CN101716618A - 一种热矫直机穿带矫直钢板的方法 - Google Patents

一种热矫直机穿带矫直钢板的方法 Download PDF

Info

Publication number
CN101716618A
CN101716618A CN200910237312A CN200910237312A CN101716618A CN 101716618 A CN101716618 A CN 101716618A CN 200910237312 A CN200910237312 A CN 200910237312A CN 200910237312 A CN200910237312 A CN 200910237312A CN 101716618 A CN101716618 A CN 101716618A
Authority
CN
China
Prior art keywords
steel plate
straightening
straightener
aligning
band
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN200910237312A
Other languages
English (en)
Inventor
田鹏
王普
田士平
闫智平
丁志勇
刘彦川
张蕴涛
侯文立
邱志宏
孙伟
荀利涛
肖斌
李群
李涛
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Shougang Co Ltd
Shougang Corp
Qinhuangdao Shouqin Metal Materials Co Ltd
Original Assignee
Shougang Corp
Qinhuangdao Shouqin Metal Materials Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Shougang Corp, Qinhuangdao Shouqin Metal Materials Co Ltd filed Critical Shougang Corp
Priority to CN200910237312A priority Critical patent/CN101716618A/zh
Publication of CN101716618A publication Critical patent/CN101716618A/zh
Pending legal-status Critical Current

Abstract

一种热矫直机穿带矫直钢板的方法,属于中厚板热矫直机技术领域。工艺步骤为:钢板头部进入矫直机入口时矫直机辊缝设定值为M=H+X;当矫直传带模式运行时,第一道次的钢板头部到达矫直机出口时,矫直机辊缝从M开始下降,当矫直机辊缝值下降到钢板厚度值H时开始进行矫直;矫直机穿带矫直使用低压矫直模式,矫直压力在1000kN-6000kN,其中用于压下系统的液压缸的系统压力控制在在200bar-250bar之间;钢板进入矫直机区域的速度为高速,咬入矫直机为低速,钢板矫直过程中是高速,最终达到恰当的矫直效率。优点在于,有效减少了长度大于15米且翘头的钢板头部对矫直辊的撞击。

Description

一种热矫直机穿带矫直钢板的方法
技术领域
本发明属于中厚板热矫直机技术领域,特别是提供了一种热矫直机穿带矫直钢板的方法。
背景技术
由于轧制高级别钢板,钢板屈服强度大且翘头,经常对矫直辊撞击,造成钢板磕碰严重,对矫直辊损坏严重,为了减少钢板头部对矫直辊的撞击,发明了矫直机穿带矫直方法。
发明内容
本发明的目的在于提供了一种热矫直机穿带矫直钢板的方法,有效减少了长度大于15米且翘头的钢板头部对矫直辊的撞击。
本发明的工艺步骤为:
1.矫直机传带功能即当钢板原始输入数据厚度为固定厚度H,而传带厚度补偿值为X(可人为调整,根据现场工况),第一道次矫直,钢板头部的进入矫直机入口时矫直机辊缝设定值为M=H+X(X在10mm-280mm之间)。
2.当矫直传带模式运行时,第一道次的钢板头部到达矫直机出口时,矫直机辊缝从M开始下降,当矫直机辊缝值下降到钢板厚度值H时开始进行矫直,以避开钢板头部对矫直辊的撞击。
3.矫直机穿带矫直使用低压矫直模式,矫直压力在1000KN-6000KN,其中用于压下系统的液压缸的系统压力控制在在200bar-250bar之间。
4.钢板进入矫直机区域的速度为高速,其速度值为(1米/秒---2米/秒)。咬入矫直机为低速,其速度值为0.5米/秒,钢板矫直过程中是高速,其速度值是(1米/秒---2米/秒)。最终达到恰当的矫直效率。
5.矫直机人机界面增加‘传带按钮’供操作工矫直时启动穿带矫直模式使用。同时,传带功能适用于自动化,半自动化操作。在矫直机一级自动化控制系统中根据该工艺流程进行程序的修改,同时在矫直机人机界面中制作一个按钮触发该程序段运行。
钢板头部到达1#光栅且属于第一道次矫直时,矫直机辊缝设定值=钢板厚度值+穿带矫直辊缝补偿值。穿带矫直过程的穿带速度从1.2米/秒下降为0.5米/秒,压下速度从5毫米/秒提升到为10毫米/秒。钢板头部到达距离矫直机出口1米后,钢板辊缝值快速下降为钢板PDI厚度值,同时保证有(1mm---3mm)的倾动量,入口辊缝低于出口辊缝,穿带速度提升为矫直速度,(1米/秒---2米/秒)。矫直机顺序控制过程不启动高压,在低压状态下矫直,并将矫直机穿带矫直的低压报警值从120bar提高到250bar。
上一块钢板传送离开矫直机后,下块钢板到达矫直机入口1#光栅传感器前,可以手动在人机界面中‘启动穿带矫直按钮’当钢板穿带矫直功能运行状态由灰色变为绿色时,即认为穿带矫直功能处于运行状态(这是一个确认的过程,避免误操作)。根据钢板的翘头量,可以手动调节穿带矫直辊缝补偿值,保证翘头钢板不会磕碰矫直辊。默认值为150mm,可以根据钢板翘头量进行调节,保证钢板进入矫直机前实际辊缝值大于钢板头部高出辊道水平面的数值,在保证不对设备损伤的基础上进行调节。矫直机以1.5米/秒的速度进入矫直机区域,当钢板到达2#光栅(BLS2)后减速以0.5米/秒进入矫直机,当钢板头部到达3#光栅(BLS3)后以模型计算出的矫直速度进行矫直钢板。矫直机区域的光栅位置如图1所示。
根据钢板的液压压下速度和穿带矫直速度,得到钢板穿带矫直厚度补偿值与钢板长度对应关系为:
10<辊缝补偿设定值<(钢板长度-10)*20
  钢板厚度   15米   20米   30米   40米
  辊缝补偿设定值   10mm-100mm   10mm-150mm   10mm-200mm   10mm-320mm
附图说明
图1为矫直机区域的光栅位置示意图
图2为矫直机穿带矫直操作界面其中,穿带矫直启动按钮1、穿带矫直辊缝补偿设定值2、穿带矫直功能运行状态3。
具体实施方式
1.钢板长度大于15米且钢板翘头,为了便于钢板进入矫直机减少对辊缝的磕碰,可以使用此功能。操作界面如图2所示。
2.当前钢板传送离开矫直机后,下块钢板到达矫直机入口9米前,可以手动在人机界面上点击‘Thr On’按钮
3.当钢板穿带矫直功能运行状态由灰色变为绿色时,即认为穿带矫直功能运行。
4.根据钢板的翘头量,可以手动调节穿带矫直辊缝补偿值,保证翘头钢板不会磕碰矫直辊。默认值为150mm,可以根据钢板翘头量进行调节,同时参考辊缝补偿设定值的范围值,在保证不对设备损伤的基础上进行调节。具体调节实例如下:
当钢板离开轧机后,操作工根据该规格钢种的矫直经验,手动将图2中的辊缝补偿设定值按下表设定如下,设定完成后点击‘Thr On’按钮,即进入自动穿带矫直状态,此时,穿带矫直功能运行状态变为绿色。
  钢种   钢板厚度   钢板长度   翘头量   辊缝补偿设定值
  X70   19mm   35000mm   100mm   150mm
  X70   25mm   25000mm   60mm   120mm
  钢种   钢板厚度   钢板长度   翘头量   辊缝补偿设定值
  X80   20mm   16000mm   40mm   80mm
  Q550D   30mm   25000mm   30mm   100mm

Claims (2)

1.一种热矫直机穿带矫直钢板的方法,其特征在于,工艺步骤为:
(1)钢板原始输入数据厚度为固定厚度H,而传带厚度补偿值为X,第一道次矫直,钢板头部进入矫直机入口时矫直机辊缝设定值为M=H+X,X在10mm-280mm之间;
当矫直传带模式运行时,第一道次的钢板头部到达矫直机出口时,矫直机辊缝从M开始下降,当矫直机辊缝值下降到钢板厚度值H时开始进行矫直;
(2)矫直机穿带矫直使用低压矫直模式,矫直压力在1000KN-6000KN,其中用于压下系统的液压缸的系统压力控制在在200bar-250bar之间;
(3)钢板进入矫直机区域的速度为高速,其速度值为:1米/秒---2米/秒;咬入矫直机为低速,其速度值为0.5米/秒,钢板矫直过程中是高速,其速度值为1米/秒---2米/秒;最终达到恰当的矫直效率;
(4)矫直机人机界面增加‘传带按钮’供操作工矫直时启动穿带矫直模式使用;
钢板头部到达1#光栅且属于第一道次矫直时,矫直机辊缝设定值=钢板厚度值+穿带矫直辊缝补偿值;穿带矫直过程的穿带速度从1.2米/秒下降为0.5米/秒,压下速度从5毫米/秒提升到为10毫米/秒;钢板头部到达距离矫直机出口1米后,钢板辊缝值快速下降为钢板PDI厚度值,同时保证有1mm---3mm的倾动量,入口辊缝低于出口辊缝,穿带速度提升为矫直速度:1米/秒---2米/秒;矫直机顺序控制过程不启动高压,在低压状态下矫直,并将矫直机穿带矫直的低压报警值从120bar提高到250bar;
上一块钢板传送离开矫直机后,下块钢板到达矫直机入口1#光栅传感器前,可以手动在人机界面中‘启动穿带矫直按钮’当钢板穿带矫直功能运行状态由灰色变为绿色时,认为穿带矫直功能处于运行状态;根据钢板的翘头量,手动调节穿带矫直辊缝补偿值,保证翘头钢板不会磕碰矫直辊;保证钢板进入矫直机前实际辊缝值大于钢板头部高出辊道水平面的数值,矫直机以1.5米/秒的速度进入矫直机区域,当钢板到达2#光栅后减速以0.5米/秒进入矫直机,当钢板头部到达3#光栅后以模型计算出的矫直速度进行矫直钢板。
2.根据权利要求1所述的方法,其特征在于,所述的穿带矫直辊缝补偿值的默认值为150mm。
CN200910237312A 2009-11-13 2009-11-13 一种热矫直机穿带矫直钢板的方法 Pending CN101716618A (zh)