WO2024202736A1 - 窒化ケイ素粉末およびそれを用いた樹脂組成物 - Google Patents

窒化ケイ素粉末およびそれを用いた樹脂組成物 Download PDF

Info

Publication number
WO2024202736A1
WO2024202736A1 PCT/JP2024/006305 JP2024006305W WO2024202736A1 WO 2024202736 A1 WO2024202736 A1 WO 2024202736A1 JP 2024006305 W JP2024006305 W JP 2024006305W WO 2024202736 A1 WO2024202736 A1 WO 2024202736A1
Authority
WO
WIPO (PCT)
Prior art keywords
silicon nitride
nitride powder
powder
less
particles
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2024/006305
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
一郎 有瀬
友宏 伊藤
和人 原田
好晴 鏡
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Combustion Synthesis Co Ltd
Sumitomo Chemical Co Ltd
Original Assignee
Combustion Synthesis Co Ltd
Sumitomo Chemical Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Combustion Synthesis Co Ltd, Sumitomo Chemical Co Ltd filed Critical Combustion Synthesis Co Ltd
Priority to CN202480018140.3A priority Critical patent/CN120858074A/zh
Priority to JP2025509952A priority patent/JPWO2024202736A1/ja
Priority to KR1020257035323A priority patent/KR20250165403A/ko
Publication of WO2024202736A1 publication Critical patent/WO2024202736A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01B—NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C
    • C01B21/00—Nitrogen; Compounds thereof
    • C01B21/06—Binary compounds of nitrogen with metals, with silicon, or with boron, or with carbon, i.e. nitrides; Compounds of nitrogen with more than one metal, silicon or boron
    • C01B21/068—Binary compounds of nitrogen with metals, with silicon, or with boron, or with carbon, i.e. nitrides; Compounds of nitrogen with more than one metal, silicon or boron with silicon
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K3/00—Use of inorganic substances as compounding ingredients
    • C08K3/34—Silicon-containing compounds
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L63/00—Compositions of epoxy resins; Compositions of derivatives of epoxy resins
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
    • C01P2004/00—Particle morphology
    • C01P2004/60—Particles characterised by their size
    • C01P2004/61—Micrometer sized, i.e. from 1-100 micrometer
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
    • C01P2006/00—Physical properties of inorganic compounds
    • C01P2006/11—Powder tap density
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
    • C01P2006/00—Physical properties of inorganic compounds
    • C01P2006/12—Surface area

Definitions

  • This disclosure relates to silicon nitride powder and a resin composition using the same.
  • Heat generated by passing current through an electronic component is dissipated via a heat sink.
  • a technique is known in which a heat dissipation material is filled between the electronic component and the heat sink.
  • One type of heat dissipation material is a resin composition containing a resin and inorganic particles, and it is known that silicon nitride powder can be used as the inorganic particles (for example, Patent Document 1).
  • Patent document 1 discloses a low-aluminum spherical ⁇ silicon nitride powder used as a filler in electronic packaging materials.
  • the silicon nitride powder is characterized by a sphericity of 0.5 to 0.99, an Al impurity content of less than 500 ppm, and a particle size range of 0.5 ⁇ m to 50 ⁇ m.
  • Patent Document 2 discloses a method for producing silicon nitride powder suitable for producing silicon nitride sintered bodies and silicon nitride powder obtained by said method.
  • the silicon nitride powder has an average particle size of 1-50 ⁇ m, a metal oxide content of 0-10 wt%, and an impurity content of less than 1 wt%, preferably a metal oxide content of less than 1 wt%, and the sintered body has a thermal conductivity of 90 W/mK or more and a bending strength of 700 MPa or more, and preferably the sintering conditions for the sintered body are to mix the silicon nitride powder with MgO and Y 2 O 3 , polish, dry press mold the base, and gas pressure sinter the base at 1900° C. and 1 MPa nitrogen gas pressure for 8 hours.
  • Patent Document 3 discloses silicon nitride powder suitable for producing highly thermally conductive silicon nitride sintered bodies.
  • the silicon nitride powder is characterized by having a ⁇ fraction of 30-100%, an oxygen content of less than 0.5 wt%, an average particle size of 0.2-10 ⁇ m, an aspect ratio of 10 or less, and containing columnar particles with grooves formed in the long axis direction of the particle.
  • the performance of semiconductor components contained in electronic components may be degraded by moisture. If the resin composition used as a heat dissipation material contains a large amount of moisture, the moisture may seep out of the resin composition and reach the electronic components. In order to reduce the moisture content of the resin composition as much as possible, it is desirable to use silicon nitride powder, which has a low moisture content, as a filler.
  • Patent Document 1 does not consider the moisture content of the silicon nitride particles used as a filler.
  • the silicon nitride powders in Patent Documents 2 and 3 disclose silicon nitride powders for use in silicon nitride sintered bodies, and therefore do not discuss mixing with a resin to form a resin composition, nor do they discuss silicon nitride powders suitable as fillers for resin compositions. Furthermore, Patent Documents 2 and 3 do not discuss the moisture content of silicon nitride particles.
  • one embodiment of the present invention aims to provide a silicon nitride powder that is used as a filler for resin compositions and has a low moisture content. Furthermore, another embodiment of the present invention aims to provide a resin composition that uses the silicon nitride powder according to one embodiment.
  • the silicon nitride powder includes a plurality of silicon nitride particles and has an Rsp value to ethanol of less than 105.6.
  • Aspect 2 of the present invention is 2.
  • Aspect 3 of the present invention is The silicon nitride powder according to aspect 1 or 2, wherein the silicon nitride particles have a specific surface area equivalent diameter of more than 0.71 ⁇ m.
  • Aspect 4 of the present invention is A silicon nitride powder according to any one of Aspects 1 to 3, having a specific surface area of less than 2.66 m 2 /g.
  • Aspect 5 of the present invention is The silicon nitride powder according to any one of aspects 1 to 4, having an apparent density of greater than 3.17 g/ cm3 .
  • Aspect 6 of the present invention is The silicon nitride powder according to any one of aspects 1 to 5, wherein the ratio (L2/L1) of the total length L2 of the internal boundary lines to the length L1 of the outer edge is 1% or less, and the maximum particle size of the silicon nitride particles is 6.8 ⁇ m or more.
  • Aspect 7 of the present invention is A resin composition comprising a resin and the silicon nitride powder according to any one of Aspects 1 to 6.
  • a resin composition with a low moisture content can be obtained.
  • the Rsp value for water is used as an indicator for controlling the moisture content of silicon nitride powder.
  • the inventors considered using a dispersion medium other than water because it is difficult to prepare a sample to measure the Rsp value for water and it may be difficult to obtain an accurate value.
  • the Rsp value for ethanol is relatively easy to prepare a sample for measurement, makes it easy to obtain an accurate value, and is also appropriate as an indicator for controlling the moisture content of silicon nitride powder.
  • the Rsp value for ethanol is an index relating to the mobility of the molecules of the dispersion medium (ethanol molecules) adsorbed on the surface of the silicon nitride powder.
  • the silicon nitride powder dispersed in the silicon nitride slurry is dispersed in the silicon nitride slurry with the molecules of the dispersion medium bound to its surface.
  • T2 transverse relaxation time
  • the dispersed state in the dispersion medium becomes stable, and the dispersibility of the silicon nitride powder improves.
  • the Rsp value increases, the dispersibility of the silicon nitride powder tends to improve, and therefore the Rsp value is sometimes used as an index of dispersibility.
  • the Rsp value is used as an index for knowing the amount of molecules (ethanol molecules) of the dispersion medium bound to the surface. It can be said that silicon nitride powder with a high Rsp value for ethanol has a high affinity for ethanol molecules and is easily adsorbed to the surface. Since ethanol molecules are hydrophilic polar molecules, the inventors have intensively studied the silicon nitride powder, assuming that the silicon nitride powder with a high affinity for ethanol molecules also has a high affinity for water molecules.
  • the Rsp value of the silicon nitride powder with respect to ethanol is related to the amount of moisture that the silicon nitride powder can adsorb, and that by making the Rsp value less than 105.6, the amount of moisture that the silicon nitride powder can adsorb can be suppressed to a moisture amount suitable for use as a filler for a resin composition.
  • the Rsp value of silicon nitride powder with respect to ethanol to less than 105.6, a silicon nitride powder with a low moisture content can be obtained, and by using this silicon nitride powder, a resin composition with a low moisture content can be produced.
  • the Rsp value of the silicon nitride powder with respect to ethanol is less than 105.6, preferably 90.0 or less, more preferably 80.0 or less, even more preferably 70.0 or less, and particularly preferably 65.0 or less.
  • the lower limit of the Rsp value is not particularly limited, but may be, for example, 0.5 or more, or 1.0 or more.
  • the relaxation time of 1H nuclei (the time it takes for the pulse-excited magnetization to return to the original thermal equilibrium) is measured by pulse NMR for a silicon nitride slurry in which silicon nitride powder is dispersed in a dispersion medium (ethanol) and for the dispersion medium alone (blank liquid).
  • the Rsp value is calculated using the obtained measurement results according to the following formula (1).
  • the pulse NMR measurement of the silicon nitride slurry can be performed, for example, using a pulse NMR device "the minispec mq20" manufactured by Bruker Corp.
  • the measurement conditions are, for example, a measurement frequency of 20 MHz, a measurement nucleus of 1 H NMR, a measurement method of T2 (transverse relaxation time), a sample amount of 0.3 ml, and a temperature of 25°C.
  • the surface roughness Ra (arithmetic mean roughness) of the silicon nitride powder is preferably less than 0.97 nm. If the surface roughness Ra is less than 0.97 nm, the surface area of the silicon nitride particles can be reduced, thereby reducing the amount of moisture adsorbed on the surface of the silicon nitride particles.
  • the surface roughness Ra is preferably less than 0.97 nm, more preferably 0.95 nm or less, even more preferably less than 0.93 nm, still more preferably 0.90 nm or less, even more preferably 0.80 nm or less, and particularly preferably 0.70 nm or less.
  • a measurement area of 100 nm x 100 nm is observed on the surface of any silicon nitride particle using a scanning probe microscope (SPM).
  • SPM scanning probe microscope
  • the surface roughness Ra is calculated from the obtained shape image.
  • the surface roughness Ra is measured for four silicon nitride particles, and the average value is taken as the surface roughness Ra of the silicon nitride powder.
  • the specific surface area equivalent diameter (DBET) of the silicon nitride particles is preferably more than 0.71 ⁇ m.
  • DBET is preferably more than 0.71 ⁇ m, more preferably 1.10 ⁇ m or more, even more preferably 1.40 ⁇ m or more, even more preferably 3.00 ⁇ m or more, and particularly preferably 8.00 ⁇ m or more.
  • the upper limit of DBET is not particularly limited, but may be, for example, 50 ⁇ m or less, 40 ⁇ m or less, or even 30 ⁇ m or less.
  • the specific surface area diameter (DBET) of the silicon nitride particles is calculated from the following formula (2), which is a general formula showing the relationship between the particle diameter and the specific surface area of a spherical particle.
  • DBET ( ⁇ m) 6/(S ⁇ ) (2) Where: S: the specific surface area of the silicon nitride particles (m 2 /g), and ⁇ : the apparent density of the silicon nitride particles (g/cm 3 ).
  • S and ⁇ for determining DBET are calculated as follows. Since S (the specific surface area of silicon nitride particles) is substantially equal to the specific surface area of silicon nitride powder, the measurement result of the specific surface area of silicon nitride powder measured by the method described below is used. Since ⁇ (apparent density of silicon nitride particles) is substantially equal to the apparent density of silicon nitride powder, the measurement result of the apparent density of silicon nitride powder measured by the method described below is used.
  • the specific surface area of the silicon nitride powder according to the embodiment is a BET specific surface area measured by a krypton adsorption method based on JIS Z 8830: 2013.
  • the specific surface area of the silicon nitride powder is preferably less than 2.66 m 2 /g, which can reduce the amount of moisture adsorbed on the surface.
  • the specific surface area of the silicon nitride powder is more preferably 2.00 m2 /g or less, even more preferably 1.50 m2 /g or less, still more preferably less than 1.36 m2 /g, even more preferably 0.50 m2 /g or less, and particularly preferably 0.24 m2 /g or less.
  • There is no particular lower limit to the specific surface area but it may be, for example, 0.01 m2 /g or more, or 0.05 m2 /g or more.
  • the apparent density of the silicon nitride powder is preferably more than 3.17 g/cm 3 , more preferably more than 3.18 g/cm 3. This results in a silicon nitride powder containing many silicon nitride particles with a small amount of internal voids, that is, a silicon nitride powder with a small amount of moisture that can be retained inside.
  • the upper limit of the apparent density is, for example, 3.44 g/cm 3.
  • the apparent density of the silicon nitride powder is preferably 3.30 g/cm 3 or less, more preferably 3.25 g/cm 3 or less.
  • the apparent density of silicon nitride particles is measured by the pycnometer method in accordance with JIS R 1620:1995. Measurements should be made at least five times, and the average value is taken as the apparent density of the silicon nitride powder.
  • an Accupyc 1330 (Micromeritics) can be used for the measurement.
  • the silicon nitride particles contained in the silicon nitride powder preferably have an average aspect ratio of the minor axis to the major axis of more than 0.50, more preferably more than 0.60, even more preferably 0.65 or more, and even more preferably 0.67 or more.
  • the average aspect ratio of the silicon nitride particles is preferably less than 0.87, more preferably 0.85 or less.
  • the average aspect ratio of the silicon nitride particles is measured as follows. SEM images of silicon nitride particles contained in the silicon nitride powder are analyzed using image processing software (e.g., Image J (manufactured by the National Institute of Health)). The maximum particle size of the silicon nitride particles (referred to as the "major axis") is identified, and the particle size in the direction perpendicular to the major axis is regarded as the "minor axis”. The major and minor axes are measured for 20 random silicon nitride particles, and the ratio of the minor axis to the major axis (minor axis/major axis) is determined for each particle. The arithmetic mean value of these ratios is regarded as the average aspect ratio of the silicon nitride particles.
  • ⁇ -type rate refers to the content (volume %) of ⁇ -type silicon nitride relative to the total silicon nitride contained in the silicon nitride powder.
  • the silicon nitride powder is measured by powder X-ray diffraction, and the diffraction pattern is analyzed by the Gazzara & Messier method (G.P. Gazzara and D.P. Messier, "Determination of Phase Content of Si3N4 by X - ray Diffraction Analysis", Am. Ceram. Soc. Bull., 56[9]777-80 (1977)), to calculate the ⁇ -phase ratio.
  • the maximum particle size of silicon nitride particles having a ratio (L2/L1) of the total length L2 of the internal boundary lines to the length L1 of the outer edge of 1% or less is 6.8 ⁇ m or more
  • the fewer the grain boundaries and cavities inside the silicon nitride particle, the less water can be retained inside. Therefore, the ratio of the total length L2 of the boundary lines to the length L1 of the outer edge (L2/L1) is introduced as an index of the grain boundary content inside the silicon nitride particle.
  • L1 and L2 are obtained by observing the cross section of the silicon nitride particle.
  • the "grain boundary” and "boundary line” refer to a boundary (also called a high-angle grain boundary) whose crystal orientation difference (oblique angle) exceeds 15° as a result of EBSD analysis.
  • silicon nitride particles with a small value of L2/L1 are silicon nitride particles with a low content of boundary lines.
  • silicon nitride particles with an L2/L1 of 1% or less are considered to be silicon nitride particles made of a single crystal (these are referred to as "single crystal particles").
  • the maximum particle size of silicon nitride particles with L2/L1 of 1% or less is preferably 6.8 ⁇ m or more, more preferably 10.0 ⁇ m or more, even more preferably 20.0 ⁇ m or more, even more preferably 40 ⁇ m or more, and particularly preferably 60 ⁇ m or more.
  • the silicon nitride powder preferably has a particle size D50 (hereinafter sometimes simply referred to as "D50") of 1.5 ⁇ m or more, more preferably 2.0 ⁇ m or more, even more preferably 5.0 ⁇ m or more, still more preferably 10.0 ⁇ m or more, and particularly preferably 30 ⁇ m or more, in terms of cumulative particle size distribution based on volume, from the fine particle side.
  • D50 particle size D50
  • the upper limit is not particularly limited, but is preferably 500.0 ⁇ m or less, more preferably 300.0 ⁇ m or less, and even more preferably 200.0 ⁇ m or less.
  • the D50 of silicon nitride powder is measured by the laser diffraction method. Specifically, the powder dispersed in water is irradiated with a laser beam, and the diffraction is measured to determine each particle size. A measuring device such as the CILAS 1090L can be used.
  • Silicon nitride powder is (1) synthesizing a silicon nitride composite crystal by a combustion synthesis method under a nitrogen atmosphere using a raw material containing Si; (2) crushing the silicon nitride synthetic crystals to obtain a coarsely pulverized silicon nitride powder; and (3) finely pulverizing the coarsely pulverized silicon nitride powder to obtain a finely pulverized silicon nitride powder.
  • a step of heat treating the finely pulverized silicon nitride powder may be included.
  • Step (1) Step of synthesizing silicon nitride synthetic crystal
  • Si powder is used as the raw material containing Si.
  • the average particle diameter D50 of the raw material is, for example, within the range of 2 to 10 ⁇ m. This makes it possible to suppress the amount of oxygen impurities and increase the combustion speed to raise the synthesis temperature, thereby obtaining good crystal growth.
  • the average particle diameter D50 of Si is 5 ⁇ m.
  • the diluent is used to adjust the amount of Si in the raw material.
  • a separately prepared silicon nitride powder is used as the diluent.
  • the diluent may be either ⁇ -type silicon nitride powder or ⁇ -type silicon nitride powder, or a mixture of these may be used.
  • the average particle diameter D50 of the diluent is preferably in the range of 0.5 to 2.0 ⁇ m. As an example, the average particle diameter D50 of the diluent is 1.0 ⁇ m.
  • the amount of diluent added is less than 10 mass% of the entire raw material (including the diluent). As an example, the diluent is added in an amount of 5 to 8 mass% of the entire raw material.
  • a diluent is mixed into the raw materials and filled into an insulating heat-resistant container.
  • the insulating heat-resistant container has a thermal conductivity of 1 W/mK or less, and can be made of alumina or zirconia, but carbon is preferred in consideration of the risk of impurities being mixed in.
  • the container is covered with a lid made of the same material as the insulating heat-resistant container.
  • the thickness of the mixed raw materials is made to be greater than 100 mm, preferably greater than 100 mm and less than 150 mm.
  • Combustion synthesis is performed in a nitrogen atmosphere in the range of 0.5 to 1 MPa (for example, 0.9 MPa). By adjusting the pressure range within the above range, efficient synthesis can be achieved while suppressing increases in equipment costs.
  • a layer of powder (silicon nitride) with a thickness of 1 mm to 80 mm is placed on the bottom and sides of the crucible, the mixed raw materials are then filled, and the top surface is then covered with a layer of powder with a thickness of 1 mm to 80 mm.
  • the mixed raw materials can be kept warm, and a specified amount of silicon nitride particles with an Rsp value of less than 105.6 for ethanol can be produced.
  • a catalyst may be used, for example, about 0.01 to 0.1 mass % of Y 2 O 3 , Fe 2 O 3 , CaO, Ni, Co, C, etc. is added.
  • external auxiliary heating in the range of 500° C. to 1700° C. (for example, 1500° C.) is performed to increase the combustion temperature in the combustion synthesis method by self-ignition.
  • Step (2) Obtaining a coarsely pulverized silicon nitride powder
  • the silicon nitride composite crystal is in the form of an aggregate of multiple silicon nitride particles.
  • the silicon nitride composite crystal is crushed to obtain a coarsely pulverized silicon nitride powder.
  • the composite is crushed using a general crushing device such as a hammer mill or a disk mill until it passes through a sieve with a predetermined mesh size (for example, a sieve with a mesh size in the range of 400 ⁇ m to 500 ⁇ m).
  • Step (3) Step of obtaining finely pulverized silicon nitride powder
  • the coarsely pulverized silicon nitride powder is further pulverized to obtain finely pulverized silicon nitride powder.
  • the pulverization is carried out using a pulverizing device such as a jet mill or a ball mill. If necessary, the obtained finely pulverized powder may be classified. The classification may be carried out by sieving, wet classification, or the like.
  • the resulting finely pulverized powder may be used as it is as silicon nitride powder, or the finely pulverized powder may be subjected to a heat treatment step (step (4) described below) before being used as silicon nitride powder.
  • the finely pulverized silicon nitride powder may be heat treated.
  • heat treating an oxide film is formed on the surface of the silicon nitride particles, which has the effect of chemically stabilizing the silicon nitride particles.
  • the heat treatment is carried out, for example, in the atmosphere at 500°C or more and 1200°C or less.
  • the heat treatment time can be appropriately adjusted according to the heat treatment temperature.
  • the heat treatment time is, for example, 5 hours.
  • the heat generated by the combustion synthesis method is used to synthesize silicon nitride composite crystals, which are then crushed, classified, and finely pulverized to produce the silicon nitride powder according to this embodiment.
  • the silicon nitride powder according to the embodiment of the present invention is suitable as a filler for a resin composition.
  • the resin composition contains a resin and the silicon nitride powder according to the embodiment of the present invention.
  • the compounding ratio of the silicon nitride powder and the resin according to the embodiment of the present invention can be appropriately determined depending on the purpose and application.
  • the ratio of the resin to the silicon nitride powder may be 5 to 75 volume % and 95 to 25 volume % relative to the resin composition (composite).
  • the filling rate of the silicon nitride powder in the resin composition refers to the content (volume %) of the silicon nitride powder when the volume of the resin composition (including the silicon nitride powder) is taken as 100 volume %.
  • a resin composition can be obtained by mixing silicon nitride powder and a resin using a commonly used known method.
  • the resin when the resin is liquid (such as liquid epoxy resin), the resin composition can be obtained by mixing the liquid resin, silicon nitride powder, and a curing agent, and then curing with heat or ultraviolet light.
  • Known curing agents, mixing methods, and curing methods can be used.
  • the resin when the resin is solid, the silicon nitride powder and the resin are mixed, and then kneaded by a known method such as melt kneading to obtain the desired resin composition.
  • the resin used in the resin composition may be a known resin such as an epoxy resin.
  • the type of resin may be selected from thermoplastic resins, thermoplastic elastomers, and thermosetting resins.
  • the resin may be used alone or in combination of two or more types.
  • these resin compositions may contain, as necessary, one or more of known additives such as plasticizers, curing accelerators, coupling agents, fillers, pigments, flame retardants, antioxidants, surfactants, compatibilizers, weather resistance agents, antiblocking agents, antistatic agents, leveling agents, and release agents, within the scope of the invention that does not impair the effects of the invention.
  • additives such as plasticizers, curing accelerators, coupling agents, fillers, pigments, flame retardants, antioxidants, surfactants, compatibilizers, weather resistance agents, antiblocking agents, antistatic agents, leveling agents, and release agents, within the scope of the invention that does not impair the effects of the invention.
  • the amount of diluent added was 5 to 8 mass% with respect to the entire raw material (including diluent).
  • the mixed powder was filled in a carbonaceous heat-insulating heat-resistant container with a layer of powder having a thickness of 1 mm to 80 mm on the bottom and sides so that the raw material layer thickness was more than 100 mm and 150 mm or less, and the raw material layer was further covered with a layer of powder having a thickness of 1 mm to 80 mm or less. Then, a lid made of a carbonaceous heat-insulating heat-resistant material was placed, and synthesis was performed under a nitrogen atmosphere of 0.9 MPa. After synthesis, coarse pulverization (disintegration) was performed in a mortar until the powder passed through a sieve with a predetermined opening. The openings of the sieve for each sample are shown in Table 1.
  • the obtained coarsely pulverized powder was further finely pulverized using a Nano Jet Mizer (manufactured by Aisin Nano Technologies Co., Ltd.).
  • a Nano Jet Mizer manufactured by Aisin Nano Technologies Co., Ltd.
  • the obtained finely pulverized powder was classified by the method shown in Table 1. Sample No. 2 was not classified. Thereafter, the obtained classified powders (samples No. 1, 3, and 9) and the finely pulverized powder (sample No.
  • Examples No. 5 to 7 Coarsely pulverized powders were prepared in the same manner as in the above-mentioned "Samples Nos. 1 to 3, and 9.”
  • the sieve used for the coarse pulverization (disintegration) had a mesh size of 500 ⁇ m.
  • the resulting coarsely pulverized powder was finely pulverized in a ball mill.
  • the resulting finely pulverized powder was sieved using a vibrating sieve in the following manner, and then wet-classified to obtain silicon nitride powders having the desired D50 (samples Nos. 5 to 7).
  • Example No. 8 The above-mentioned silicon nitride particles (sample No. 6) were placed in an alumina crucible and heat-treated in an air atmosphere at 900°C for 5 hours using a small powder programmable electric furnace (MMF series manufactured by AS ONE) to obtain silicon nitride powder (sample No. 8).
  • MMF series small powder programmable electric furnace
  • Example No. 4 a commercially available silicon nitride powder (manufactured by Aldrich, silicon nitride (predominantly ⁇ -phase, ⁇ 10 micron primary particle size, product code 248622); hereafter referred to as "Sample No. 4").
  • the maximum particle size of silicon nitride particles having an L2/L1 ratio of 1% or less (the maximum particle size of single crystal particles)
  • a sample for cross-sectional observation was prepared using the sample (silicon nitride particles).
  • the silicon nitride particles were embedded in resin, and then the resin and silicon nitride particles were cut with a diamond cutter. Thereafter, Pt was vapor-deposited on the cross-section as a protective film, the cross-section was prepared by Ar ion milling, and the sample was fixed to the SEM sample stage with Cu double-sided tape, and SEM-EBSD measurement was performed without vapor deposition.
  • the observation position was determined so that two or more silicon nitride particles were completely contained within the observation area (i.e., two or more silicon nitride particles were not in contact with the frame of the observation area).
  • the measurement was performed with ⁇ -type silicon nitride particles.
  • Ion milling device E-3500 (manufactured by Hitachi High-Tech Corporation)
  • Ion sputtering device E-1030 (manufactured by Hitachi, Ltd.)
  • Schottky scanning electron microscope SU5000 (Hitachi High-Tech Corporation)
  • Backscattered electron diffraction device Velocity (manufactured by METEK Corporation)
  • the total length L2 of the boundary lines was also calculated.
  • the “total length L2 of the boundary lines” is the sum of the boundary lines contained inside the silicon nitride particle, and does not include the outer edge of the silicon nitride particle.
  • the total length L2 of the boundary lines was calculated by adding the total length of the grain boundaries inside the silicon nitride particle and the total length of the inner walls of the cavity (if there is a cavity inside the silicon nitride particle).
  • Such measurements were carried out once for 20 random silicon nitride particles, and silicon nitride particles with an L2/L1 ratio of 1% or less were regarded as single crystal particles, and the length of their major axis was measured and recorded as the "maximum particle size of the single crystal particle.” If the 20 silicon nitride particles measured contained multiple single crystal particles, the arithmetic average of their maximum particle sizes was calculated.
  • the SEM images were processed using the image processing software Image J (manufactured by the National Institute of Health) to determine the aspect ratio of 20 randomly selected silicon nitride particles in the SEM images.
  • the maximum diameter of the silicon nitride particle was taken as the major axis, and the particle size in the direction perpendicular to the major axis was taken as the minor axis.
  • the major and minor axes were measured for 20 randomly selected silicon nitride particles, and the ratio of the minor axis to the major axis (minor axis/major axis) was determined for each particle.
  • the arithmetic mean value of these ratios was taken as the average aspect ratio of the silicon nitride particles (referred to as "aspect ratio" in the table).
  • the specific surface area of the sample (silicon nitride powder) was measured.
  • the specific surface area of a powder (solid) was measured by gas adsorption in accordance with JIS Z 8830: 2013, using krypton as the adsorption gas.
  • 1 g of silicon nitride powder was placed in a sample tube, an adsorption/desorption isotherm was obtained, and the specific surface area ( m2 /g) was calculated by the multipoint plot method.
  • the surface roughness Ra was measured using a scanning probe microscope SPA300HV manufactured by Seiko Instruments Inc. The measurement conditions were as follows: Probe station/unit SPI4000/SPA300HV Cantilever: SI-DF20 Scanner: 20 ⁇ m Data type: Shape image Observation mode: DFM (Dynamic Force Mode Microscope) Scanning area: 100 nm x 100 nm Scanning frequency: 0.25Hz Analysis software: (included with the measuring device)
  • Epoxy resin main agent: room temperature curing type potting resin 53 type (manufactured by Sankei Corporation) 010-8140, hardener: room temperature curing type potting resin 53 type (manufactured by Sankei Corporation) 010-8143
  • a sample silicon nitride powder
  • the filling rate of the silicon nitride powder in the resin composition was 50 volume %.
  • a 1 mm thick aluminum plate with a rectangular hole of 1 cm x 10 cm was prepared as a mold form.
  • a PET film coated with a release agent (rear side film) was attached to the rear side of the mold form so as to cover the rectangular hole, with the release agent-coated surface facing the mold form.
  • a PET film coated with a release agent front side film
  • Another aluminum plate was placed on top of the front side film and heated at 100°C for 1 hour to harden the composite. After curing was complete, the aluminum plate was left to cool, and when its temperature had dropped to room temperature, it was removed.
  • the PET films on the front and back sides of the cured composite were then peeled off to obtain a sheet-like sample for measuring the moisture content.
  • the moisture content of the obtained sheet sample was measured.
  • the water content was measured based on the Karl Fischer method in accordance with JIS K 0068:2001 "Method for measuring water content in chemical products.”
  • a resin composition having a water content of less than 380 ppm was evaluated as pass ( ⁇ ), and a resin composition having a water content of 380 ppm or more was evaluated as fail ( ⁇ ).
  • the measurement results are discussed below.
  • the silicon nitride powder of sample No. 4 which does not satisfy the requirements of this embodiment, had a high water content. Therefore, the resin composition prepared using this silicon nitride powder had a high water content.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Organic Chemistry (AREA)
  • Health & Medical Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Medicinal Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Inorganic Chemistry (AREA)
  • Ceramic Products (AREA)
PCT/JP2024/006305 2023-03-31 2024-02-21 窒化ケイ素粉末およびそれを用いた樹脂組成物 Ceased WO2024202736A1 (ja)

Priority Applications (3)

Application Number Priority Date Filing Date Title
CN202480018140.3A CN120858074A (zh) 2023-03-31 2024-02-21 氮化硅粉末和使用其的树脂组合物
JP2025509952A JPWO2024202736A1 (cg-RX-API-DMAC7.html) 2023-03-31 2024-02-21
KR1020257035323A KR20250165403A (ko) 2023-03-31 2024-02-21 질화규소 분말 및 이를 이용한 수지 조성물

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2023-058739 2023-03-31
JP2023058739 2023-03-31

Publications (1)

Publication Number Publication Date
WO2024202736A1 true WO2024202736A1 (ja) 2024-10-03

Family

ID=92905103

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2024/006305 Ceased WO2024202736A1 (ja) 2023-03-31 2024-02-21 窒化ケイ素粉末およびそれを用いた樹脂組成物

Country Status (5)

Country Link
JP (1) JPWO2024202736A1 (cg-RX-API-DMAC7.html)
KR (1) KR20250165403A (cg-RX-API-DMAC7.html)
CN (1) CN120858074A (cg-RX-API-DMAC7.html)
TW (1) TW202500501A (cg-RX-API-DMAC7.html)
WO (1) WO2024202736A1 (cg-RX-API-DMAC7.html)

Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS63274604A (ja) * 1987-05-01 1988-11-11 Nkk Corp 窒化けい素粉末の製造方法
JP2015081205A (ja) * 2013-10-21 2015-04-27 独立行政法人産業技術総合研究所 窒化ケイ素フィラー、樹脂複合物、絶縁基板、半導体封止材
WO2021107021A1 (ja) * 2019-11-28 2021-06-03 株式会社トクヤマ 窒化ケイ素焼結体の製造方法
JP2022135240A (ja) * 2021-03-05 2022-09-15 三菱マテリアル株式会社 窒化珪素粉末及びその製造方法並びにこれを用いたアンダーフィル材用組成物

Family Cites Families (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP4089974B2 (ja) 2004-04-27 2008-05-28 日立金属株式会社 窒化ケイ素質粉末、窒化ケイ素質焼結体及びこれを用いた電子部品用回路基板
CN109761206A (zh) 2019-03-18 2019-05-17 青岛瓷兴新材料有限公司 一种高纯低铝类球形β氮化硅粉体、其制造方法及应用
CN110357052A (zh) 2019-07-16 2019-10-22 青岛瓷兴新材料有限公司 一种通过金属还原制备氮化硅粉末的方法

Patent Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS63274604A (ja) * 1987-05-01 1988-11-11 Nkk Corp 窒化けい素粉末の製造方法
JP2015081205A (ja) * 2013-10-21 2015-04-27 独立行政法人産業技術総合研究所 窒化ケイ素フィラー、樹脂複合物、絶縁基板、半導体封止材
WO2021107021A1 (ja) * 2019-11-28 2021-06-03 株式会社トクヤマ 窒化ケイ素焼結体の製造方法
JP2022135240A (ja) * 2021-03-05 2022-09-15 三菱マテリアル株式会社 窒化珪素粉末及びその製造方法並びにこれを用いたアンダーフィル材用組成物

Also Published As

Publication number Publication date
JPWO2024202736A1 (cg-RX-API-DMAC7.html) 2024-10-03
TW202500501A (zh) 2025-01-01
KR20250165403A (ko) 2025-11-25
CN120858074A (zh) 2025-10-28

Similar Documents

Publication Publication Date Title
WO2020004600A1 (ja) 塊状窒化ホウ素粒子、窒化ホウ素粉末、窒化ホウ素粉末の製造方法、樹脂組成物、及び放熱部材
JP2015081205A (ja) 窒化ケイ素フィラー、樹脂複合物、絶縁基板、半導体封止材
EP4084060B1 (en) Boron nitride sintered body, composite body, method for producing said boron nitride sintered body and method for producing said composite body
WO2024202733A1 (ja) 窒化ケイ素粉末およびそれを用いた樹脂組成物
TW202500501A (zh) 氮化矽粉末及使用其的樹脂組成物
WO2024202729A1 (ja) 窒化ケイ素粉末およびそれを用いた樹脂組成物
WO2024202726A1 (ja) 窒化ケイ素粉末およびそれを用いた樹脂組成物
WO2024202735A1 (ja) 窒化ケイ素粉末およびそれを用いた樹脂組成物
WO2024202734A1 (ja) 窒化ケイ素粉末およびそれを用いた樹脂組成物
WO2024202728A1 (ja) 窒化ケイ素粉末およびそれを用いた樹脂組成物
WO2025178081A1 (ja) 樹脂組成物
WO2025178086A1 (ja) 樹脂組成物
JP7343734B1 (ja) 粉末、粉末の製造方法、及び放熱シート
WO2025178089A1 (ja) 無機粉末およびそれを用いた樹脂組成物
WO2025178088A1 (ja) 無機粉末およびそれを用いた樹脂組成物
TW202534120A (zh) 樹脂組成物
WO2025178082A1 (ja) 樹脂組成物
JP3636514B2 (ja) 六方晶bn焼結体、その製造方法及び半導体用基板
JP2024080633A (ja) アルミナ粒子およびそれを用いた樹脂組成物
TW202436230A (zh) 氧化鋁粒子及使用其的樹脂組成物
TW202423838A (zh) 氧化鋁粒子及使用其的樹脂組成物
JP2026060111A (ja) 窒化ホウ素粉末、窒化ホウ素粉末の製造方法、及び樹脂成形体

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 24778879

Country of ref document: EP

Kind code of ref document: A1

WWE Wipo information: entry into national phase

Ref document number: 202480018140.3

Country of ref document: CN

ENP Entry into the national phase

Ref document number: 2025509952

Country of ref document: JP

Kind code of ref document: A

WWE Wipo information: entry into national phase

Ref document number: 2025509952

Country of ref document: JP

ENP Entry into the national phase

Ref document number: 1020257035323

Country of ref document: KR

Free format text: ST27 STATUS EVENT CODE: A-0-1-A10-A15-NAP-PA0105 (AS PROVIDED BY THE NATIONAL OFFICE)

WWE Wipo information: entry into national phase

Ref document number: KR1020257035323

Country of ref document: KR

WWP Wipo information: published in national office

Ref document number: 202480018140.3

Country of ref document: CN

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 24778879

Country of ref document: EP

Kind code of ref document: A1