent, handle 20~40min, add chelated dispersants, stabilizing agent, caustic soda, hydrogen peroxide again, be warming up to 85~95 ℃, handle 40~60min, remove the impurity on the fiber.
4. a kind of method that look spins numb cotton textiles of producing as claimed in claim 3 is characterized in that: emulsifying agent described in the body lotion is an isomery alcohol polyoxyethylene ether, and volumetric concentration is 1.0~1.5ml/L; Described refining agent is refining agent CZ-4, and volumetric concentration is 0.5ml/L; Described chelated dispersants is chelated dispersants G600, and volumetric concentration is 2~3ml/L; Described stabilizing agent is SM-90, and volumetric concentration is 3~4ml/L; Described caustic soda is a 36 ' Be ° caustic soda, and volumetric concentration is 1.0~1.6ml/L; Described hydrogen peroxide is the hydrogen peroxide of mass content 27.5%, and volumetric concentration is 6~8ml/L.
5. a kind of method that look spins numb cotton textiles of producing as claimed in claim 1 is characterized in that, blending becomes yarn to comprise step to the china-hemp fibers after described will the dyeing with cotton fiber:
The step of soaping: by bath raio 1: 6~10, add detergent LS, detergent LS 0.1~0.3g/L in the body lotion, 90~100 ℃ of 5~15min that soap carry out hot water wash and cold wash more respectively;
Add soft step: the sillicon oil treatment agent DT-30 of use, volumetric concentration is 3ml/L, antistatic additive ElnctivKH, volumetric concentration is 1ml/L, handles 5~35min for 40~50 ℃.
6. a kind of method that look spins numb cotton textiles of producing as claimed in claim 5 is characterized in that: described blending is china-hemp fibers and the cotton fiber yarn by weight proportioning blending in 45: 55.
7. a kind of method that look spins numb cotton textiles of producing as claimed in claim 1 is characterized in that: described post processing be with described grey cloth through destarch, wash, add soft, oven dry and sewing and make described look and spin numb cotton textiles.
CN 201010596769 2010-12-20 2010-12-20 Method for producing color spinning cotton textiles Pending CN102021848A (en)

Priority Applications (1)

Application Number Priority Date Filing Date Title
CN 201010596769 CN102021848A (en) 2010-12-20 2010-12-20 Method for producing color spinning cotton textiles

Applications Claiming Priority (1)

Application Number Priority Date Filing Date Title
CN 201010596769 CN102021848A (en) 2010-12-20 2010-12-20 Method for producing color spinning cotton textiles

Publications (1)

Publication Number Publication Date
CN102021848A true CN102021848A (en) 2011-04-20

Family

ID=43863591

Family Applications (1)

Application Number Title Priority Date Filing Date
CN 201010596769 Pending CN102021848A (en) 2010-12-20 2010-12-20 Method for producing color spinning cotton textiles

Country Status (1)

Country Link
CN (1) CN102021848A (en)

Cited By (9)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN102230252A (en) * 2011-06-13 2011-11-02 江阴福斯特纺织有限公司 CVC and hemp-woven fabric and production method thereof
CN102277755A (en) * 2011-06-29 2011-12-14 湖南华升株洲雪松有限公司 Dyeing technology of ramie strips and manufacturing method of spinning
CN102517722A (en) * 2011-12-08 2012-06-27 绍兴国周针织科技有限公司 Spun-dyed yarn produced by vortex spinning and process thereof
CN102517723A (en) * 2011-12-08 2012-06-27 绍兴国周针织科技有限公司 Full-color yarn and its production process
CN102888686A (en) * 2012-09-28 2013-01-23 孚日集团股份有限公司 Spinning process of covering yarn with high hollowness degree, prepared covering yarn and process for weaving towel by utilizing covering yarn
CN103397428A (en) * 2013-07-30 2013-11-20 常熟市新达纬编厂 Production process of cotton-hemp blended yarn-dyed woven fabric
CN104594040A (en) * 2015-02-04 2015-05-06 江苏明源纺织有限公司 Functional colored spun yarn, fabric and preparation method thereof
CN105648787A (en) * 2016-03-25 2016-06-08 太仓市锦达印染有限公司 High temperature and pressure dyeing process for cotton and linen fabrics
CN106491029A (en) * 2016-12-30 2017-03-15 孚日集团股份有限公司 The manufacturing process of grey towel is spent in a kind of resistance to drift

Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN1058439A (en) * 1990-07-25 1992-02-05 山东省泰安印染厂 Pure hemp and cotton hemp interweaving fabric dyeing and finishing process
CN1144855A (en) * 1996-03-27 1997-03-12 开原市亚麻纺织厂 New production technology for flax- cotton dyed fabric
CN101498074A (en) * 2009-03-02 2009-08-05 北京铜牛集团有限公司 Method for manufacturing Chinese hemp multi-component covering type two-sided knit fabric
CN101838876A (en) * 2010-02-23 2010-09-22 孚日集团股份有限公司 Weaving process of hemp textile product

Patent Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN1058439A (en) * 1990-07-25 1992-02-05 山东省泰安印染厂 Pure hemp and cotton hemp interweaving fabric dyeing and finishing process
CN1144855A (en) * 1996-03-27 1997-03-12 开原市亚麻纺织厂 New production technology for flax- cotton dyed fabric
CN101498074A (en) * 2009-03-02 2009-08-05 北京铜牛集团有限公司 Method for manufacturing Chinese hemp multi-component covering type two-sided knit fabric
CN101838876A (en) * 2010-02-23 2010-09-22 孚日集团股份有限公司 Weaving process of hemp textile product

Cited By (14)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN102230252A (en) * 2011-06-13 2011-11-02 江阴福斯特纺织有限公司 CVC and hemp-woven fabric and production method thereof
CN102277755A (en) * 2011-06-29 2011-12-14 湖南华升株洲雪松有限公司 Dyeing technology of ramie strips and manufacturing method of spinning
CN102277755B (en) * 2011-06-29 2013-01-02 湖南华升株洲雪松有限公司 Dyeing technology of ramie strips and manufacturing method of spinning
CN102517722A (en) * 2011-12-08 2012-06-27 绍兴国周针织科技有限公司 Spun-dyed yarn produced by vortex spinning and process thereof
CN102517723A (en) * 2011-12-08 2012-06-27 绍兴国周针织科技有限公司 Full-color yarn and its production process
CN102517722B (en) * 2011-12-08 2014-08-27 绍兴国周针织科技有限公司 Spun-dyed yarn produced by vortex spinning and process thereof
CN102517723B (en) * 2011-12-08 2014-08-27 绍兴国周针织科技有限公司 Full-color yarn and its production process
CN102888686A (en) * 2012-09-28 2013-01-23 孚日集团股份有限公司 Spinning process of covering yarn with high hollowness degree, prepared covering yarn and process for weaving towel by utilizing covering yarn
CN102888686B (en) * 2012-09-28 2015-05-20 孚日集团股份有限公司 Spinning process of covering yarn with high hollowness degree, prepared covering yarn and process for weaving towel by utilizing covering yarn
CN103397428A (en) * 2013-07-30 2013-11-20 常熟市新达纬编厂 Production process of cotton-hemp blended yarn-dyed woven fabric
CN104594040A (en) * 2015-02-04 2015-05-06 江苏明源纺织有限公司 Functional colored spun yarn, fabric and preparation method thereof
CN104594040B (en) * 2015-02-04 2015-10-28 江苏明源纺织有限公司 Functional fiber dyed yarn, fabric and preparation method thereof
CN105648787A (en) * 2016-03-25 2016-06-08 太仓市锦达印染有限公司 High temperature and pressure dyeing process for cotton and linen fabrics
CN106491029A (en) * 2016-12-30 2017-03-15 孚日集团股份有限公司 The manufacturing process of grey towel is spent in a kind of resistance to drift

Similar Documents

Publication Publication Date Title
CN102021848A (en) Method for producing color spinning cotton textiles
CN102383235B (en) Ecological bacteriostatic breathable smooth tatting fabric
CN102733207B (en) Method for dyeing cheese prepared from polyester-cotton blending stretch yarn
CN102493054B (en) A kind of processing method of blended dischargeable spun-dyed yarn
CN101671905A (en) Weaving process of hemp towel
CN107419403A (en) One preparation method for growing flax hidden bar fabric
CN102965870B (en) Single-yarn single-face double-mercerization fabric and processing method thereof
CN103820994A (en) Production technology for cotton, viscose and tencel colored woven fabric
CN101289812B (en) Dyeing process for silk and pashm blended yarn
CN103654002A (en) Moon-curved woven blanket manufacturing technology
CN106939515B (en) The preparation of ball warp mercerization and efficient silkete penetrating agent in a kind of production of denim fabric
CN101705567A (en) Method for producing silver ion antibacterial towel
CN101481880A (en) Production method of nostalgic ecological cotton, hemp and blended fabric thereof
CN105506836A (en) Double-face wool fabric preparation method
CN101603235A (en) Soybean fiber knitted terry and production technology thereof
CN103572580B (en) A kind of polyamide fibre or polyamide fibre/cotton blending PRINTED FABRIC and preparation method thereof
CN102021710B (en) Method for producing cupro textile product
CN104120540A (en) Composite-function fiber knitted fabric with moisture absorption and heating functions and manufacturing method thereof
CN100999848A (en) Veloutine fabric using wool and modified dacron miced spinning and tech. ethereof
CN103014996A (en) Production technique for copper ammonia fiber looped fabrics
CN101748601A (en) Distressed processing method for colored fabric
CN101988269A (en) Dyeing process of real silk and wood pulp cellulose intertextures
CN103215713B (en) Production method of bastose wet spinning yarn
CN105908538B (en) A kind of wool fabric dyeing and printing process
CN102587004B (en) Weaving method for wool looped fabric

Legal Events

Date Code Title Description
PB01 Publication
C06 Publication
SE01 Entry into force of request for substantive examination
C10 Entry into substantive examination
WD01 Invention patent application deemed withdrawn after publication

Application publication date: 20110420

C02 Deemed withdrawal of patent application after publication (patent law 2001)