WO2024128155A1 - 光学用積層体、積層光学フィルム、光学物品および仮想現実表示装置 - Google Patents

光学用積層体、積層光学フィルム、光学物品および仮想現実表示装置 Download PDF

Info

Publication number
WO2024128155A1
WO2024128155A1 PCT/JP2023/044019 JP2023044019W WO2024128155A1 WO 2024128155 A1 WO2024128155 A1 WO 2024128155A1 JP 2023044019 W JP2023044019 W JP 2023044019W WO 2024128155 A1 WO2024128155 A1 WO 2024128155A1
Authority
WO
WIPO (PCT)
Prior art keywords
layer
liquid crystal
reflective
optical
laminated
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2023/044019
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
竜二 実藤
真道 岸野
克己 篠田
直良 山田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Fujifilm Corp
Original Assignee
Fujifilm Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Fujifilm Corp filed Critical Fujifilm Corp
Priority to CN202380085543.5A priority Critical patent/CN120344886A/zh
Priority to JP2024564350A priority patent/JPWO2024128155A1/ja
Publication of WO2024128155A1 publication Critical patent/WO2024128155A1/ja
Priority to US19/228,771 priority patent/US20250298238A1/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Images

Classifications

    • G—PHYSICS
    • G02—OPTICS
    • G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
    • G02B27/00—Optical systems or apparatus not provided for by any of the groups G02B1/00 - G02B26/00, G02B30/00
    • G02B27/28—Optical systems or apparatus not provided for by any of the groups G02B1/00 - G02B26/00, G02B30/00 for polarising
    • G02B27/286—Optical systems or apparatus not provided for by any of the groups G02B1/00 - G02B26/00, G02B30/00 for polarising for controlling or changing the state of polarisation, e.g. transforming one polarisation state into another
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B7/00—Layered products characterised by the relation between layers; Layered products characterised by the relative orientation of features between layers, or by the relative values of a measurable parameter between layers, i.e. products comprising layers having different physical, chemical or physicochemical properties; Layered products characterised by the interconnection of layers
    • B32B7/02—Physical, chemical or physicochemical properties
    • B32B7/023—Optical properties
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B9/00—Layered products comprising a layer of a particular substance not covered by groups B32B11/00 - B32B29/00
    • G—PHYSICS
    • G02—OPTICS
    • G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
    • G02B1/00—Optical elements characterised by the material of which they are made; Optical coatings for optical elements
    • G02B1/10—Optical coatings produced by application to, or surface treatment of, optical elements
    • G02B1/11—Anti-reflection coatings
    • G02B1/111—Anti-reflection coatings using layers comprising organic materials
    • G—PHYSICS
    • G02—OPTICS
    • G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
    • G02B1/00—Optical elements characterised by the material of which they are made; Optical coatings for optical elements
    • G02B1/10—Optical coatings produced by application to, or surface treatment of, optical elements
    • G02B1/11—Anti-reflection coatings
    • G02B1/118—Anti-reflection coatings having sub-optical wavelength surface structures designed to provide an enhanced transmittance, e.g. moth-eye structures
    • G—PHYSICS
    • G02—OPTICS
    • G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
    • G02B1/00—Optical elements characterised by the material of which they are made; Optical coatings for optical elements
    • G02B1/10—Optical coatings produced by application to, or surface treatment of, optical elements
    • G02B1/14—Protective coatings, e.g. hard coatings
    • G—PHYSICS
    • G02—OPTICS
    • G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
    • G02B27/00—Optical systems or apparatus not provided for by any of the groups G02B1/00 - G02B26/00, G02B30/00
    • G02B27/0018—Optical systems or apparatus not provided for by any of the groups G02B1/00 - G02B26/00, G02B30/00 with means for preventing ghost images
    • G—PHYSICS
    • G02—OPTICS
    • G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
    • G02B27/00—Optical systems or apparatus not provided for by any of the groups G02B1/00 - G02B26/00, G02B30/00
    • G02B27/01—Head-up displays
    • G02B27/017—Head mounted
    • G02B27/0172—Head mounted characterised by optical features
    • G—PHYSICS
    • G02—OPTICS
    • G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
    • G02B27/00—Optical systems or apparatus not provided for by any of the groups G02B1/00 - G02B26/00, G02B30/00
    • G02B27/02—Viewing or reading apparatus
    • G—PHYSICS
    • G02—OPTICS
    • G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
    • G02B5/00—Optical elements other than lenses
    • G02B5/08—Mirrors
    • G02B5/0816—Multilayer mirrors, i.e. having two or more reflecting layers
    • G02B5/0825—Multilayer mirrors, i.e. having two or more reflecting layers the reflecting layers comprising dielectric materials only
    • G—PHYSICS
    • G02—OPTICS
    • G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
    • G02B5/00—Optical elements other than lenses
    • G02B5/20—Filters
    • G02B5/26—Reflecting filters
    • G—PHYSICS
    • G02—OPTICS
    • G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
    • G02B5/00—Optical elements other than lenses
    • G02B5/30—Polarising elements
    • G—PHYSICS
    • G02—OPTICS
    • G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
    • G02B5/00—Optical elements other than lenses
    • G02B5/30—Polarising elements
    • G02B5/3016—Polarising elements involving passive liquid crystal elements
    • G—PHYSICS
    • G02—OPTICS
    • G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
    • G02B5/00—Optical elements other than lenses
    • G02B5/30—Polarising elements
    • G02B5/3025—Polarisers, i.e. arrangements capable of producing a definite output polarisation state from an unpolarised input state
    • G02B5/3033—Polarisers, i.e. arrangements capable of producing a definite output polarisation state from an unpolarised input state in the form of a thin sheet or foil, e.g. Polaroid
    • G02B5/3041—Polarisers, i.e. arrangements capable of producing a definite output polarisation state from an unpolarised input state in the form of a thin sheet or foil, e.g. Polaroid comprising multiple thin layers, e.g. multilayer stacks
    • G02B5/305—Polarisers, i.e. arrangements capable of producing a definite output polarisation state from an unpolarised input state in the form of a thin sheet or foil, e.g. Polaroid comprising multiple thin layers, e.g. multilayer stacks including organic materials, e.g. polymeric layers
    • G—PHYSICS
    • G09—EDUCATION; CRYPTOGRAPHY; DISPLAY; ADVERTISING; SEALS
    • G09F—DISPLAYING; ADVERTISING; SIGNS; LABELS OR NAME-PLATES; SEALS
    • G09F9/00—Indicating arrangements for variable information in which the information is built-up on a support by selection or combination of individual elements

Definitions

  • the present invention relates to an optical laminate, a laminated optical film, an optical article, and a virtual reality display device.
  • a reflective polarizer is a polarizer that reflects one polarized light of incident light and transmits the other polarized light.
  • the reflected light and transmitted light by the reflective polarizer have mutually orthogonal polarization states.
  • mutually orthogonal polarization states refer to polarization states located at antipodes on the Poincaré sphere, such as mutually orthogonal linear polarization, and right-handed circular polarization and left-handed circular polarization.
  • Known examples of reflective linear polarizers in which transmitted light and reflected light are linearly polarized include a film made of a stretched dielectric multilayer film as described in Patent Document 1, and a wire grid polarizer as described in Patent Document 2.
  • a reflective circular polarizer in which transmitted light and reflected light are circularly polarized for example, a film having a light-reflecting layer in which a cholesteric liquid crystal phase is fixed, as described in Patent Document 3, is known.
  • Reflective polarizers are used for the purpose of extracting only a specific polarized light from incident light or splitting incident light into two polarized lights.
  • it is used as a brightness enhancement film that reflects and reuses unnecessary polarized light from the backlight to improve light utilization efficiency
  • liquid crystal projectors it is used as a beam splitter that splits light from a light source into two linearly polarized lights and supplies each to a liquid crystal panel.
  • Patent Literature 4 discloses an in-vehicle rearview mirror that uses a reflective polarizer to reflect light from behind.
  • Patent Literature 5 discloses a method for generating a virtual image by reflecting light back and forth between a reflective polarizer and a half mirror in order to reduce the size and thickness of a display unit in a virtual reality display device, an electronic viewfinder, or the like.
  • the inventors believe that the reason for this is that the light-reflecting layer in which a cholesteric liquid crystal phase is fixed allows a reflective circular polarizer with a high degree of polarization to be realized as a thin film, and therefore the polarizer is less susceptible to the influence of foreign matter contamination and fluctuations due to the density of the material distribution. Furthermore, according to the study by the present inventors, in virtual reality display devices and electronic viewfinders, etc., transmitted light is used in addition to reflected light, and in such cases, it is important to suppress ghosting, which is a visible phenomenon caused by the transmitted light that is originally intended to be blocked being transmitted. In the conventional reflective circular polarizer described in Patent Document 3, ghosting suppression was observed, leaving room for further improvement.
  • the present invention has been made in consideration of the above problems, and the problem that the present invention aims to solve is to provide an optical laminate that can be used with a reflective circular polarizer that generates little ghosting when used in a virtual reality display device, an electronic viewfinder, etc., a laminated optical film that includes the above-mentioned reflective circular polarizer, an optical article that includes the optical laminate, and a virtual reality display device that includes the optical article.
  • the laminated reflective layer includes a reflective layer A including at least one cholesteric liquid crystal layer formed using a first liquid crystal compound substantially consisting of a rod-shaped liquid crystal compound, and not including a cholesteric liquid crystal layer formed using a second liquid crystal compound substantially consisting of a discotic liquid crystal compound; a reflective layer B including at least one cholesteric liquid crystal layer formed using the second liquid crystal compound substantially consisting of a discotic liquid crystal compound, and a reflective layer B including no cholesteric liquid crystal layer formed using the first liquid crystal compound substantially consisting of a rod-shaped liquid crystal compound;
  • the laminated reflective layer is composed of one of the reflective layers A and one of the reflective layers B in direct contact with each other, or is composed of one of the reflective layers A and one of the reflective layers B, and an adhesive layer disposed between the reflective layers A and B.
  • the reflective circular polarizer is the optical laminate according to any one of [1] to [9].
  • the laminated optical film according to [10] further comprising a positive C plate.
  • the laminated optical film according to [10] further comprising an antireflection layer on a surface thereof.
  • An optical article comprising the optical laminate according to any one of [1] to [9].
  • a virtual reality display device comprising the optical article according to [16].
  • an optical laminate that can be used for a reflective circular polarizer that generates little ghosting when used in a virtual reality display device, an electronic viewfinder, or the like. Furthermore, according to the present invention, it is possible to provide a laminated optical film including the above-mentioned reflective circular polarizer, an optical article including the above-mentioned optical laminate, and a virtual reality display device including the above-mentioned optical article.
  • FIG. 1 is a schematic view showing an example of the optical laminate according to the first embodiment of the present invention.
  • FIG. 2 is a schematic diagram showing an example of the optical laminate according to the first embodiment of the present invention.
  • FIG. 3 shows an example of a virtual reality display device using the laminated optical film of the present invention.
  • FIG. 4 shows an example of a virtual reality display device using the laminated optical film of the present invention.
  • FIG. 5 is a schematic diagram showing an example of the laminated optical film of the present invention.
  • FIG. 6 is a schematic diagram for explaining the function of the optical laminate of the present invention.
  • FIG. 7 is a conceptual diagram for explaining the function of a conventional optical laminate.
  • orthogonal does not mean strictly 90°, but means 90° ⁇ 10°, preferably 90° ⁇ 5°.
  • parallel does not mean strictly 0°, but means 0° ⁇ 10°, preferably 0° ⁇ 5°.
  • 45° does not mean strictly 45°, but means 45° ⁇ 10°, preferably 45° ⁇ 5°.
  • absorption axis refers to the polarization direction in which absorbance is maximum in the plane when linearly polarized light is incident.
  • reflection axis refers to the polarization direction in which reflectance is maximum in the plane when linearly polarized light is incident.
  • transmission axis refers to the direction in the plane that is perpendicular to the absorption axis or reflection axis.
  • slow axis refers to the direction in the plane where the refractive index is maximum.
  • Frest axis refers to the direction in the plane where the refractive index is minimum, and is the direction perpendicular to the slow axis.
  • the phase difference means the in-plane retardation and is expressed as Re( ⁇ ), where Re( ⁇ ) represents the in-plane retardation at a wavelength ⁇ , and unless otherwise specified, the wavelength ⁇ is 550 nm.
  • the retardation in the thickness direction at a wavelength ⁇ is referred to as Rth( ⁇ ).
  • the wavelength ⁇ is 550 nm.
  • Re( ⁇ ) and Rth( ⁇ ) can be values measured at a wavelength ⁇ using an AxoScan OPMF-1 (manufactured by Optosciences Inc.).
  • optical laminate of the present invention may be exemplified by the following first embodiment.
  • a first embodiment of the optical laminate of the present invention will be described below.
  • the optical laminate of the first embodiment of the present invention has two or more laminated reflective layers
  • the laminated reflective layer includes a reflective layer A including at least one cholesteric liquid crystal layer (hereinafter also referred to as "liquid crystal layer 1") formed using a first liquid crystal compound substantially consisting of a rod-shaped liquid crystal compound, and not including a cholesteric liquid crystal layer (hereinafter also referred to as "liquid crystal layer 2") formed using a second liquid crystal compound substantially consisting of a discotic liquid crystal compound; a reflective layer B including at least one liquid crystal layer 2 and no liquid crystal layer 1;
  • the reflective layers A face each other in two of the two or more laminated reflective layers adjacent to each other in the lamination direction, the central wavelengths of the reflected light of the reflective layers A included in the two adjacent laminated reflective layers are different from each other,
  • the reflective layers B are opposed to each other in two of the two or more laminated reflective layers adjacent to each other in the lamination direction, the central wavelengths of the reflected light of the reflective layers B included in the
  • Fig. 1 is a schematic cross-sectional view showing an example of the configuration of an optical laminate 10 according to the first embodiment.
  • the optical laminate 10 is composed of a first laminate reflective layer 25, a second laminate reflective layer 26, an optical interference layer 27, and an adhesive layer 28.
  • the first laminate reflective layer 25 is composed of a reflective layer A21a and a reflective layer B22b
  • the second laminate reflective layer 26 is composed of a reflective layer A23a and a reflective layer B24b.
  • the reflective layer A21a, the reflective layer B22b, the reflective layer A23a, and the reflective layer B24b are laminated in this order.
  • the optical laminate of the first embodiment of the present invention can be used for a reflective circular polarizer.
  • the reflective layer A has a positive Rth
  • the reflective layer B has a negative Rth, so that the Rths are offset, and it is considered that the occurrence of ghosts can be suppressed even for light incident from an oblique direction.
  • the refractive index and film thickness of the optical interference layer is set to satisfy the above relationship, it is possible to provide an anti-reflection effect at the interface between the first laminated reflective layer and the adhesive layer.
  • this can suppress the change in the rotation direction of circularly polarized light caused by interface reflection, for example, the change of right-handed circularly polarized light to left-handed circularly polarized light caused by interface reflection. Since the change in the rotation direction of circularly polarized light caused by interface reflection is one of the causes of ghost generation, it is considered that the generation of ghost can be suppressed by suppressing interface reflection. Regarding this point, it will be described in detail later.
  • the first embodiment of the present invention will be described in detail below.
  • the optical laminate of the first embodiment of the present invention has two or more laminated reflective layers each including one reflective layer A and one reflective layer B, which will be described in detail later. That is, the optical laminate of the first embodiment of the present invention includes two or more reflective layers A and two or more reflective layers B.
  • the reflective layer A and the reflective layer B may be in direct contact with each other, or the reflective layer A and the reflective layer B may be laminated via another layer.
  • the other layer is not particularly limited, but may include an adhesive layer, a refractive index adjustment layer, a resin film, a positive C plate, and an orientation layer.
  • the adhesive layer is, for example, an adhesive layer or a pressure-sensitive adhesive layer.
  • the laminated reflective layer may be configured such that one reflective layer A and one reflective layer B are in direct contact with each other, or may be configured such that one reflective layer A, one reflective layer B, and an adhesive layer disposed between the reflective layer A and the reflective layer B.
  • the laminated reflective layer is preferably configured such that one reflective layer A and one reflective layer B are in direct contact with each other.
  • the reflective layers A and B may be stacked alternately, the reflective layers A may be stacked opposite each other, or the reflective layers B may be stacked opposite each other.
  • the layers may be laminated in the order of reflective layer A, reflective layer B, reflective layer A and reflective layer B, or the order of reflective layer A, reflective layer B, reflective layer B and reflective layer A, or the order of reflective layer B, reflective layer A, reflective layer A and reflective layer B.
  • the central wavelengths of the reflected light of the reflective layers A included in the two adjacent laminated reflective layers are different.
  • the reflective layers B of the two laminated reflective layers adjacent to each other in the lamination direction face each other, for example, when laminated in the order of reflective layer A, reflective layer B, reflective layer B, and reflective layer A, the central wavelengths of the reflected light of the reflective layers B included in the two adjacent laminated reflective layers are different.
  • the optical laminate 11 shown in Fig. 2 is composed of a first laminated reflective layer 25, a second laminated reflective layer 26, an optical interference layer 27, and an adhesive layer 28.
  • the first laminated reflective layer 25 is composed of a reflective layer B21b and a reflective layer A22a
  • the second laminated reflective layer 26 is composed of a reflective layer A23a and a reflective layer B24b.
  • the reflective layer B21b, the reflective layer A22a, the reflective layer A23a, and the reflective layer B24b are laminated in this order.
  • the central wavelength of the reflected light of the reflective layer A22a is different from the central wavelength of the reflected light of the reflective layer A23a in this optical laminate 11.
  • the reflective layer A22a is included in the first laminated reflective layer 25, and the reflective layer A23a is included in the second laminated reflective layer 26.
  • the reflective layer A may contain two or more liquid crystal layers 1 having different central wavelengths of reflected light, but when two or more liquid crystal layers 1 are arranged in succession in the optical laminate, the reflective layer A and the stacked reflective layers are arranged so that the number of stacked reflective layers is maximized.
  • the reflective layer B may contain two or more liquid crystal layers 2 having different central wavelengths of reflected light, but when two or more liquid crystal layers 2 are arranged in succession in the optical laminate, the reflective layer B and the stacked reflective layers are arranged so that the number of stacked reflective layers is maximized.
  • the laminated reflective layer is preferably formed such that the reflective layer A and the reflective layer B are alternately arranged. That is, the reflective layer A and the reflective layer B are alternately arranged in the thickness direction of the optical laminate.
  • the optical laminate of the first embodiment includes two or more laminated reflective layers. Therefore, the optical laminate of the present invention may include three or four or more laminated reflective layers. That is, the optical laminate includes two or more of the reflective layer A and the reflective layer B, but may include three or four or more of the reflective layer A and the reflective layer B.
  • the total number of laminated reflective layers included in the optical laminate is preferably 30 or less, more preferably 20 or less, and even more preferably 10 or less. That is, the total number of the reflective layers A and B in the optical laminate is preferably 60 or less, more preferably 40 or less, and more preferably 20 or less.
  • the thickness of the laminated reflective layer is preferably 0.2 ⁇ m or more, more preferably 0.4 ⁇ m or more, and even more preferably 0.6 ⁇ m or more.
  • the thickness of the laminated reflective layer is preferably 20.0 ⁇ m or less, more preferably 14.0 ⁇ m or less, and even more preferably 10.0 ⁇ m or less.
  • the thickness of the laminated reflective layer can be measured in the same manner as for the reflective layer A and the reflective layer B described below.
  • Reflective layer A and reflective layer B are explained below.
  • the laminated reflective layer included in the optical laminate of the first embodiment of the present invention includes a reflective layer A that includes at least one liquid crystal layer 1 and does not include a liquid crystal layer 2 .
  • the liquid crystal layer 1 is a cholesteric liquid crystal layer formed using a first liquid crystal compound substantially composed of a rod-shaped liquid crystal compound, and is substantially composed of a rod-shaped liquid crystal compound.
  • cholesteric liquid crystal layer formed using a first liquid crystal compound substantially composed of a rod-shaped liquid crystal compound refers to a layer formed by fixing the orientation state of the cholesteric liquid crystal phase of the first liquid crystal compound.
  • the term "substantially composed of a rod-shaped liquid crystal compound” means that the liquid crystal compound (first liquid crystal compound) contained in the liquid crystal layer 1 is 95% by mass or more of the rod-shaped liquid crystal compound.
  • first liquid crystal compound substantially composed of a rod-shaped liquid crystal compound means that the content of the rod-shaped liquid crystal compound is 95% by mass or more with respect to the total mass of the first liquid crystal compound.
  • the first liquid crystal compound is composed only of a rod-shaped liquid crystal compound.
  • the liquid crystal layer 2 is a cholesteric liquid crystal layer formed using a second liquid crystal compound substantially made of a discotic liquid crystal compound, and is substantially made of a discotic liquid crystal compound.
  • cholesteric liquid crystal layer formed using a second liquid crystal compound substantially made of a discotic liquid crystal compound refers to a layer formed by fixing the orientation state of the cholesteric liquid crystal phase of the second liquid crystal compound.
  • substantially made of a discotic liquid crystal compound means that the liquid crystal compound (second liquid crystal compound) contained in the liquid crystal layer 2 is 95% by mass or more of the discotic liquid crystal compound.
  • second liquid crystal compound substantially made of a discotic liquid crystal compound means that the content of the discotic liquid crystal compound is 95% by mass or more with respect to the total mass of the second liquid crystal compound.
  • the second liquid crystal compound is made of only a discotic liquid crystal compound.
  • the reflective layer A may contain one or more layers of the liquid crystal layer 1, and therefore may contain two or more layers.
  • layers other than the liquid crystal layer 2 may or may not be included between the two or more liquid crystal layers 1.
  • the other layers include, but are not limited to, an adhesion layer (e.g., an adhesive layer, a pressure-sensitive adhesive layer, etc.), a refractive index adjustment layer, a resin film, a positive C plate, and an alignment layer.
  • the number of layers of the liquid crystal layer 1 included in the reflective layer A is preferably 5 or less, more preferably 3 or less, and even more preferably 2 or less.
  • the number of layers of the liquid crystal layer 1 included in the reflective layer A is preferably 1.
  • liquid crystal layers 1 when two liquid crystal layers 1 have different central wavelengths of reflected light, they are regarded as two liquid crystal layers 1. Furthermore, when two or more liquid crystal layers 1 have the same central wavelength of reflected light, they are regarded as one liquid crystal layer 1 even if they are formed by successive coating or separated by the other layer.
  • the central wavelength of the reflected light of the reflective layer A is the central wavelength of the reflected light of the entire reflective layer A.
  • the method for measuring the central wavelength of the reflected light is described below.
  • the thickness of the reflective layer A is preferably 0.1 ⁇ m or more, more preferably 0.2 ⁇ m or more, and even more preferably 0.3 ⁇ m or more.
  • the thickness of the reflective layer A is preferably 10.0 ⁇ m or less, more preferably 7.0 ⁇ m or less, and even more preferably 5.0 ⁇ m or less, in terms of further suppressing ghosts.
  • the thickness of the reflective layer A can be measured by preparing a cross section of the optical laminate and observing it with a scanning electron microscope.
  • the thickness of the reflective layer A is a value obtained by averaging the thickness of the reflective layer A at any five points on the cross section of the optical laminate.
  • the region of the reflective layer A and the region of the reflective layer B described later can be distinguished by the difference in contrast of the captured image.
  • the reflective layer A and the reflective layer B can also be distinguished by using composition analysis in the thickness direction by time-of-flight secondary ion mass spectrometry (TOF-SIMS).
  • the Rth of the reflective layer A is preferably from 8 to 800 nm, more preferably from 16 to 560 nm, and further preferably from 24 to 400 nm, at a wavelength of 550 nm.
  • the Rth of the reflective layer A may be measured by taking out only the reflective layer A from the optical laminate, or the Rth of a layer prepared under the same conditions as when the reflective layer A is prepared may be measured.
  • the rod-shaped liquid crystal compound contained in the liquid crystal layer 1 may be any known rod-shaped liquid crystal compound, and preferably a polymerizable rod-shaped liquid crystal compound having a polymerizable group.
  • Examples of the rod-shaped liquid crystal compound are not particularly limited, but include those described in claim 1 of JP-T-11-513019 or paragraphs [0026] to [0098] of JP-A-2005-289980.
  • a rod-shaped liquid crystal compound having a high refractive index anisotropy ⁇ n (high ⁇ n), where ⁇ n is the difference between the refractive index in the slow axis direction and the refractive index in the fast axis direction.
  • ⁇ n is the difference between the refractive index in the slow axis direction and the refractive index in the fast axis direction.
  • the liquid crystal compound having a high refractive index anisotropy ⁇ n is not particularly limited, but the compounds exemplified in paragraphs [0014] to [0029] of International Publication No. 2019/182129 and the following general formula (I) can be preferably used.
  • P1 and P2 each independently represent a hydrogen atom, -CN, -NCS or a polymerizable group.
  • Sp1 and Sp2 each independently represent a single bond or a divalent linking group, provided that Sp1 and Sp2 do not represent a divalent linking group containing at least one group selected from the group consisting of an aromatic hydrocarbon ring group, an aromatic heterocyclic group, and an aliphatic hydrocarbon ring group.
  • R represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms.
  • R's When there are a plurality of R's, they may be the same or different.
  • Z 1 and Z 2 's they may be the same or different.
  • Z 3 's they may be the same or different.
  • Z 3 's linked to Sp 2 represent a single bond.
  • X1 and X2 each independently represent a single bond or S-. Multiple X1s and multiple X2s may be the same or different. However, at least one of the multiple X1s and multiple X2s represents -S-.
  • k represents an integer of 2 to 4.
  • m and n each independently represent an integer of 0 to 3.
  • a plurality of m's may be the same or different.
  • a 1 , A 2 , A 3 and A 4 each independently represent a group represented by any one of the following general formulae (B-1) to (B-7), or a group formed by linking two or more and three or less groups represented by any one of the following general formulae (B-1) to (B-7).
  • B-1 and A 4 When there are multiple A 2 and A 3 , they may be the same or different.
  • a 1 and A 4 they may be the same or different.
  • W 1 to W 18 each independently represent CR 1 or N, and R 1 represents a hydrogen atom or a substituent L described below.
  • Y 1 to Y 6 each independently represent NR 2 , O or S, and R 2 represents a hydrogen atom or a substituent L as described below.
  • G 1 to G 4 each independently represent CR 3 R 4 , NR 5 , O or S, and R 3 to R 5 each independently represent a hydrogen atom or the following substituent L.
  • M 1 and M 2 each independently represent CR 6 or N, and R 6 represents a hydrogen atom or the following substituent L. * indicates the bond position.
  • the substituent L is an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkanoyl group having 1 to 10 carbon atoms, an alkanoyloxy group having 1 to 10 carbon atoms, an alkanoylamino group having 1 to 10 carbon atoms, an alkanoylthio group having 1 to 10 carbon atoms, an alkyloxycarbonyl group having 2 to 10 carbon atoms, an alkylaminocarbonyl group having 2 to 10 carbon atoms, an alkylthiocarbonyl group having 2 to 10 carbon atoms, a hydroxy group, an amino group, a mercapto group, a carboxy group, a sulfo group, an amido group, a cyano group, a nitro group, a halogen atom, or a polyme
  • the substituent L when the above group described as the substituent L has -CH 2 -, the substituent L also includes a group in which at least one of the -CH 2 - contained in the above group is replaced with -O-, -CO-, -CH ⁇ CH-, or C ⁇ C-.
  • the substituent L when the above group described as the substituent L has a hydrogen atom, the substituent L also includes a group in which at least one of the hydrogen atoms contained in the above group is replaced with at least one selected from the group consisting of a fluorine atom and a polymerizable group.
  • the refractive index anisotropy ⁇ n 550 (refractive index anisotropy at a wavelength of 550 nm) of the liquid crystal compound is preferably 0.12 or more, more preferably 0.16 or more, even more preferably 0.20 or more, and most preferably 0.25 or more.
  • the upper limit of ⁇ n 550 (refractive index anisotropy at a wavelength of 550 nm) is preferably 0.90 or less, more preferably 0.70 or less, and even more preferably 0.50 or less, from the viewpoint of suppressing interface reflection.
  • the liquid crystal layer 1 may be any layer in which the orientation of the rod-shaped liquid crystal compound in a cholesteric liquid crystal phase is maintained, and may typically be formed by polymerizing and curing a polymerizable rod-shaped liquid crystal compound having a polymerizable group by a method such as adding a chiral agent to bring the compound into an oriented state of a cholesteric liquid crystal phase, and then polymerizing and curing the compound by ultraviolet irradiation, heating, etc., to form a layer with no fluidity.
  • the liquid crystal layer 1 formed as described above may be any layer in which the orientation form is changed to a state in which it is not changed by an external field, an external force, etc.
  • the rod-like liquid crystal compound in the liquid crystal layer 1 does not need to exhibit liquid crystallinity any more.
  • the polymerizable rod-like liquid crystal compound may be polymerized by a curing reaction and lose its liquid crystallinity.
  • the central wavelength of the reflected light of the liquid crystal layer 1 can be obtained as follows. When the transmission spectrum of the reflective layer A is measured from the normal direction of the liquid crystal layer 1 using a spectrophotometer UV3150 (Shimadzu Corporation), a spectrum having a peak where the transmittance decreases in the region near the central wavelength of the reflected light is obtained.
  • the pitch of the cholesteric liquid crystal phase varies with the type of chiral agent used together with the polymerizable rod-like liquid crystal compound and its concentration, and a cholesteric liquid crystal phase with the desired pitch can be obtained by adjusting one or more of the above.
  • the helical direction and pitch can be measured using the methods described in "Introduction to Liquid Crystal Chemistry Experiments” edited by the Japanese Liquid Crystal Society, published by Sigma Publishing in 2007, p. 46, and "Liquid Crystal Handbook” edited by the Liquid Crystal Handbook Editorial Committee, published by Maruzen, p. 196.
  • the laminated reflective layer included in the optical laminate of the first embodiment of the present invention includes at least one liquid crystal layer 2 and a reflective layer B not including a liquid crystal layer 1 .
  • the liquid crystal layer 2 and the liquid crystal layer 1 are defined as above.
  • the reflective layer B may include one or more liquid crystal layers 2, and therefore may include two or more layers.
  • a layer other than the liquid crystal layer 1 may or may not be included between the two or more liquid crystal layers 2.
  • the other layers include, but are not limited to, an adhesion layer (e.g., an adhesive layer, a pressure-sensitive adhesive layer, etc.), a refractive index adjustment layer, a resin film, a positive C plate, and an alignment layer.
  • the number of layers of the liquid crystal layer 2 included in the reflective layer B is preferably 5 or less, more preferably 3 or less, and further preferably 2 or less.
  • the number of layers of the liquid crystal layer 2 included in the reflective layer B is preferably 1.
  • liquid crystal layers 2 when two liquid crystal layers 2 have different central wavelengths of reflected light, they are regarded as two liquid crystal layers 2. Furthermore, when the central wavelengths of reflected light of two or more liquid crystal layers 2 are the same, they are regarded as one liquid crystal layer 2 even if they are formed by successive coating or separated by the other layer.
  • the central wavelength of the reflected light of the reflective layer B is the central wavelength of the reflected light of the entire reflective layer B.
  • the central wavelength of the reflected light of each liquid crystal layer 2 is measured in accordance with the method for measuring the central wavelength of the reflected light of the liquid crystal layer 1 described above.
  • the thickness of the reflective layer B is preferably 0.1 ⁇ m or more, more preferably 0.2 ⁇ m or more, and even more preferably 0.3 ⁇ m or more.
  • the thickness of the reflective layer B is preferably 10.0 ⁇ m or less, more preferably 7.0 ⁇ m or less, and even more preferably 5.0 ⁇ m or less, in terms of further suppressing ghosts.
  • the thickness of the reflective layer B can be measured by preparing a cross section of the optical laminate and observing it with a transmission electron microscope.
  • the Rth of the reflective layer B is preferably from ⁇ 8 to ⁇ 800 nm, more preferably from ⁇ 16 to ⁇ 560 nm, and further preferably from ⁇ 24 to ⁇ 400 nm, at a wavelength of 550 nm.
  • the Rth of the reflective layer B may be measured by taking out only the reflective layer B from the optical laminate, or the Rth of a layer prepared under the same conditions as those for preparing the reflective layer B may be measured.
  • discotic liquid crystal compound contained in the liquid crystal layer 2 there are no particular limitations on the discotic liquid crystal compound contained in the liquid crystal layer 2, and any known discotic liquid crystal compound can be used.
  • the discotic liquid crystal compound described in paragraphs [0020] to [0122] of JP-A-2007-108732 can be suitably used.
  • a discotic liquid crystal compound When a discotic liquid crystal compound has a high ⁇ n characteristic, a high reflectance can be obtained even if the number of turns of the helical structure of the cholesteric liquid crystal phase is small, so that the desired reflection characteristic can be obtained even with a thin film thickness. By reducing the film thickness, the magnitude of the phase difference generated for incident light obliquely inclined from the normal direction of the cholesteric liquid crystal layer can be reduced, and as a result, ghosts can be further reduced.
  • the discotic compound having a high ⁇ n for example, the discotic liquid crystal compound described in paragraphs [0012] to [0108] of JP2010-244038A can be suitably used.
  • the refractive index anisotropy ⁇ n 550 (refractive index anisotropy at a wavelength of 550 nm) of the liquid crystal compound is preferably 0.12 or more, more preferably 0.16 or more, further preferably 0.20 or more, and most preferably 0.25 or more.
  • the upper limit of ⁇ n 550 (refractive index anisotropy at a wavelength of 550 nm) is preferably 0.90 or less, more preferably 0.70 or less, and even more preferably 0.50 or less, from the viewpoint of suppressing interface reflection.
  • the liquid crystal layer 2 may be any layer in which the orientation of the discotic liquid crystal compound in a cholesteric liquid crystal phase is maintained, and may typically be formed by aligning a polymerizable discotic liquid crystal compound having a polymerizable group in a cholesteric liquid crystal phase by a method such as adding a chiral agent, and then polymerizing and curing the compound by ultraviolet irradiation, heating, etc., to form a layer with no fluidity.
  • the liquid crystal layer 2 formed as described above may be any layer in which the orientation form is changed to a state in which it is not changed by an external field, external force, etc.
  • the optical properties of the cholesteric liquid crystal phase are maintained within the layer, and the discotic liquid crystal compound in the liquid crystal layer 2 does not need to exhibit liquid crystallinity any more.
  • the polymerizable discotic liquid crystal compound may be polymerized by a curing reaction and may have lost its liquid crystallinity.
  • the central wavelength ⁇ of the reflected light from liquid crystal layer 2 depends on the pitch of the helical structure in the cholesteric liquid crystal phase and can be defined in the same way as for liquid crystal layer 1 and measured in the same way.
  • the pitch of the cholesteric liquid crystal phase varies depending on the type of chiral agent used together with the polymerizable discotic liquid crystal compound and its concentration, and a cholesteric liquid crystal phase with the desired pitch can be obtained by adjusting one or more of the above.
  • the above-mentioned literature can be used as a reference for the direction of helix rotation and the method for measuring the pitch.
  • the pitch of the cholesteric liquid crystal phase may also change in the film thickness direction.
  • the state in which the pitch changes in the film thickness direction is called a pitch gradient, and the layer in which the pitch changes in the film thickness direction is called a pitch gradient layer.
  • the pitch gradient layer can be produced by a known method, for example, by referring to JP-A-2020-060627.
  • the pitch gradient layer the helical pitch changes in the film thickness direction, and therefore light in a plurality of wavelength ranges can be reflected.
  • the reflectance of the optical laminate of the first embodiment of the present invention for light having a wavelength of 400 to 700 nm is preferably 40% or more and less than 50%. When the reflectance is 40% or more, ghosts are more easily suppressed.
  • the light having a wavelength of 400 to 700 nm refers to non-polarized light.
  • the reflectance of the optical laminate for light having a wavelength of 400 to 700 nm is measured under the following conditions. For the measurement, an automatic absolute reflectance measurement system consisting of a UV-Vis-NIR spectrophotometer V-750 manufactured by JASCO Corporation is used. Polarized S-wave and P-wave light with wavelengths of 350 to 900 nm are incident on the optical laminate at an incident angle of 5°.
  • the absolute reflectance for each of the S-wave and P-wave is measured, and the average value is calculated for each wavelength to obtain a reflectance spectrum. From the obtained reflectance spectrum, the average reflectance for light with a wavelength of 400 to 700 nm is calculated, and this is regarded as the reflectance of the optical laminate for light with a wavelength of 400 to 700 nm.
  • the optical laminate of the first embodiment of the present invention includes the above-mentioned reflective layer A and reflective layer B.
  • the optical laminate preferably includes at least a blue light reflecting layer having a reflectance of 40% or more at a wavelength of 460 nm, a green light reflecting layer having a reflectance of 40% or more at a wavelength of 550 nm, a yellow light reflecting layer having a reflectance of 40% or more at a wavelength of 600 nm, and a red light reflecting layer having a reflectance of 40% or more at a wavelength of 650 nm.
  • the blue light reflecting layer, the green light reflecting layer, the yellow light reflecting layer, and the red light reflecting layer may each be either the reflecting layer A or the reflecting layer B.
  • the central wavelength of the reflected light of reflective layer A may be adjusted to about 460 nm by the above-mentioned method.
  • the central wavelength of the reflected light of reflective layer B may be adjusted to about 460 nm by the above-mentioned method.
  • the above reflectances are those when non-polarized light of each wavelength is incident on the reflective layer.
  • the optical laminate contains the above-mentioned blue light reflective layer, green light reflective layer, yellow light reflective layer and red light reflective layer, it may have two or more blue light reflective layers, may have two or more green light reflective layers, may have two or more yellow light reflective layers, or may have two or more red light reflective layers.
  • the central wavelength of the reflected light from the blue light reflecting layer is preferably within the range of 430 nm or more and less than 500 nm.
  • the central wavelength of the reflected light from the green light reflecting layer is preferably within the range of 500 nm or more and less than 570 nm.
  • the central wavelength of the reflected light from the yellow light reflecting layer is preferably within the range of 570 nm or more and less than 620 nm.
  • the central wavelength of the reflected light from the red light reflecting layer is preferably within the range of 620 nm or more and less than 670 nm.
  • the method for measuring the central wavelength of the reflected light is as described above.
  • the central wavelengths of the reflected light of the reflective layer A and the reflective layer B contained in the optical laminate may be adjusted so that the reflectance is 40% or more over the entire visible light region (wavelengths of 400 to 700 nm).
  • the optical laminate has the above-mentioned blue light reflective layer, green light reflective layer, yellow light reflective layer and red light reflective layer laminated in this order. Furthermore, when the optical laminate having the above-mentioned stacking order is applied to a reflective circular polarizer described later, the reflective layer on the long wavelength side (e.g., a red light reflective layer) requires a large thickness to obtain sufficient reflectance, and the effect of the Rth of the reflective layer itself on the light passing through the reflective layer becomes large. Therefore, it is preferable that the reflective layer arranged on the light source side is a reflective layer on the short wavelength side (e.g., a blue light reflective layer).
  • the reflective layer A has a positive Rth
  • the reflective layer B has a negative Rth, so that the Rths are offset by each other, as described above. Details of this will be described below.
  • L n (n is an integer of 4 or more) in order from the light source side
  • the sum of Rth of each layer from reflective layer L 1 to reflective layer L i (i is an integer of n or less) is defined as SRth i .
  • the absolute value of all of these SRth i is preferably 0.3 ⁇ m or less, more preferably 0.2 ⁇ m or less, and even more preferably 0.1 ⁇ m or less.
  • Rth i of each layer in the above formula is calculated by the above-mentioned formula for calculating Rth.
  • the liquid crystal compounds (rod-shaped liquid crystal compounds or discotic liquid crystal compounds) so that their orientation direction (slow axis direction) changes continuously at the interface in order to reduce the refractive index difference.
  • the above-mentioned arrangement can be achieved by directly applying a coating liquid containing a rod-shaped liquid crystal compound onto reflective layer B, and aligning the slow axis direction so that it is continuous at the interface due to the orientation control force of the discotic liquid crystal compound contained in reflective layer B.
  • the thickness of the optical laminate of the first embodiment of the present invention is preferably 30 ⁇ m or less, more preferably 15 ⁇ m or less.
  • the lower limit is not particularly limited, but may be, for example, 1 ⁇ m or more, and preferably 5 ⁇ m or more.
  • the optical laminate of the present invention includes an optical interference layer, the refractive index of which satisfies the following conditions. That is, when the refractive index of the adhesive layer adjacent to the optical interference layer is nA, and the average refractive index of the reflective layer A and the reflective layer B of the laminated reflective layer adjacent to the optical interference layer is nL, the refractive index nI of the optical interference layer is (nA ⁇ nL) 1/2 ⁇ 0.03 ⁇ nI ⁇ (nA ⁇ nL) 1/2 +0.03 It is.
  • the refractive index nI of the optical interference layer is (nA ⁇ nL) 1/2 ⁇ 0.03 ⁇ nI ⁇ (nA ⁇ nL) 1/2 +0.03 It is.
  • the refractive index nA of the adhesive layer 28, the average refractive index nL of the reflective layer A 21a, and the refractive index nI of the optical interference layer 27 satisfy the above relationship.
  • the refractive index nA of the adhesive layer adjacent to the optical interference layer, the average refractive index nL of the reflective layer A and the reflective layer B of the laminated reflective layer adjacent to the optical interference layer, and the refractive index nI of the optical interference layer are (nA ⁇ nL) 1/2 -0.02 ⁇ nI ⁇ (nA ⁇ nL) 1/2 +0.02 It is preferable to satisfy (nA ⁇ nL) 1/2 -0.01 ⁇ nI ⁇ (nA ⁇ nL) 1/2 +0.01 It is more preferable that the following conditions are satisfied: In the laminated reflective layer, either the reflective layer A or the reflective layer B may be adjacent to the optical interference layer.
  • the average refractive index of the reflective layer A or the reflective layer B adjacent to the optical interference layer of the laminated reflective layer is nL
  • nL the average refractive index of the reflective layer A
  • the refractive index of the optical interference layer By setting the refractive index of the optical interference layer within this range, it is possible to make the amplitude reflectances on both sides of the optical interference layer approximately equal, which is believed to result in a significant anti-reflection effect. That is, in the case where the optical laminate does not have an optical interference layer, the reflective layer and the adhesive layer of the laminated reflective layer are adjacent to each other. In the case of the optical laminate 10 shown in Fig. 1, the reflective layer A21a and the adhesive layer 28 are adjacent to each other. At the interface between the two layers, reflection occurs at the interface according to the difference in refractive index.
  • the cholesteric liquid crystal layer (reflective layer) of the laminated reflective layer reflects right-handed circularly polarized light
  • left-handed circularly polarized light unnecessarily passes through the laminated reflective layer
  • this light becomes a ghost.
  • the reflective layer constituting the laminated reflective layer reflects the right-handed circularly polarized light toward the adhesive layer side.
  • a part of the right-handed circularly polarized light reflected by the reflective layer (cholesteric liquid crystal layer) is reflected at the interface between the reflective layer and the adhesive layer of the laminated reflective layer.
  • the reflective layer (cholesteric liquid crystal layer) of the laminated reflective layer reflects right-handed circularly polarized light, so left-handed circularly polarized light is transmitted. This unnecessarily transmitted left-handed circularly polarized light becomes a ghost.
  • the optical laminate of the present invention has an optical interference layer having the above-mentioned refractive index between the laminated reflective layer and the adhesive layer. The optical laminate of the present invention has such an optical interference layer, so that the difference in refractive index at the interface of the layer existing between the laminated reflective layer and the adhesive layer can be reduced.
  • the optical laminate of the present invention has such an optical interference layer, so that the difference in refractive index between the reflective layer adjacent to the optical interference layer and the optical interference layer, and the difference in refractive index between the optical interference layer and the adhesive layer can be reduced.
  • the optical laminate of the present invention can thereby reduce the interfacial reflection at the interface between the reflective layer and the adhesive layer, and suppress a change in the rotation direction of circularly polarized light caused by interfacial reflection, for example, a change from right-handed circularly polarized light to left-handed circularly polarized light caused by interfacial reflection.
  • the refractive indexes of the optical interference layer, the reflective layer and the adhesive layer can be measured by referring to the method described in the Examples.
  • the refractive index of each layer is the refractive index for light having a wavelength of 550 nm.
  • the thickness of the optical interference layer is in the range of 60 to 110 nm, or 230 to 330 nm.
  • the difference in refractive index between the reflective layer adjacent to the optical interference layer of the laminated reflective layer and the optical interference layer, and the difference in refractive index between the optical interference layer and the adhesive layer are small, so that the reflection at this interface can be reduced.
  • some interfacial reflection occurs between the two interfaces.
  • the optical laminate of the present invention can suitably shift the phase of the reflected light at both interfaces by setting the film thickness of the optical interference layer within the above range, so that the reflected light at both interfaces can be canceled out.
  • the thickness of the optical interference layer is preferably in the range of 75 to 100 nm or 245 to 300 nm, and more preferably in the range of 80 to 95 nm or 260 to 285 nm.
  • the material for forming the optical interference layer can be a hard coat material obtained by crosslinking a monomer, a photo-alignment film, or a C-plate using a liquid crystal material.
  • the C plate is more preferable because it can also play a role in optical compensation adjustment.
  • a positive C plate is more preferable.
  • the positive C plate is a retardation layer having Re substantially zero and Rth having a negative value.
  • the positive C plate can be obtained, for example, by vertically aligning a rod-shaped liquid crystal compound.
  • the positive C plate functions as an optical compensation layer for increasing the degree of polarization of transmitted light with respect to obliquely incident light.
  • the positive C plate can be installed at any position of the laminated optical film, and a plurality of positive C plates may be installed.
  • the Re(550) of the C plate is preferably about 10 nm or less, and the Rth(550) is preferably -100 to -1 nm, and more preferably -30 to -5 nm.
  • a material for an interlayer photo-alignment film is present between the optical interference layer and the laminated reflective layer.
  • the material for an interlayer photo-alignment film may be contained in the optical interference layer. This allows the liquid crystal compound to be aligned when a liquid crystal material is applied onto the optical interference layer, and allows the formation of a structure in which the optical interference layer and the reflective layer are adjacent to each other.
  • a material for the interlayer photoalignment film the photoalignment polymer described in JP-A-2021-143336 can be used.
  • the material for the interlayer photo-alignment film is preferably a compound having a cinnamoyl group.
  • the optical interference layer is a C plate
  • the compound having a cinnamoyl group i.e., the cinnamoyl compound
  • the cinnamoyl compound exists between the optical interference layer and the laminated reflective layer. That is, it is preferable that the cinnamoyl compound exists in the region near the boundary between the optical interference layer (preferably the C plate) and the laminated reflective layer.
  • the hard coat layer is not particularly limited as long as it satisfies the above-mentioned requirements regarding nI, and any known hard coat layer can be used.
  • An example of a method for forming the hard coat layer is a method in which a curable composition containing a crosslinkable monomer is applied onto the outermost cholesteric liquid crystal layer to form a coating layer, and the formed coating layer is cured to form the hard coat layer.
  • the crosslinkable monomer contained in the curable composition may be a monomer having a crosslinkable group.
  • the crosslinkable group is not particularly limited, but may be a radical polymerizable group or a cationically polymerizable group.
  • the radical polymerizable group is not particularly limited, but examples thereof include vinyl group, butadiene group, (meth)acryloyl group, (meth)acrylamide group, vinyl acetate group, fumaric acid ester group, styryl group, vinylpyrrolidone group, and maleimide group, and (meth)acrylic group is preferable.
  • the (meth)acryloyl group represents a concept including acryloyl group and methacryloyl group.
  • the cationically polymerizable group is not particularly limited, but examples thereof include a vinyl ether group, an epoxy group, and an oxetanyl group.
  • the monomer having a crosslinkable group may be used alone or in combination of two or more types.
  • the curable composition may also contain a polymerization initiator.
  • the polymerization initiator may be a known polymerization initiator such as a photopolymerization initiator or a thermal polymerization initiator.
  • the refractive index of the hard coat layer can be adjusted, for example, by the refractive index of the crosslinkable monomer contained in the curable composition.
  • the refractive index of the hard coat layer can be increased by using a crosslinkable monomer having an aromatic ring or the like in the molecule as the crosslinkable monomer, whereas the refractive index of the hard coat layer can be decreased by using a crosslinkable monomer not having an aromatic ring or the like in the molecule as the crosslinkable monomer.
  • the refractive index of the hard coat layer can be adjusted by mixing inorganic oxide fine particles in the curable composition.
  • Photo-alignment film As the optical interference layer, it is also a preferred embodiment to use a so-called optical alignment film (optical alignment layer) in which an optical alignment material is irradiated with polarized or non-polarized light to form an alignment layer. It is preferable that the photo-alignment film is provided with an alignment regulating force by a step of irradiating the film with polarized light from a vertical or oblique direction, or by irradiating the film with non-polarized light from an oblique direction. By using the photo-alignment film, it is possible to horizontally align a specific liquid crystal compound with excellent symmetry.
  • the retardation layer positive A plate formed by using the photo-alignment film is useful for optical compensation in a liquid crystal display device that does not require a pre-tilt angle of the driving liquid crystal, such as an IPS (In-Place-Switching) mode liquid crystal display device.
  • IPS In-Place-Switching
  • photo-alignment materials used in the photo-alignment film include those described in JP-A-2006-285197, JP-A-2007-076839, JP-A-2007-138138, JP-A-2007-094071, JP-A-2007-121721, JP-A-2007-140465, JP-A-2007-156439, and JP-A-2007- azo compounds described in JP-A-133184, JP-A-2009-109831, JP-A-3883848 and JP-A-4151746; aromatic ester compounds described in JP-A-2002-229039; maleimides having photo-orienting units described in JP-A-2002-265541 and JP-A-2002-317013; and/or alkenyl-substituted nadimide compounds, photocrosslinkable silane derivatives described in Japanese Patent No.
  • the optical layered body of the present invention includes an adhesive layer.
  • This adhesive layer is used to attach the optical laminate of the present invention to some optical member (optical component).
  • the optical laminate of the present invention is used as a reflective circular polarizer of a virtual reality display device described later, the optical laminate of the present invention is attached to the lens of the optical system (pancake lens) constituting the virtual reality display device by the adhesive layer.
  • the adhesive layer may be made of any known adhesive or pressure-sensitive adhesive as long as it has a refractive index that satisfies the above-mentioned relational expression.
  • the adhesive or pressure-sensitive adhesive used in the laminated optical film described below may be used.
  • There is no limitation on the thickness of the adhesive layer and the thickness that provides the necessary adhesive strength may be appropriately set depending on the material from which the adhesive layer is formed.
  • optical laminate of the present invention (first embodiment) can be produced by a known method, and the method is not particularly limited.
  • the manufacturing method of the first embodiment may include a method of applying a composition containing a rod-shaped liquid crystal compound onto a substrate to form a cholesteric liquid crystal phase, then fixing the orientation state of the cholesteric liquid crystal phase to form a first cholesteric liquid crystal layer, applying a composition containing a discotic liquid crystal compound onto the first cholesteric liquid crystal layer to form a cholesteric liquid crystal phase, then fixing the orientation state of the cholesteric liquid crystal phase to form a second cholesteric liquid crystal layer, forming a third cholesteric liquid crystal layer on the second cholesteric liquid crystal layer in the same manner as the first cholesteric liquid crystal layer, and forming a fourth cholesteric liquid crystal layer on the third cholesteric liquid crystal layer in the same manner as the second cholesteric liquid crystal layer.
  • the first cholesteric liquid crystal layer and the third cholesteric liquid crystal layer correspond to the reflective layer A of the first embodiment
  • an optical interference layer is formed on the surface of the laminated reflective layer.
  • the method for forming the light interference layer there is no limitation on the method for forming the light interference layer, and it may be appropriately selected depending on the material for forming the light interference layer.
  • the light interference layer is a positive C plate using a liquid crystal compound
  • a composition containing the liquid crystal compound constituting the positive C plate is prepared, the composition is applied to the surface of the laminated reflective layer, dried, and then the liquid crystal compound is cured by irradiation with ultraviolet light or the like to form the light interference layer.
  • the light interference layer is a hard coat layer
  • a composition containing a polymerizable compound that will become the hard coat layer is prepared, the composition is applied to the surface of the laminated reflective layer, dried, and then the polymerizable compound is cured by irradiation with ultraviolet light or the like to form the light interference layer.
  • the optical interference layer is a photo-alignment film
  • a composition containing a compound that forms a photo-alignment film is prepared, and this composition is applied to the surface of the laminated reflective layer, dried, and then the polymerizable compound is cured by irradiation with ultraviolet light or the like to form the optical interference layer.
  • the optical interference layer is formed on the laminated reflective layer, but conversely, the optical interference layer may be formed first, and then the reflective layer (cholesteric liquid crystal layer) may be formed on the optical interference layer using the above-mentioned composition.
  • an adhesive layer is formed on this optical interference layer to obtain the optical laminate of the present invention.
  • the method for forming the adhesive layer is not limited, and various known methods can be used depending on the material for forming the adhesive layer. Therefore, the adhesive layer may be formed by a coating method or by attaching a sheet-like pressure-sensitive adhesive layer.
  • the adhesive layer may be formed when the optical laminate of the present invention is attached to an optical member (optical component) using the optical laminate of the present invention.
  • a composition that becomes an adhesive layer may be applied to an optical member (optical component) using the optical laminate of the present invention and/or the light interference layer of the laminate of the laminate of the laminated reflective layer and the light interference layer prepared as described above, and the adhesive layer may be used to bond the optical member and the laminate of the laminated reflective layer and the light interference layer to form an adhesive layer in the optical laminate of the present invention.
  • an adhesive layer made of a pressure-sensitive adhesive or the like may be provided in an optical member (optical component) using the optical laminate of the present invention, and the laminate of the laminated reflective layer and the light interference layer prepared as described above may be laminated on the adhesive layer with the light interference layer side facing and attached to form an adhesive layer in the optical laminate of the present invention.
  • the reflection wavelength range of the reflective circular polarizer may shift to the short wavelength side when the reflective circular polarizer is stretched or molded. Therefore, it is preferable to manufacture the optical laminate in advance, assuming the shift in the reflection wavelength range.
  • the optical laminate may be stretched by stretching and molding, and the helical pitch of the cholesteric liquid crystal phase may become small, so it is preferable to set the helical pitch of the cholesteric liquid crystal phase large in advance.
  • the optical laminate has an infrared light reflective layer with a reflectance of 40% or more at a wavelength of 800 nm.
  • the optical laminate may be manufactured by selecting an appropriate reflection wavelength range in accordance with the wavelength shift caused by stretching at each location in the plane of the optical laminate. That is, there may be regions in the plane of the optical laminate with different reflection wavelength ranges. It is also preferable to set the reflection wavelength range wider than the required wavelength range in advance, assuming that the stretching ratio is different at each location in the plane of the optical laminate.
  • the above describes a method of forming a cholesteric liquid crystal layer by applying a composition for forming a cholesteric liquid crystal layer directly onto each cholesteric liquid crystal layer, and a method of forming a light interference layer by applying a composition for forming a light interference layer directly onto a reflective layer consisting of a cholesteric liquid crystal layer.
  • the manufacturing method of the optical laminate of the present invention is not limited thereto, and the cholesteric liquid crystal layer and/or the optical interference layer may be formed by coating each on a separate substrate, and the cholesteric liquid crystal layer and the optical interference layer may be laminated via an adhesion layer (sticking layer) such as an adhesive layer or a pressure-sensitive adhesive layer.
  • the adhesive used in the adhesive layer can be any commercially available adhesive.
  • the thickness of the adhesive is preferably 25 ⁇ m or less, more preferably 15 ⁇ m or less, and even more preferably 6 ⁇ m or less.
  • the adhesive is one that is unlikely to generate outgassing.
  • the adhesive used in the adhesive layer may be any commercially available adhesive, such as an epoxy resin adhesive or an acrylic resin adhesive.
  • the adhesive has a thickness of preferably 25 ⁇ m or less, more preferably 5 ⁇ m or less, and even more preferably 1 ⁇ m or less.
  • the adhesive has a viscosity of preferably 300 cP or less, more preferably 100 cP or less.
  • the pressure-sensitive adhesive and adhesive can be selected with appropriate viscoelasticity or thickness so as to bury the surface irregularities of the layer to be adhered, from the viewpoint of reducing the surface roughness Ra of the reflective circular polarizer using the optical laminate.
  • the pressure-sensitive adhesive and adhesive preferably have a viscosity of 50 cP or more.
  • the thickness is preferably thicker than the height of the surface irregularities.
  • a method for adjusting the viscosity of the adhesive for example, a method of using an adhesive containing a solvent can be mentioned. In this case, the viscosity of the adhesive can be adjusted by the ratio of the solvent. In addition, the thickness of the adhesive can be further reduced by drying the solvent after applying the adhesive to the adherend.
  • the pressure-sensitive adhesive or adhesive used for bonding each layer has a small refractive index difference with adjacent layers.
  • the difference between the refractive index n ave of the adjacent adhesive layer or bonding layer is preferably 0.075 or less, more preferably 0.05 or less, and even more preferably 0.025 or less.
  • the refractive index of the adhesive or bonding agent can be adjusted, for example, by mixing titanium oxide fine particles and zirconia fine particles.
  • the adhesive layer between each layer is preferably 100 nm or less in thickness.
  • the thickness of the adhesive layer is more preferably 50 nm or less, and further preferably 30 nm or less.
  • a method for forming an adhesive layer having a thickness of 100 nm or less includes, for example, a method of depositing a ceramic adhesive such as silicon oxide (SiOx layer) on the bonding surface.
  • the bonding surface of the bonding member may be subjected to a surface modification treatment such as plasma treatment, corona treatment, and saponification treatment before bonding, and a primer layer may be applied.
  • an adhesive layer having a thickness of 100 nm or less can be provided by the following steps (1) to (3).
  • the layers to be laminated are attached to a temporary support made of a glass substrate.
  • a SiOx layer having a thickness of 100 nm or less is formed by deposition or the like.
  • the deposition can be performed using, for example, a deposition device (model number ULEYES) manufactured by ULVAC, Inc., using SiOx powder as a deposition source.
  • the temporary support is peeled off.
  • the bonding is preferably performed at a temperature of, for example, 120°C.
  • the coating, adhesion or lamination of each layer may be performed by a roll-to-roll method or a sheet-fed method.
  • the roll-to-roll method is preferable from the viewpoints of improving productivity and reducing axial misalignment of each layer.
  • the single-wafer system is preferable in that it is suitable for small-lot, high-mix production and that it allows the selection of a special bonding method such as one that results in an adhesive layer having a thickness of 100 nm or less, as described above.
  • Methods for applying the adhesive to the adherend include known methods such as roll coating, gravure printing, spin coating, wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spraying, and inkjet printing.
  • the reflective circular polarizer using the optical laminate of the present invention may include a support and an orientation layer, etc., but the support and the orientation layer may be a temporary support that is peeled off and removed when preparing the laminated optical film described later.
  • the reflective circular polarizer is transferred to another laminate, and then the temporary support is peeled off and removed, so that the laminated optical film can be made thin, and further, the retardation of the temporary support can be eliminated from the adverse effect on the polarization degree of transmitted light, which is preferable.
  • the type of the support is not particularly limited, but is preferably transparent to visible light, and for example, films of cellulose acylate, polycarbonate, polysulfone, polyethersulfone, polyacrylate and polymethacrylate, cyclic polyolefin, polyolefin, polyamide, polystyrene, and polyester can be used. Among them, cellulose acylate film, cyclic polyolefin, polyacrylate, and polymethacrylate are preferred. Commercially available cellulose acetate films (for example, "TD80U” and "Z-TAC” manufactured by Fujifilm Corporation) can also be used.
  • the support When the support is a temporary support, it is preferable to use a support having high tear strength in order to prevent breakage during peeling, such as polycarbonate and polyester films.
  • the support preferably has a small phase difference from the viewpoint of suppressing the adverse effect on the polarization degree of transmitted light.
  • the magnitude of Re at 550 nm is preferably 10 nm or less
  • the absolute value of the magnitude of Rth is preferably 50 nm or less.
  • the phase difference of the temporary support is small in order to perform quality inspection of the reflective circular polarizer and other laminates.
  • the reflective circular polarizer using the optical laminate used in the laminated optical film described below is transparent to near-infrared light.
  • the laminated optical film of the present invention has at least a reflective circular polarizer, a retardation layer that converts circularly polarized light into linearly polarized light, and a linear polarizer, in this order.
  • the above-mentioned optical laminate (first embodiment) of the present invention is used as a reflective circular polarizer.
  • a preferred embodiment of the optical laminate (first embodiment) is as described above.
  • the virtual reality display device of the present invention includes the optical component of the present invention, which will be described later.
  • FIG. 3 is a schematic diagram of a virtual reality display device using the laminated optical film of the present invention.
  • a laminated optical film 100 having a reflective circular polarizer using the above-mentioned optical laminate, a lens 200, a half mirror 300, a circular polarizing plate 400, and an image display panel 500 are arranged in order from the viewing side.
  • a linear polarizer, a retardation layer, and a reflective circular polarizer are arranged in this order from the viewing side in the laminated optical film 100.
  • the laminated optical film 100 is attached to the lens 200 by the adhesive layer of the reflective circular polarizer, i.e., the optical laminate of the present invention.
  • the circular polarizer 400 converts the light (image) emitted by the image display panel 500 into right-handed circularly polarized light and transmits it.
  • the reflective layer of the laminated reflective layer constituting the reflective circular polarizer is a cholesteric liquid crystal layer that selectively reflects right-handed circularly polarized light.
  • the retardation layer and the linear polarizer have their slow axes and transmission axes set so that when left-handed circularly polarized light is incident from the retardation layer side, the converted linearly polarized light is transmitted.
  • a light ray 1000 (a light ray 1000 forming a virtual image) emitted from the image display panel 500 passes through the circular polarizer 400 to become circularly polarized light (right-handed circularly polarized light), and passes through the half mirror 300 .
  • the light ray 1000 enters the laminated optical film 100 of the present invention from the side of the reflective circular polarizer, is totally reflected, is reflected again by the half mirror 300, and enters the laminated optical film 100 again.
  • the light ray 1000 is reflected by the half mirror and becomes circularly polarized light (left circularly polarized light) having a rotation direction opposite to that of the circularly polarized light when it entered the laminated optical film 100 the first time.
  • the light ray 1000 passes through the laminated optical film 100 and is visually recognized by the user. Furthermore, when the light beam 1000 is reflected by the half mirror 300, the image displayed on the image display panel 500 is magnified by the half mirror 300 and the lens 200 because the half mirror has a concave mirror shape, and the user can visually recognize the magnified virtual image.
  • the above-mentioned mechanism is called a reciprocating optical system or a folded optical system.
  • FIG. 4 is a schematic diagram for explaining a case where a ghost occurs in the virtual reality display device shown in FIG. More specifically, in a virtual reality display device, when a light ray 2000 (a light ray 2000 forming a ghost) is incident on the laminated optical film 100 for the first time, it is not properly reflected but is transmitted, resulting in leakage light. As shown in Fig. 4, when the light ray 2000 is incident on the laminated optical film 100 for the first time, it is not reflected but is transmitted, resulting in leakage light, and as can be seen from Fig. 4, the user will see an image that is not magnified. This image is called a ghost or the like, and it is desired to reduce it.
  • a ghost or the like an image that is not magnified.
  • the reflective circular polarizer that is, the optical laminate of the present invention
  • the optical laminate 10 shown in Fig. 1 is illustrated as an example.
  • right-handed circularly polarized light that is emitted from the image display panel 500 and transmitted through the circular polarizer 400 enters from the lens 200 side, transmits through the adhesive layer 28, and is reflected toward the adhesive layer 28 by the reflective layers A 21a to B 24b.
  • a part of the right-handed circularly polarized light (light ray 1000) is reflected at the interface between the adhesive layer 28 and the reflective layer A21a.
  • the right-handed circularly polarized light is converted into left-handed circularly polarized light.
  • this left-handed circularly polarized light passes through the reflective layers A21a to B24b, the retardation layer, and the linear polarizer, i.e., the laminated optical film 100, and is visually recognized by the user as a ghost.
  • the optical laminate of the present invention has an optical interference layer 27 between an adhesive layer 28 and a reflective layer A 21a (laminated reflective layer), as conceptually shown in FIG.
  • the refractive index nI of the optical interference layer 27 is expressed as follows: (nA ⁇ nL) 1/2 -0.03 ⁇ nI ⁇ (nA ⁇ nL) 1/2 +0.03 Meet the following.
  • the optical laminate of the present invention can reduce the difference in refractive index at the interface between the laminated reflective layer (reflective layer) and the adhesive layer.
  • the difference in refractive index between the reflective layer (reflective layer A21a) adjacent to the optical interference layer of the laminated reflective layer and the optical interference layer 27, and the difference in refractive index between the optical interference layer 27 and the adhesive layer 28 can be reduced.
  • the optical laminate of the present invention can reduce interfacial reflection at the interface between the adhesive layer 28 and the reflective layer A21a, i.e., the interface between the reflective layer A21a and the optical interference layer 27, and the interface between the optical interference layer 27 and the adhesive layer 28.
  • the optical laminate of the present invention has such a configuration, and thus can suppress a change in the rotation direction of circularly polarized light caused by interfacial reflection, for example, a change from right-handed circularly polarized light (light ray 1000) to left-handed circularly polarized light (light ray 2000).
  • a change in the rotation direction of circularly polarized light caused by interfacial reflection for example, a change from right-handed circularly polarized light (light ray 1000) to left-handed circularly polarized light (light ray 2000).
  • ghosting can be reduced by using the optical laminate of the present invention as, for example, reflected circularly polarized light in a virtual reality display device.
  • the film thickness of the optical interference layer 27 is in the range of 60 to 110 nm, or 230 to 330 nm.
  • the difference in refractive index between the reflective layer A21a adjacent to the optical interference layer 27 and the optical interference layer 27, and the difference in refractive index between the optical interference layer 27 and the adhesive layer 28 are small, so that reflection at this interface can be reduced.
  • some interfacial reflection occurs between both interfaces.
  • the film thickness of the optical interference layer 27, that is, the distance between the interfaces that reflect light is set within the above range.
  • this configuration can suitably shift the phase of the light (light ray 2000) reflected at the interface between the reflective layer A21a and the optical interference layer 27 from the phase of the light (light ray 2000) reflected at the interface between the optical interference layer 27 and the adhesive layer 28.
  • this configuration can preferably shift the phase of the light reflected at the interface between the reflective layer A21a and the optical interference layer 27 from the phase of the light reflected at the interface between the optical interference layer 27 and the adhesive layer 28 by ⁇ /2. Therefore, according to the optical laminate of the present invention, the reflected light at both interfaces can be cancelled out, and as a result, according to the optical laminate of the present invention, ghosts caused by unnecessary light reflection at the interfaces can be further reduced.
  • the laminated optical film 100 of the present invention having a laminated reflective layer including the above-mentioned reflective layer A and reflective layer B has a high polarization degree, so that leakage of transmitted light (i.e., ghost) when a light ray is incident on the laminated optical film 100 for the first time can be reduced.
  • the laminated optical film 100 of the present invention since the laminated optical film 100 of the present invention has a high degree of polarization even for transmitted light, it is possible to increase the transmittance when a light ray enters the laminated optical film 100 for the second time, thereby improving the brightness of the virtual image and further suppressing coloring of the virtual image.
  • the laminated optical film 100 may be formed onto a curved surface such as a lens.
  • Conventional optical films which are conventionally known as reflective circular polarizers and are formed by laminating a reflective linear polarizer and a retardation layer having a phase difference of 1/4 wavelength, have optical axes such as a transmission axis, a reflection axis, and a slow axis, and therefore the optical axes are distorted when stretched and molded into a curved shape, thereby reducing the degree of polarization of transmitted light.
  • the laminated optical film 100 of the present invention is less likely to suffer from a reduction in the degree of polarization due to stretching and molding, since the reflective circular polarizer (optical laminate) does not have an optical axis. Therefore, the laminated optical film 100 is less likely to suffer from a reduction in the degree of polarization even when molded into a curved shape.
  • FIG. 1 An example of the layer structure of the laminated optical film 100 of the present invention is shown in FIG.
  • a reflective circular polarizer 103, a positive C plate 104, a retardation layer 105, and a linear polarizer 106 are arranged in this order.
  • the optical laminate of the present invention is used for the reflective circular polarizer 103.
  • the laminated optical film 100 shown in Fig. 5 has the positive C plate 104 as a preferred embodiment, the laminated optical film of the present invention does not necessarily have the positive C plate 104.
  • the laminated optical film of the present invention has, in this order, a reflective circular polarizer 103, a retardation layer 105 that converts circularly polarized light into linearly polarized light, and a linear polarizer 106, and therefore leaked light from the reflective circular polarizer 103 can be converted into linearly polarized light and then absorbed by the linear polarizer, thereby increasing the degree of polarization of transmitted light.
  • a reflective circular polarizer 103 When the laminated optical film is stretched or molded, there is a concern that the slow axis of the retardation layer and the absorption axis of the linear polarizer may be distorted.
  • the reflective circular polarizer retains a high degree of polarization even after stretching and molding, and the amount of leaked light from the reflective circular polarizer is small, so that the increase in leaked light is kept to a small amount.
  • the laminated optical film of the present invention preferably has a surface roughness Ra of 100 nm or less. If Ra is small, for example, when the laminated optical film is used in a virtual reality display device or the like, the sharpness of the image can be improved.
  • the present inventors presume that when light is reflected in the laminated optical film, if there are irregularities, the angle of the reflected light is distorted, leading to image distortion and blurring.
  • the Ra of the laminated optical film is more preferably 50 nm or less, even more preferably 30 nm or less, and particularly preferably 10 nm or less.
  • the laminated optical film of the present invention is produced by laminating a large number of layers.
  • each layer of the laminated optical film of the present invention preferably has Ra of 50 nm or less, more preferably 30 nm or less, and even more preferably 10 nm or less. From the viewpoint of increasing the image sharpness of a reflected image, it is particularly preferable that the Ra of the reflective circular polarizer is small.
  • the surface roughness Ra can be measured, for example, by using a non-contact surface/layer cross-sectional shape measuring system VertScan (manufactured by Ryoka Systems Co., Ltd.). Since Vertscan is a surface shape measurement method that utilizes the phase of reflected light from a sample, when measuring a reflective circular polarizer (above-mentioned optical laminate) consisting of a reflective layer formed by fixing a cholesteric liquid crystal phase, the reflected light from inside the film may overlap and the surface shape may not be measured accurately.
  • a metal layer may be formed on the surface of the sample to increase the reflectance of the surface and further suppress reflection from the inside.
  • a sputtering method is used as a method for forming a metal layer on the surface of the sample. Au, Al, Pt, etc. are used as materials to be sputtered.
  • the laminated optical film of the present invention preferably has a small number of point defects per unit area. Since the laminated optical film of the present invention is produced by laminating a large number of layers, in order to reduce the number of point defects in the laminated optical film as a whole, it is preferable that the number of point defects in each layer is also small. Specifically, the number of point defects in each layer is preferably 20 or less per square meter, more preferably 10 or less, and even more preferably 1 or less. In the laminated optical film as a whole, the number of point defects is preferably 100 or less per square meter, more preferably 50 or less, and even more preferably 5 or less.
  • Point defects lead to a decrease in the degree of polarization of transmitted light and a decrease in image sharpness, so it is preferable to have as few point defects as possible.
  • point defects include foreign matter, scratches, stains, film thickness variations, and alignment defects of liquid crystal compounds.
  • the number of point defects is preferably counted by counting the number of point defects having a size of 100 ⁇ m or more, more preferably 30 ⁇ m or more, and even more preferably 10 ⁇ m or more.
  • various sensors that use near-infrared light as a light source such as for eye tracking, facial expression recognition, and iris authentication, may be incorporated into the optical systems of virtual reality display devices and electronic viewfinders, and in order to minimize the effects on the sensors, it is preferable that the laminated optical film of the present invention is transparent to near-infrared light.
  • the retardation layer used in the laminated optical film of the present invention has a function of converting the emitted light into approximately linearly polarized light when circularly polarized light is incident.
  • a retardation layer having an Re of approximately 1/4 wavelength at any wavelength in the visible range can be used.
  • the in-plane retardation Re(550) at a wavelength of 550 nm is preferably 120 to 150 nm, more preferably 125 to 145 nm, and even more preferably 135 to 140 nm.
  • retardation layers having Re of about 3/4 wavelength and Re of about 5/4 wavelength are also preferable because they can convert linearly polarized light into circularly polarized light.
  • the retardation layer used in the laminated optical film of the present invention preferably has a reverse dispersion with respect to wavelength. If it has a reverse dispersion, it is preferable because it can convert circularly polarized light into linearly polarized light over a wide wavelength range in the visible range.
  • having a reverse dispersion with respect to wavelength means that the value of retardation at the wavelength increases as the wavelength increases.
  • the retardation layer having reverse dispersion can be produced by uniaxially stretching a polymer film such as a modified polycarbonate resin film having reverse dispersion, for example, with reference to JP-A-2017-049574.
  • the retardation layer having reverse dispersion may have substantially reverse dispersion, and for example, as disclosed in Japanese Patent No.
  • a retardation layer having Re of approximately 1/4 wavelength and a retardation layer having Re of approximately 1/2 wavelength can be prepared by laminating them so that their slow axes form an angle of approximately 60°.
  • the 1/4 wavelength retardation layer and the 1/2 wavelength retardation layer each have normal dispersion (the value of the retardation at the wavelength decreases as the wavelength increases)
  • circularly polarized light can be converted into linearly polarized light over a wide wavelength range in the visible range and can be considered to have substantially reverse dispersion.
  • the laminated optical film of the present invention has a reflective circular polarizer, a 1/4 wavelength retardation layer, a 1/2 wavelength retardation layer, and a linear polarizer in this order.
  • the retardation layer used in the laminated optical film of the present invention preferably has a layer in which a uniformly aligned liquid crystal compound is fixed.
  • a layer in which a rod-shaped liquid crystal compound is uniformly aligned horizontally to the in-plane direction and a layer in which a discotic liquid crystal compound is uniformly aligned vertically to the in-plane direction can be used.
  • a retardation layer having reverse dispersion can be produced by uniformly aligning and fixing a rod-shaped liquid crystal compound having reverse dispersion.
  • the retardation layer used in the laminated optical film of the present invention preferably has a layer formed by fixing a liquid crystal compound that is twisted and aligned with the thickness direction as a helical axis.
  • a retardation layer having a layer formed by fixing a rod-shaped liquid crystal compound or a discotic liquid crystal compound that is twisted and aligned with the thickness direction as a helical axis can be used.
  • the retardation layer can be considered to have substantially reverse dispersion, which is preferable.
  • the thickness of the retardation layer is not particularly limited, but from the viewpoint of achieving a thin film, it is preferably 0.1 to 8 ⁇ m, and more preferably 0.3 to 5 ⁇ m.
  • the retardation layer may include a support, an alignment layer, and the like.
  • the support and the orientation layer may be a temporary support that is peeled off and removed when preparing the laminated optical film.When using a temporary support, the retardation layer is transferred to another laminate, and then the temporary support is peeled off and removed, so that the laminated optical film can be thinned, and further, the retardation of the temporary support can be eliminated from the adverse effect on the polarization degree of transmitted light, which is preferable.
  • the type of the support is not particularly limited, but is preferably transparent to visible light, and for example, films such as cellulose acylate, polycarbonate, polysulfone, polyethersulfone, polyacrylate, polymethacrylate, cyclic polyolefin, polyolefin, polyamide, polystyrene, and polyester can be used. Among them, cellulose acylate film, cyclic polyolefin, polyacrylate, and polymethacrylate are preferred. In addition, a commercially available cellulose acetate film can also be used as the support. Examples of commercially available cellulose acetate films include "TD80U" and "Z-TAC" manufactured by Fujifilm Corporation.
  • the support When the support is a temporary support, it is preferable to use a support having high tear strength in order to prevent breakage during peeling, such as polycarbonate and polyester films.
  • the support preferably has a small phase difference from the viewpoint of suppressing the adverse effect on the polarization degree of transmitted light.
  • the magnitude of Re(550) is preferably 10 nm or less
  • the absolute value of the magnitude of Rth is preferably 50 nm or less.
  • the phase difference of the temporary support is small in quality inspection of the retardation layer and other laminates.
  • the retardation layer used in the laminated optical film of the present invention is preferably transparent to near-infrared light.
  • the linear polarizer used in the laminated optical film of the present invention is preferably an absorptive linear polarizer, which absorbs linearly polarized light in the absorption axis direction of incident light and transmits linearly polarized light in the transmission axis direction.
  • a general polarizer can be used, for example, a polarizer in which a dichroic material is dyed on polyvinyl alcohol or other polymer resin and then stretched to be oriented, or a polarizer in which a dichroic material is oriented by utilizing the orientation of a liquid crystal compound may be used.
  • a polarizer in which polyvinyl alcohol is dyed with iodine and then stretched is preferred.
  • the thickness of the linear polarizer is preferably 10 ⁇ m or less, more preferably 7 ⁇ m or less, and even more preferably 5 ⁇ m or less.
  • the single plate transmittance of the linear polarizer is preferably 40% or more, more preferably 42% or more.
  • the degree of polarization is preferably 90% or more, more preferably 95% or more, and even more preferably 99% or more.
  • the single plate transmittance and degree of polarization of the linear polarizer are measured using an automatic polarizing film measuring device: VAP-7070 (manufactured by JASCO Corporation).
  • VAP-7070 automatic polarizing film measuring device
  • the direction of the transmission axis of the linear polarizer preferably coincides with the direction of the polarization axis of the light converted into linearly polarized light by the retardation layer.
  • the angle between the transmission axis of the linear polarizer and the slow axis of the retardation layer is preferably about 45°.
  • the linear polarizer used in the laminated optical film of the present invention is also preferably a light-absorption anisotropic layer containing a liquid crystal compound and a dichroic substance.
  • a linear polarizer containing a liquid crystal compound and a dichroic substance is preferable because it can be thinned and is unlikely to crack or break even when stretched and molded.
  • the thickness of the light-absorption anisotropic layer is not particularly limited, but is preferably 0.1 to 8 ⁇ m, more preferably 0.3 to 5 ⁇ m, from the viewpoint of thinning.
  • a linear polarizer containing a liquid crystal compound and a dichroic substance can be produced, for example, by referring to JP-A-2020-023153, etc. From the viewpoint of improving the polarization degree of the linear polarizer, the light absorption anisotropic layer preferably has an orientation degree of the dichroic substance of 0.95 or more, more preferably 0.97 or more.
  • the liquid crystal compound contained in the composition for forming an optically absorptive anisotropic layer for forming the optically absorptive anisotropic layer is preferably a liquid crystal compound that does not exhibit dichroism in the visible range.
  • the liquid crystal compound either a low molecular weight liquid crystal compound or a polymeric liquid crystal compound can be used.
  • the term “low molecular weight liquid crystal compound” refers to a liquid crystal compound that does not have a repeating unit in its chemical structure.
  • polymeric liquid crystal compound refers to a liquid crystal compound that has a repeating unit in its chemical structure. Examples of the polymer liquid crystal compound include the thermotropic liquid crystal polymer described in JP 2011-237513 A.
  • the polymer liquid crystal compound preferably has a crosslinkable group at the end.
  • the crosslinkable group at the end of the polymer liquid crystal compound include an acryloyl group and a methacryloyl group.
  • the liquid crystal compounds may be used alone or in combination of two or more. It is also preferable to use a high molecular weight liquid crystal compound and a low molecular weight liquid crystal compound in combination.
  • the content of the liquid crystal compound is preferably 25 to 2000 parts by mass, more preferably 33 to 1000 parts by mass, and even more preferably 50 to 500 parts by mass, relative to 100 parts by mass of the content of the dichroic substance in the composition. When the content of the liquid crystal compound is within the above range, the degree of orientation of the polarizer is further improved.
  • the dichroic substance contained in the composition for forming an optically absorptive anisotropic layer for forming an optically absorptive anisotropic layer is not particularly limited, and examples thereof include visible light absorbing substances (dichroic dyes), ultraviolet absorbing substances, infrared absorbing substances, nonlinear optical substances, and carbon nanotubes, and any conventionally known dichroic substance (dichroic dye) can be used. In the present invention, two or more dichroic substances may be used in combination.
  • the linear polarizer of the present invention consists of a light-absorbing anisotropic layer containing a liquid crystal compound and a dichroic substance
  • the linear polarizer may include a support, an orientation layer, etc., but the support and the orientation layer may be temporary supports that are peeled off when producing a laminated optical film.
  • the optically absorbing anisotropic layer is transferred to another laminate, and then the temporary support is peeled off and removed, thereby making it possible to reduce the thickness of the laminated optical film, and further, it is preferable because the adverse effect of the phase difference of the temporary support on the polarization degree of transmitted light can be eliminated.
  • the type of the support is not particularly limited, but is preferably transparent to visible light, and for example, the same support as the support used as the retardation layer can be used.
  • a preferred embodiment of the support used in the linear polarizer is the same as the preferred embodiment of the support used as the retardation layer.
  • the linear polarizer used in the laminated optical film of the present invention is preferably transparent to near-infrared light.
  • the laminated optical film of the present invention may have other functional layers in addition to the reflective circular polarizer, the retardation layer, and the linear polarizer.
  • the other functional layers are transparent to near-infrared light.
  • the laminated optical film of the present invention further has a positive C plate as shown in Fig. 5.
  • the positive C plate is a retardation layer having Re substantially zero and Rth having a negative value.
  • the positive C plate can be obtained, for example, by vertically aligning a rod-shaped liquid crystal compound.
  • the positive C plate functions as an optical compensation layer for increasing the degree of polarization of transmitted light with respect to obliquely incident light.
  • the positive C plate may be disposed at any position in the laminated optical film, and a plurality of positive C plates may be disposed.
  • the positive C-plate may be placed adjacent to or inside the reflective circular polarizer.
  • the reflective layer has a positive Rth.
  • the polarization state of the reflected light and the transmitted light may change due to the action of Rth, and the polarization degree of the transmitted light may decrease.
  • the positive C plate is preferably provided on the side of the blue light reflecting layer opposite to the green light reflecting layer, but may be provided in other locations.
  • the Re(550) of the positive C plate is preferably about 10 nm or less, and the Rth(550) is preferably ⁇ 600 to ⁇ 100 nm, and more preferably ⁇ 400 to ⁇ 200 nm.
  • the positive C plate may be disposed adjacent to the retardation layer or inside the retardation layer.
  • the retardation layer has a positive Rth.
  • the polarization state of the transmitted light may change due to the action of Rth, and the degree of polarization of the transmitted light may decrease.
  • the positive C plate is disposed on the opposite side of the retardation layer to the linear polarizer, but it may be disposed in another place.
  • the Re(550) of the positive C plate is preferably about 10 nm or less, and the Rth(550) is preferably -90 to -40 nm.
  • the laminated optical film of the present invention has an anti-reflection layer on the surface.
  • the laminated optical film of the present invention has a function of reflecting a specific circularly polarized light and transmitting a circularly polarized light perpendicular thereto, but the reflection on the surface of the laminated optical film generally includes the reflection of unintended polarized light, which may reduce the polarization degree of the transmitted light. Therefore, it is preferable that the laminated optical film has an anti-reflection layer on the surface.
  • the anti-reflection layer may be installed only on one surface of the laminated optical film, or on both surfaces.
  • the type of the anti-reflection layer is not particularly limited, but from the viewpoint of further reducing the reflectance, a moth-eye film and an AR (anti-reflective) film are preferred.
  • a moth-eye film and the AR film known ones can be used.
  • the laminated optical film is stretched or molded, a moth-eye film is preferred because it can maintain high antireflection performance even if the film thickness varies due to stretching.
  • the antireflection layer includes a support and is stretched and molded, the peak temperature of the glass transition temperature Tg of the support is preferably 170° C. or less, more preferably 130° C. or less, from the viewpoint of facilitating stretching and molding.
  • the support is preferably, for example, a PMMA film or the like.
  • the laminated optical film of the present invention further includes a second retardation layer.
  • the laminated optical film may include a reflective circular polarizer, a retardation layer, a linear polarizer, and a second retardation layer in this order.
  • the second retardation layer is preferably one that converts linearly polarized light into circularly polarized light, and is preferably a retardation layer having an Re of, for example, a quarter wavelength, for the reasons described below.
  • the light that is incident on the laminated optical film from the reflective circular polarizer side and transmitted through the reflective circular polarizer, the retardation layer, and the linear polarizer is linearly polarized, and a part of it is reflected at the outermost surface on the linear polarizer side and is again emitted from the surface on the reflective circular polarizer side.
  • Such light is unnecessary reflected light and can be a factor in reducing the polarization degree of the reflected light, so it is preferable to reduce it.
  • the second retardation layer has substantially reverse dispersion.
  • the laminated optical film of the present invention may further have a support (resin substrate).
  • the support can be installed at any location, and for example, when the reflective circular polarizer, the retardation layer, or the linear polarizer is a film to be transferred from a temporary support, the support can be used as the transfer destination.
  • the type of the support is not particularly limited, but is preferably transparent to visible light, and for example, films such as cellulose acylate, polycarbonate, polysulfone, polyethersulfone, polyacrylate, polymethacrylate, cyclic polyolefin, polyolefin, polyamide, polystyrene, and polyester can be used.
  • the support preferably has a small retardation from the viewpoint of suppressing adverse effects on the polarization degree of transmitted light and from the viewpoint of facilitating optical inspection of the laminated optical film.
  • the magnitude of Re(550) is preferably 10 nm or less, and the absolute value of the magnitude of Rth(550) is preferably 50 nm or less.
  • the support preferably has a peak temperature of loss tangent tan ⁇ of 170°C or less.
  • the peak temperature of loss tangent tan ⁇ is preferably 150°C or less, and more preferably 130°C or less.
  • a variety of resin substrates can be used as the support having a peak temperature of loss tangent tan ⁇ of 170°C or less, without any particular restrictions.
  • Examples include polyolefins such as polyethylene, polypropylene, and norbornene-based polymers; cyclic olefin-based resins; polyvinyl alcohol; polyethylene terephthalate; acrylic resins such as polymethacrylic acid esters and polyacrylic acid esters; polyethylene naphthalate; polycarbonate; polysulfone; polyethersulfone; polyetherketone; polyphenylene sulfide and polyphenylene oxide.
  • cyclic olefin-based resins polyethylene terephthalate, and acrylic resins are preferred, as they are easily available on the market and have excellent transparency, and cyclic olefin-based resins and polymethacrylic acid esters are particularly preferred.
  • resin substrates include Technoloy S001G, Technoloy S014G, Technoloy S000, Technoloy C001 and Technoloy C000 (Sumika Acrylic Sales Co., Ltd.), Lumirror U Type, Lumirror FX10 and Lumirror SF20 (Toray Industries, Inc.), HK-53A (Higashiyama Films Co., Ltd.), Teflex FT3 (Teijin DuPont Films Co., Ltd.), S-Cina and SCA40 (Sekisui Chemical Co., Ltd.), Zeonor Film (Optes Co., Ltd.), and Arton Film (JSR Corporation).
  • the thickness of the support is not particularly limited, but is preferably 5 to 300 ⁇ m, more preferably 5 to 100 ⁇ m, and even more preferably 5 to 30 ⁇ m.
  • the laminated optical film may have layers other than the above-mentioned layers, for example, a pressure-sensitive adhesive layer formed by a pressure-sensitive adhesive described later, an adhesive layer formed by an adhesive described later, and a refractive index adjusting layer.
  • a refractive index adjustment layer having a smaller difference in refractive index between the fast axis direction and the slow axis direction than the reflective circular polarizer may be provided between the reflective circular polarizer and the adhesive, or between the reflective circular polarizer and the adhesive.
  • the refractive index adjustment layer preferably has a layer formed by fixing the orientation state of cholesteric liquid crystal.
  • the interface reflection can be further suppressed, and the occurrence of ghosts can be further suppressed.
  • the average refractive index of the refractive index adjustment layer is more preferably smaller than the average refractive index of the reflective circular polarizer.
  • the central wavelength of the reflected light of the refractive index adjustment layer may be smaller than 430 nm or larger than 670 nm, and is more preferably smaller than 430 nm.
  • the laminated optical film of the present invention is a laminate consisting of a number of layers.
  • Each layer can be bonded (attached) by any bonding method, for example, a pressure sensitive adhesive or a bonding agent.
  • the adhesive any commercially available adhesive can be used, but from the viewpoint of thinning and reducing the surface roughness Ra of the laminated optical film, the thickness is preferably 25 ⁇ m or less, more preferably 15 ⁇ m or less, and even more preferably 6 ⁇ m or less. In addition, it is preferable that the adhesive is one that is unlikely to generate outgassing.
  • the adhesive when performing stretching and molding, a vacuum process and a heating process may be performed, and it is preferable that outgassing is not generated even under these conditions.
  • any commercially available adhesive can be used, for example, an epoxy resin adhesive, an acrylic resin adhesive, or the like. From the viewpoint of thinning and reducing the surface roughness Ra of the laminated optical film, the adhesive has a thickness of preferably 25 ⁇ m or less, more preferably 5 ⁇ m or less, and even more preferably 1 ⁇ m or less.
  • the adhesive has a viscosity of preferably 300 cP or less, more preferably 100 cP or less, and even more preferably 10 cP or less.
  • the pressure-sensitive adhesive and the adhesive can be selected with appropriate viscoelasticity or thickness so as to bury the surface irregularities of the layer to be adhered, from the viewpoint of reducing the surface roughness Ra of the laminated optical film. From the viewpoint of burying the surface irregularities, the pressure-sensitive adhesive and the adhesive preferably have a viscosity of 50 cP or more.
  • the thickness is preferably thicker than the height of the surface irregularities.
  • a method for adjusting the viscosity of the adhesive for example, a method of using an adhesive containing a solvent can be mentioned.
  • the viscosity of the adhesive can be adjusted by the ratio of the solvent.
  • the thickness of the adhesive can be further reduced by drying the solvent after applying the adhesive to the adherend.
  • the adhesive or adhesive used for bonding each layer has a small refractive index difference with the adjacent layer.
  • the refractive index difference between the adjacent layers is preferably 0.1 or less, more preferably 0.05 or less, and even more preferably 0.01 or less.
  • the refractive index of the adhesive or adhesive can be adjusted, for example, by mixing titanium oxide fine particles and zirconia fine particles.
  • the reflective circular polarizer, the retardation layer, and the linear polarizer may have anisotropy of the refractive index in the plane, but it is preferable that the difference in the refractive index between the adjacent layers is 0.05 or less in all directions in the plane. Therefore, the pressure-sensitive adhesive and the adhesive may have anisotropy of the refractive index in the plane.
  • the adhesive layer between each layer has a thickness of 100 nm or less.
  • the thickness of the adhesive layer is more preferably 50 nm or less.
  • a method for forming an adhesive layer having a thickness of 100 nm or less for example, a method of depositing a ceramic adhesive such as silicon oxide (SiOx layer) on the bonding surface can be mentioned.
  • the bonding surface of the bonding member can be subjected to a surface modification treatment such as plasma treatment, corona treatment, saponification treatment, etc.
  • an adhesive layer having a thickness of 100 nm or less can be provided by the procedure shown in (1) to (3) below.
  • (1) The layers to be laminated are attached to a temporary support made of a glass substrate.
  • a SiOx layer having a thickness of 100 nm or less is formed by deposition or the like.
  • the deposition can be performed using, for example, a deposition device (model number ULEYES) manufactured by ULVAC, Inc., using SiOx powder as a deposition source. It is also preferable to subject the surface of the formed SiOx layer to plasma treatment.
  • the temporary support is peeled off. The bonding is preferably performed at a temperature of, for example, 120°C.
  • each layer may be performed by roll-to-roll or sheet-to-sheet, with the roll-to-roll method being preferred from the viewpoints of improving productivity and reducing axial misalignment of each layer.
  • the single-wafer system is preferable in that it is suitable for small-lot, high-mix production and that a special bonding method can be selected such that the thickness of the adhesive layer described above is 100 nm or less.
  • Methods for applying the adhesive to the adherend include known methods such as roll coating, gravure printing, spin coating, wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spraying, and inkjet printing.
  • the adhesive layer can be eliminated by directly coating the layer on the adjacent layer that is already formed.
  • the alignment direction of the liquid crystal compound is continuously changed at the interface in order to reduce the difference in refractive index in all directions in the plane.
  • a retardation layer containing a liquid crystal compound can be directly coated on a linear polarizer containing a liquid crystal compound and a dichroic substance, and the liquid crystal compound of the retardation layer can be continuously aligned at the interface by the alignment control force of the liquid crystal compound of the linear polarizer.
  • the laminated optical film of the present invention is composed of a large number of layers, and the order of steps for laminating these layers is not particularly limited and can be selected arbitrarily.
  • the order of steps for laminating these layers is not particularly limited and can be selected arbitrarily.
  • wrinkles and cracks during transfer can be prevented by adjusting the stacking order so that the thickness of the film to which the functional layer is transferred is 10 ⁇ m or more.
  • the surface roughness Ra of the laminated optical film when a layer having a large surface roughness is laminated on top of another layer, the surface roughness may be further amplified, and therefore it is preferable to laminate the layers in order from the layer with the smallest surface roughness Ra.
  • the order of lamination may be selected from the viewpoint of quality evaluation in the manufacturing process of the laminated optical film.
  • the reflective circular polarizer may be laminated and the quality evaluation using a reflection optical system may be performed.
  • the order of lamination can be selected from the viewpoint of improving the production yield of the laminated optical film and reducing costs.
  • the laminated optical film of the present invention can be used as a reflective polarizer incorporated in vehicle rearview mirrors, virtual reality display devices, electronic viewfinders, and the like, as described in, for example, Patent Documents 4 and 5.
  • the laminated optical film of the present invention is very useful from the viewpoint of improving the clarity of the displayed image.
  • virtual reality display devices and electronic viewfinders having a reciprocating optical system may have optical films such as an absorptive polarizer and a circular polarizer in addition to the reflective polarizer, but the clarity of the displayed image can be further improved by using a part of the members and bonding method used in the laminated optical film of the present invention for optical films other than the above-mentioned reflective polarizer.
  • the optical laminate and the laminate optical film of the present invention may be used in a flat form or may be molded into any shape.
  • the optical laminate and the laminate optical film are collectively referred to as an optical film, and the molding method will be described.
  • the method for forming an optical film includes a step of heating the optical film, a step of pressing the optical film against a mold to deform the optical film according to the shape of the mold, and a step of cutting the optical film.
  • Methods for heating the optical film include heating by contacting with a heated solid, heating by contacting with a heated liquid, heating by contacting with a heated gas, heating by infrared radiation, and heating by microwave radiation. Heating by infrared radiation, which allows heating remotely just before molding, is preferred.
  • the wavelength of the infrared rays used for heating is preferably 1.0 to 30.0 ⁇ m, and more preferably 1.5 to 5 ⁇ m.
  • a near-infrared lamp heater having a tungsten filament sealed in a quartz tube a wavelength control heater having multiple quartz tubes and a mechanism for cooling some of the spaces between the quartz tubes with air, or the like can be used.
  • the physical properties during molding can be controlled according to purpose. The temperature distribution can be achieved by distributing the amount of infrared radiation used for heating, controlling the cooling air strength distribution, or controlling the temperature and contact time of the mold to distribute the cooling progress caused by contact with the mold.
  • the infrared radiation distribution can be achieved by varying the density of the IR light source arrangement, or by disposing a filter with a patterned transmittance for infrared light between the IR light source and the optical film.
  • filters with a patterned transmittance include glass with metal vapor deposition, a cholesteric liquid crystal layer with an infrared reflection band, a dielectric multilayer film with an infrared reflection band, and ink that absorbs infrared rays.
  • the temperature of the optical film is controlled by the intensity of infrared radiation, the infrared radiation time, and the illuminance of infrared radiation.
  • the temperature of the optical film can be monitored using a temperature measuring means such as a non-contact radiation thermometer and a thermocouple, and molding can be performed at a target temperature.
  • Step of pressing the optical film against the mold and deforming it to fit the shape of the mold The optical film is pressed against the mold and deformed to conform to the shape of the mold by reducing or increasing the pressure in the molding space. It is also possible to use a mold pressing method.
  • the molded optical film can be cut into any desired shape using a cutter, scissors, a cutting plotter, a laser cutter, or the like.
  • One form of molding apparatus is an apparatus that consists of box 1 having an opening at the top and box 2 having an opening at the bottom, and forms a sealed molding space by aligning the openings of box 1 and box 2 directly or via other tools to form the molding space.
  • a mold also called an adherend
  • the film to be formed acts as a partition to divide the forming space consisting of box 1 and box 2 into two spaces. The mold is placed on the box 1 side, below the film to be formed.
  • the vacuum forming device has a plurality of heating elements for heating the film to be formed, which are distributed in the vacuum forming device.
  • the heating elements may be placed inside the forming space, or may be placed outside the forming space to irradiate the film to be formed with heat through a transparent window.
  • the optical component of the present invention includes the optical layered body of the present invention.
  • One embodiment of the optical article of the present invention is a composite lens having a lens and the optical laminate of the present invention or the laminated optical film of the present invention.
  • a half mirror may be formed on one side of the lens.
  • a convex lens and a concave lens can be used.
  • a biconvex lens, a plano-convex lens, and a convex meniscus lens can be used.
  • As the concave lens a biconcave lens, a plano-concave lens, and a concave meniscus lens can be used.
  • a convex meniscus lens and a concave meniscus lens are preferable, and a concave meniscus lens is more preferable in that aberration can be suppressed to a small extent.
  • the lens may be made of a material that is transparent to visible light, such as glass, crystal, or plastic. Since birefringence of the lens causes unevenness and noise, it is preferable that it is small, and a material with zero birefringence is more preferable.
  • the laminated optical film of the present invention used in the optical article of the present invention may be flat or curved, but a curved surface is preferable in that image distortion and aberration are small.
  • optical article of the present invention has a prism or a substrate, and the optical laminate of the present invention or the laminated optical film of the present invention.
  • materials for forming the prism and the substrate include glass, crystal, and plastic. These materials may be transparent or opaque to visible light.
  • the birefringence of the prism and the substrate is preferably small because it can cause unevenness and noise, and materials with zero birefringence are more preferable.
  • ⁇ Reflective Layer Coating Solution R-1> The composition shown below was stirred and dissolved in a container kept at 70° C. to prepare a coating solution R-1 for a reflective layer, where R represents a coating solution using a rod-like liquid crystal compound.
  • the numerical values are mass %. Furthermore, R is a group bonded via an oxygen atom. Furthermore, the average molar absorption coefficient of the above rod-shaped liquid crystal compound at wavelengths of 300 to 400 nm was 140/mol cm.
  • Chiral agent A is a chiral agent whose helical twisting power (HTP) is reduced by light.
  • ⁇ Reflective layer coating solution R-2> The coating solution was prepared in the same manner as in the coating solution R-1 for the reflective layer, except that the amount of chiral agent A added was changed as shown in Table 1 below.
  • ⁇ Reflective Layer Coating Solution D-1> The composition shown below was stirred and dissolved in a container kept at 50° C. to prepare a coating solution D-1 for a reflective layer, where D represents a coating solution using a discotic liquid crystal compound.
  • ⁇ Coating solution for optical interference layer PA-1> The composition shown below was stirred and dissolved in a container kept at 60° C. to prepare a coating solution for optical interference layer PA-1.
  • the coating solution for optical interference layer PA-1 prepared above was applied to the tack film described above using a wire bar coater, and then dried at 80° C. for 60 seconds. Thereafter, in a low-oxygen atmosphere (100 ppm), the liquid crystal compound was cured by irradiating it with light from an ultraviolet LED lamp (wavelength 365 nm) at 78° C. with an irradiation dose of 300 mJ/cm 2 , and at the same time, the cleavable group of the interlayer photo-alignment film material was cleaved. Then, the substrate was heated at 115° C. for 25 seconds to eliminate the substituent containing a fluorine atom.
  • a positive C plate layer having a cinnamoyl group on the outermost surface and a thickness of 90 nm was formed.
  • the refractive index nI at a wavelength of 550 nm measured with an interference thickness meter OPTM was 1.57.
  • Rth(550) at a wavelength of 550 nm measured with an Axoscan was ⁇ 9 nm.
  • polarized UV (wavelength 313 nm) was irradiated from the positive C plate side at an illuminance of 7 mW/cm 2 and an exposure dose of 7.9 mJ/cm 2.
  • the polarized UV with a wavelength of 313 nm was obtained by transmitting ultraviolet light emitted from a mercury lamp through a bandpass filter having a transmission band at a wavelength of 313 nm and a wire grid polarizer.
  • the above-prepared reflective layer coating solution R-1 was applied with a wire bar coater, and then dried for 72 seconds at 110° C.
  • the coating was cured by irradiating light from a metal halide lamp at an illuminance of 80 mW/cm 2 and an exposure dose of 500 mJ/cm 2 at 100° C. in a low-oxygen atmosphere (100 ppm or less) to form a first blue light reflective layer (first light reflective layer) made of a cholesteric liquid crystal layer.
  • the light irradiation was performed from the cholesteric liquid crystal layer side in all cases.
  • the coating thickness was adjusted so that the film thickness of the first blue light reflective layer after curing was 2.6 ⁇ m.
  • the first blue light reflecting layer surface was subjected to a corona treatment at a discharge amount of 150 W ⁇ min/m 2 , and then the reflecting layer coating liquid D-1 was applied onto the corona-treated surface with a wire bar coater.
  • the coating film was then dried at 70°C for 2 minutes, and the solvent was evaporated, followed by heating and aging at 115°C for 3 minutes to obtain a uniform alignment state.
  • the coating film was then held at 45°C, and irradiated with ultraviolet light (300 mJ/ cm2 ) using a metal halide lamp under a nitrogen atmosphere to harden the film, forming a second blue light reflective layer (second light reflective layer) on the first blue light reflective layer.
  • the light irradiation was performed from the cholesteric liquid crystal layer side in both cases. At this time, the coating thickness was adjusted so that the film thickness of the second blue light reflective layer after hardening was 2.0 ⁇ m.
  • the second blue light reflective layer was coated with the reflective layer coating solution D-2 using a wire bar coater.
  • the coating film was then dried at 70° C. for 2 minutes, and the solvent was evaporated, followed by heating and aging at 115° C. for 3 minutes to obtain a uniform alignment state.
  • the coating film was then held at 45°C and irradiated with ultraviolet light (300 mJ/ cm2 ) using a metal halide lamp in a nitrogen atmosphere to harden it, forming a green light reflective layer (third light reflective layer) on the second blue light reflective layer.
  • the light was irradiated from the cholesteric liquid crystal layer side in all cases.
  • the coating thickness was adjusted so that the hardened green light reflective layer had a film thickness of 2.7 ⁇ m.
  • the reflective layer coating solution R-2 was applied onto the green light reflective layer using a wire bar coater, and then dried at 110° C. for 72 seconds. Thereafter, the red light reflecting layer (fourth light reflecting layer) was formed on the green light reflecting layer by irradiating light from a metal halide lamp at 100° C. with an illuminance of 80 mW and an exposure dose of 500 mJ/cm 2 in a low-oxygen atmosphere (100 ppm or less). The light was irradiated from the cholesteric liquid crystal layer side in all cases. At this time, the coating thickness was adjusted so that the red light reflecting layer after curing had a film thickness of 3.4 ⁇ m.
  • the red light reflective layer surface was subjected to a corona treatment at a discharge amount of 150 W min/ m2 , and then the reflective layer coating solution D-3 was applied onto the corona-treated surface with a wire bar coater.
  • the coating film was then dried at 70°C for 2 minutes, and after the solvent was evaporated, it was heat-aged at 115°C for 3 minutes to obtain a uniform alignment state.
  • the coating film was then held at 45°C and irradiated with ultraviolet light (300 mJ/ cm2 ) using a metal halide lamp in a nitrogen atmosphere to harden the film, forming a yellow light reflective layer (fifth light reflective layer) on the red light reflective layer.
  • the light was irradiated from the cholesteric liquid crystal layer side in all cases.
  • the coating thickness was adjusted so that the yellow light reflective layer after hardening had a thickness of 3.4 ⁇ m.
  • Table 3 shows the central reflection wavelength and film thickness for each reflective layer of the reflective circular polarizer 1 produced.
  • the central reflection wavelength is used to define the characteristics of a light reflective film with a reflection band using cholesteric liquid crystal, and refers to the midpoint of the spectral band reflected by the film. Specifically, it was obtained by calculating the average value of the short wavelength side and the long wavelength side wavelengths that show half the peak reflectance.
  • the central reflection wavelength central wavelength of reflected light
  • the film thickness was confirmed using an SEM.
  • Reflective circular polarizers 2 to 5 and 7 to 15 were produced in the same manner as reflective circular polarizer 1, except that the film thickness of the optical interference layer was changed as shown in Table 4 below.
  • a reflective circular polarizer 6 was produced without a light interference layer by forming a reflective layer on a rubbed PET film under the same conditions as those for the reflective circular polarizer 1.
  • the reflective circular polarizer 16 was produced in the same manner as the reflective circular polarizer 1, except that a photo-alignment layer was formed as the optical interference layer by the following process.
  • the coating solution PA2 for forming an alignment layer was continuously applied onto a 60 ⁇ m-thick tack (triacetyl cellulose) film (TG60, manufactured by Fujifilm Corporation) using a wire bar.
  • the support on which the coating film was formed was dried for 120 seconds with hot air at 140° C., and then the coating film was irradiated with polarized ultraviolet light (10 mJ/cm 2 , using an ultra-high pressure mercury lamp) to form a photoalignment layer.
  • the film thickness was 80 nm.
  • Reflective layer coating solution R-4 A coating solution for a reflective layer R-4 was prepared in the same manner as the coating solution for a reflective layer R-3, except that the amount of the chiral agent A added was changed as shown in Table 4 below.
  • Reflective layer coating solution D-4 The composition shown below was stirred and dissolved to prepare a coating solution D-4 for a reflective layer, where D represents a coating solution using a discotic liquid crystal compound.
  • a retardation layer 1 having reverse dispersion properties was prepared with reference to the method described in paragraphs 0151 to 0163 of JP-A-2020-084070.
  • a positive C plate 2 was prepared by adjusting the film thickness with reference to the method described in paragraphs 0132 to 0134 of JP 2016-053709 A. However, the support was changed from a polyethylene terephthalate film (PET film) to a triacetyl cellulose film (TAC film).
  • PET film polyethylene terephthalate film
  • TAC film triacetyl cellulose film
  • cellulose acylate dope To 90 parts by weight of the above-mentioned cellulose acylate dope for the core layer, 10 parts by weight of the following matting agent solution was added to prepare a cellulose acetate solution for use as the cellulose acylate dope for the outer layer.
  • the film was further dried by conveying it between rolls of a heat treatment device to prepare an optical film having a thickness of 40 ⁇ m, which was used as cellulose acylate film 1.
  • the in-plane retardation of the obtained cellulose acylate film 1 was 0 nm.
  • the coating solution for forming an alignment layer S-PA-1 described later was continuously applied onto the cellulose acylate film 1 using a wire bar.
  • the support on which the coating film was formed was dried with hot air at 140° C. for 120 seconds, and then the coating film was irradiated with polarized ultraviolet light (10 mJ/cm 2 , using an ultra-high pressure mercury lamp) to form a photoalignment layer PA1.
  • the film thickness was 0.3 ⁇ m.
  • the following coating solution SP-1 for forming an optically absorptive anisotropic layer was continuously coated with a wire bar.
  • the coating layer P1 was heated at 140° C. for 30 seconds, and then cooled to room temperature (23° C.), followed by heating at 90° C. for 60 seconds, and then cooling again to room temperature.
  • an LED lamp center wavelength 365 nm was used to irradiate the film with an illuminance of 200 mW/cm 2 for 2 seconds to form an optically absorptive anisotropic layer P1 on the alignment layer PA1.
  • the film thickness was 1.6 ⁇ m.
  • ⁇ Transfer for producing laminated optical film> The transfer for producing the laminated optical film was carried out according to the following procedure.
  • a PMMA substrate was coated with a UV adhesive Chemiseal U2084B (manufactured by Chemitech Corporation, refractive index after curing n 1.60) to a thickness of 2 ⁇ m using a wire bar coater.
  • An optically absorptive anisotropic layer P1 was transferred onto the UV adhesive.
  • the optically absorptive anisotropic layer P1 was laminated with a laminator so that the side opposite to the temporary support of the optically absorptive anisotropic layer P1 was in contact with the UV adhesive.
  • the light absorption anisotropic layer P1 was cured by irradiating it with ultraviolet light from a high pressure mercury lamp from the temporary support side.
  • the illuminance was 25 mW/cm 2 and the dose was 1000 mJ/cm 2 .
  • the temporary support of the optically absorptive anisotropic layer P1 was peeled off.
  • the retardation layer 1 was transferred to the optically absorptive anisotropic layer P1 by the same transfer procedure as described above. However, the retardation layer 1 and the optically absorptive anisotropic layer P1 were laminated so that the slow axis of the retardation layer 1 and the absorption axis of the optically absorptive anisotropic layer P1 were at an angle of 45°.
  • the positive C plate 2 was transferred to the retardation layer 1 by the same transfer procedure as described above.
  • the reflective circular polarizer 1 was transferred to the positive C plate 2 by the same transfer procedure as described above. In this manner, a laminated optical film using the reflective circular polarizer 1 of Example 1 was obtained.
  • laminated optical films 2 to 16 were produced using the same procedure. Also, for the reflective circular polarizer 17, laminated optical film 23 was produced using the same procedure.
  • a hard coat layer having a refractive index of 1.57 and a thickness of 90 nm was formed by coating on the surface of the laminated optical film 6 facing the reflective circular polarizer 6 to form an optical interference layer.
  • the hard coat layer had an Rth(550) of 0 nm.
  • the composition of the hard coat layer coating solution and the coating process are shown below.
  • the hard coat layer coating solution HC-1 prepared above was applied to the surface of the laminated optical film 6 on the side of the reflective circular polarizer 6 using a wire bar coater, and then dried at 80° C. for 60 seconds. Thereafter, the polymerizable compound was cured by irradiating it with light from an ultraviolet LED lamp (wavelength 365 nm) at a dose of 300 mJ/cm 2 at 78° C. in a low-oxygen atmosphere (100 ppm). As a result, a laminated optical film 17 was produced, having, on the outermost surface, a light interference layer made of a hard coat material and having a thickness of 90 nm.
  • An optical interference layer was formed by the same preparation procedure as for the laminated optical film 17.
  • the refractive index of the hard coat layer was changed by changing the ratio of the polymerizable compound 1 and the polymerizable compound 2 in the coating liquid HC-1 for the hard coat layer.
  • a hard coat layer having a refractive index of 1.55 and a thickness of 90 nm was applied to the surface of the laminated optical film 6 on the side of the reflective circular polarizer 6 to obtain a laminated optical film 18.
  • a hard coat layer having a refractive index of 1.53 and a thickness of 90 nm was formed by a coating method to obtain a laminated optical film 19.
  • a hard coat layer having a refractive index of 1.51 and a thickness of 90 nm was formed by a coating method to obtain a laminated optical film 20.
  • a hard coat layer having a refractive index of 1.56 and a thickness of 90 nm was formed by a coating method to obtain a laminated optical film 21.
  • a hard coat layer having a refractive index of 1.54 and a thickness of 90 nm was formed by a coating method to obtain a laminated optical film 22. All of the hard coat layers had an Rth(550) of 0 nm.
  • the produced laminated optical film was molded into a curved shape.
  • the laminated optical film 1 was set in a molding device.
  • the molding space in the molding device was composed of box 1 and box 2 partitioned by laminated optical film 1, and a convex meniscus lens LE1076-A (diameter 2 inches, focal length 100 mm, radius of curvature on the concave side 65 mm) manufactured by Thorlab Corp. with aluminum vapor deposition applied to the convex side as a mold was placed with the concave side facing up in box 1 below the laminated optical film 1.
  • the reflective circular polarizer side of the laminated optical film 1 was placed on the mold side.
  • a transparent window was provided at the top of the box 2 above the laminated optical film 1 , and an IR light source for heating the laminated optical film 1 was provided outside the window.
  • a patterned infrared reflection filter made of a cholesteric liquid crystal layer that reflects infrared rays with wavelengths of 2.2 ⁇ m to 3.0 ⁇ m at a reflectance of approximately 50% was placed between the IR light source and the laminated optical film 1.
  • the pattern of the patterned infrared reflection filter was doughnut-shaped, and the center of a circular infrared reflection filter with a diameter of 2 inches was hollowed out to a diameter of 1 inch. In this case, the center of the patterned infrared reflection filter was placed at the center of the mold when viewed from directly above.
  • the inside of box 1 and the inside of box 2 were evacuated to a vacuum of 0.1 atmosphere or less using a vacuum pump.
  • a step of heating the laminated optical film 1 infrared rays were irradiated and the laminated optical film 1 was heated until the center reached 108° C. and the ends reached 99° C. Since the glass transition temperature Tg of the PMMA film used as the support was 105° C., the aim was to make the center easily stretchable and the ends less stretchable during molding.
  • Laminated optical films 2 to 22 and 24 were also molded into curved surfaces using the same procedure.
  • the laminated optical film 1 and the complex lens 1 were attached to each other using an adhesive (SK2057, manufactured by Soken Chemical & Engineering Co., Ltd.) so that the optical interference layer faced the complex lens 1.
  • This adhesive became the adhesive layer in the optical laminate of the present invention.
  • the refractive index nA at a wavelength of 550 nm of the adhesive layer used when mounting the laminated optical film 1 (Example 1) on the lens was 1.49
  • the average refractive index nL at a wavelength of 550 nm of the light reflective layer (corresponding to reflective layer A (reflective layer A21a)) was 1.63.
  • the square root of the product of these values ((nA ⁇ nL) 1/2 ) was 1.56, and the refractive index difference with the refractive index nI (1.57) of the optical interference layer at a wavelength of 550 nm was 0.01.
  • the laminated optical films 2 to 20 and 24 were also attached to the composite lens 1 and incorporated into the main body of the virtual reality display device to fabricate the virtual reality display devices of Examples 2 to 13 and 16 and Comparative Examples 1 to 7.
  • the adhesive was changed to a pressure sensitive adhesive (NCF-D692) manufactured by Lintec Corporation, they were similarly bonded to the composite lens 1 and incorporated into the main body of the virtual reality display device to produce the virtual reality display devices of Examples 14 and 15.
  • the optical interference layer had a refractive index nI of 1.57 at a wavelength of 550 nm, and the refractive index difference was 0.01.
  • the refractive index nI of the optical interference layer of Example 10 (reflective polarizer 16) at a wavelength of 550 nm was 1.56, and the refractive index difference was 0.00.
  • the optical interference layer of Example 12 had a refractive index nI of 1.55 at a wavelength of 550 nm, and the refractive index difference was 0.01.
  • the optical interference layer of Example 13 had a refractive index nI of 1.53 at a wavelength of 550 nm, and the refractive index difference was 0.03.
  • the optical interference layer of Comparative Example 7 had a refractive index nI of 1.51 at a wavelength of 550 nm, and the refractive index difference was 0.05.
  • the refractive index nA of the adhesive layer used when mounting the laminated optical film 21 (Example 14) on the lens was 1.46 at a wavelength of 550 nm, and the average refractive index nL of the light reflecting layer (corresponding to the reflective layer A (reflective layer A21a)) at a wavelength of 550 nm was 1.63.
  • the square root of the product of these values ((nA x nL) 1/2 ) was 1.54, and the refractive index difference with the refractive index nI (1.56) of the optical interference layer at a wavelength of 550 nm was 0.02.
  • the refractive index nI of the optical interference layer at a wavelength of 550 nm of Example 15 was 1.54, and the refractive index difference was 0.00.
  • the adhesive layer used when mounting the laminated optical film 24 (Example 16) on the lens had a refractive index nA of 1.49 at a wavelength of 550 nm, and the light reflecting layer (corresponding to the reflecting layer A (reflecting layer A21a)) had an average refractive index nL of 1.66 ( ⁇ n was 0.225) at a wavelength of 550 nm.
  • the refractive index of the adhesive layer was measured by an interference film thickness meter OPTM (manufactured by Otsuka Electronics, analyzed by the least squares method), and the average refractive index of the light reflecting layer was measured by the following method.
  • OPTM interference film thickness meter
  • the light reflecting layer adjacent to the adhesive layer was peeled off and obtained, and the cross section of the light reflecting layer was observed with an SEM to obtain the helical pitch P.
  • the helical pitch P is two periods of the light and dark stripes that appear in the SEM image.
  • the reflection spectrum (manufactured by JASCO Corporation, ultraviolet-visible-near infrared spectrophotometer V-750) was measured to obtain the short wavelength side half-value wavelength ⁇ l and the long wavelength side half-value wavelength ⁇ h of the reflection band of the light reflecting layer.

Landscapes

  • Physics & Mathematics (AREA)
  • General Physics & Mathematics (AREA)
  • Optics & Photonics (AREA)
  • Chemical & Material Sciences (AREA)
  • Crystallography & Structural Chemistry (AREA)
  • Engineering & Computer Science (AREA)
  • Theoretical Computer Science (AREA)
  • Polarising Elements (AREA)
PCT/JP2023/044019 2022-12-13 2023-12-08 光学用積層体、積層光学フィルム、光学物品および仮想現実表示装置 Ceased WO2024128155A1 (ja)

Priority Applications (3)

Application Number Priority Date Filing Date Title
CN202380085543.5A CN120344886A (zh) 2022-12-13 2023-12-08 光学用层叠体、层叠光学膜、光学物品及虚拟现实显示装置
JP2024564350A JPWO2024128155A1 (cg-RX-API-DMAC7.html) 2022-12-13 2023-12-08
US19/228,771 US20250298238A1 (en) 2022-12-13 2025-06-05 Optical laminate, laminated optical film, optical article, and virtual reality display device

Applications Claiming Priority (4)

Application Number Priority Date Filing Date Title
JP2022-198779 2022-12-13
JP2022198779 2022-12-13
JP2023186933 2023-10-31
JP2023-186933 2023-10-31

Related Child Applications (1)

Application Number Title Priority Date Filing Date
US19/228,771 Continuation US20250298238A1 (en) 2022-12-13 2025-06-05 Optical laminate, laminated optical film, optical article, and virtual reality display device

Publications (1)

Publication Number Publication Date
WO2024128155A1 true WO2024128155A1 (ja) 2024-06-20

Family

ID=91484951

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2023/044019 Ceased WO2024128155A1 (ja) 2022-12-13 2023-12-08 光学用積層体、積層光学フィルム、光学物品および仮想現実表示装置

Country Status (4)

Country Link
US (1) US20250298238A1 (cg-RX-API-DMAC7.html)
JP (1) JPWO2024128155A1 (cg-RX-API-DMAC7.html)
CN (1) CN120344886A (cg-RX-API-DMAC7.html)
WO (1) WO2024128155A1 (cg-RX-API-DMAC7.html)

Citations (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2008023719A (ja) * 2006-07-18 2008-02-07 Mitsubishi Polyester Film Copp 反射防止フィルム用積層ポリエステルフィルム
WO2021065532A1 (ja) * 2019-09-30 2021-04-08 富士フイルム株式会社 発光装置
WO2022075475A1 (ja) * 2020-10-09 2022-04-14 富士フイルム株式会社 積層光学フィルムおよび画像表示装置

Patent Citations (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2008023719A (ja) * 2006-07-18 2008-02-07 Mitsubishi Polyester Film Copp 反射防止フィルム用積層ポリエステルフィルム
WO2021065532A1 (ja) * 2019-09-30 2021-04-08 富士フイルム株式会社 発光装置
WO2022075475A1 (ja) * 2020-10-09 2022-04-14 富士フイルム株式会社 積層光学フィルムおよび画像表示装置

Also Published As

Publication number Publication date
CN120344886A (zh) 2025-07-18
JPWO2024128155A1 (cg-RX-API-DMAC7.html) 2024-06-20
US20250298238A1 (en) 2025-09-25

Similar Documents

Publication Publication Date Title
US20230314679A1 (en) Laminated optical film and image display device
CN100380197C (zh) 视场角扩大的液晶显示装置
JP6321052B2 (ja) 輝度向上フィルム、光学シート部材および液晶表示装置
JP6859109B2 (ja) 光学補償層付偏光板およびそれを用いた有機elパネル
TW202346953A (zh) 光學積層體、光學透鏡、虛擬實境顯示裝置、光學各向異性膜、成形體、反射型圓偏振器、非平面反射型圓偏振器、積層光學體、複合透鏡
US12345907B2 (en) Optical laminate, laminated optical film, optical article, and virtual reality display device
WO2023199950A1 (ja) 成形方法、光学フィルム、コレステリック液晶層、光学積層体、および、曲面状光学機能性層の作製方法
WO2022270502A1 (ja) 光学積層体、光学積層体の製造方法、光学積層体の裁断方法
TW202406714A (zh) 光學功能性膜、光學積層體、成形體、光學組件的製造方法、光學組件、虛擬實境顯示裝置、光學膜及其成形方法
US20260126575A1 (en) Lens, image display device, and virtual reality display apparatus
US20250085466A1 (en) Optical laminate, laminated optical film, optical article, and virtual reality display device
CN121969965A (zh) 膜、光学部件、光学装置、头戴式显示器
US20250298238A1 (en) Optical laminate, laminated optical film, optical article, and virtual reality display device
WO2025094817A1 (ja) 光学積層体、積層光学フィルムおよび光学物品
WO2024154594A1 (ja) 位相差フィルム、積層光学フィルム、光学物品、仮想現実表示装置
KR100882411B1 (ko) 편광판의 제조 방법 및 액정 표시 장치
WO2025063263A1 (ja) 赤外光反射素子、積層光学フィルムおよび光学物品
WO2025063244A1 (ja) 赤外光反射素子、積層光学フィルムおよび光学物品
US20260003113A1 (en) Optical laminate, optical lens, and virtual reality display apparatus
WO2025258461A1 (ja) 反射円偏光子、積層光学フィルム、および、仮想現実表示装置
CN117460976A (zh) 光学用层叠体、层叠光学膜、光学物品、虚拟现实显示装置
KR100847650B1 (ko) 편광판의 제조 방법 및 액정 표시 장치
WO2025004991A1 (ja) 光学フィルム、レンズ、および仮想現実表示装置
WO2024195606A1 (ja) 光吸収異方性膜、積層体、複合レンズ、仮想現実表示装置
WO2026023452A1 (ja) 光吸収異方性膜、積層体、複合レンズ、ゴーグル型表示装置および光吸収異方性膜の製造方法

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 23903442

Country of ref document: EP

Kind code of ref document: A1

WWE Wipo information: entry into national phase

Ref document number: 2024564350

Country of ref document: JP

WWE Wipo information: entry into national phase

Ref document number: 202380085543.5

Country of ref document: CN

NENP Non-entry into the national phase

Ref country code: DE

WWP Wipo information: published in national office

Ref document number: 202380085543.5

Country of ref document: CN

122 Ep: pct application non-entry in european phase

Ref document number: 23903442

Country of ref document: EP

Kind code of ref document: A1