WO2023199576A1 - ガラス繊維強化樹脂成形品 - Google Patents

ガラス繊維強化樹脂成形品 Download PDF

Info

Publication number
WO2023199576A1
WO2023199576A1 PCT/JP2023/003464 JP2023003464W WO2023199576A1 WO 2023199576 A1 WO2023199576 A1 WO 2023199576A1 JP 2023003464 W JP2023003464 W JP 2023003464W WO 2023199576 A1 WO2023199576 A1 WO 2023199576A1
Authority
WO
WIPO (PCT)
Prior art keywords
glass fiber
reinforced resin
glass
resin molded
fiber reinforced
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2023/003464
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
遼 佐々木
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nitto Boseki Co Ltd
Original Assignee
Nitto Boseki Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nitto Boseki Co Ltd filed Critical Nitto Boseki Co Ltd
Priority to JP2024514812A priority Critical patent/JPWO2023199576A1/ja
Priority to GB2410568.6A priority patent/GB2629724A/en
Priority to KR1020247027855A priority patent/KR20250007494A/ko
Priority to US18/730,844 priority patent/US20250101191A1/en
Priority to CN202380032168.8A priority patent/CN118974145A/zh
Publication of WO2023199576A1 publication Critical patent/WO2023199576A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J5/00—Manufacture of articles or shaped materials containing macromolecular substances
    • C08J5/04—Reinforcing macromolecular compounds with loose or coherent fibrous material
    • C08J5/0405—Reinforcing macromolecular compounds with loose or coherent fibrous material with inorganic fibres
    • C08J5/043—Reinforcing macromolecular compounds with loose or coherent fibrous material with inorganic fibres with glass fibres
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G65/00—Macromolecular compounds obtained by reactions forming an ether link in the main chain of the macromolecule
    • C08G65/34—Macromolecular compounds obtained by reactions forming an ether link in the main chain of the macromolecule from hydroxy compounds or their metallic derivatives
    • C08G65/38—Macromolecular compounds obtained by reactions forming an ether link in the main chain of the macromolecule from hydroxy compounds or their metallic derivatives derived from phenols
    • C08G65/40—Macromolecular compounds obtained by reactions forming an ether link in the main chain of the macromolecule from hydroxy compounds or their metallic derivatives derived from phenols from phenols (I) and other compounds (II), e.g. OH-Ar-OH + X-Ar-X, where X is halogen atom, i.e. leaving group
    • C08G65/4012—Other compound (II) containing a ketone group, e.g. X-Ar-C(=O)-Ar-X for polyetherketones
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J5/00—Manufacture of articles or shaped materials containing macromolecular substances
    • C08J5/04—Reinforcing macromolecular compounds with loose or coherent fibrous material
    • C08J5/06—Reinforcing macromolecular compounds with loose or coherent fibrous material using pretreated fibrous materials
    • C08J5/08—Reinforcing macromolecular compounds with loose or coherent fibrous material using pretreated fibrous materials glass fibres
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K7/00—Use of ingredients characterised by shape
    • C08K7/02—Fibres or whiskers
    • C08K7/04—Fibres or whiskers inorganic
    • C08K7/14—Glass
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L71/00—Compositions of polyethers obtained by reactions forming an ether link in the main chain; Compositions of derivatives of such polymers
    • C08L71/08—Polyethers derived from hydroxy compounds or from their metallic derivatives
    • C08L71/10—Polyethers derived from hydroxy compounds or from their metallic derivatives from phenols
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G2650/00—Macromolecular compounds obtained by reactions forming an ether link in the main chain of the macromolecule
    • C08G2650/28—Macromolecular compounds obtained by reactions forming an ether link in the main chain of the macromolecule characterised by the polymer type
    • C08G2650/38—Macromolecular compounds obtained by reactions forming an ether link in the main chain of the macromolecule characterised by the polymer type containing oxygen in addition to the ether group
    • C08G2650/40—Macromolecular compounds obtained by reactions forming an ether link in the main chain of the macromolecule characterised by the polymer type containing oxygen in addition to the ether group containing ketone groups, e.g. polyarylethylketones, PEEK or PEK
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K2201/00—Specific properties of additives
    • C08K2201/002—Physical properties
    • C08K2201/003—Additives being defined by their diameter

Definitions

  • the present invention relates to glass fiber reinforced resin molded products.
  • glass fiber reinforced resin molded products using glass fiber as a reinforcing material have been known.
  • glass fibers having an E-glass composition are most commonly used as the glass fibers.
  • the glass fiber is also required to increase the impact strength of glass fiber reinforced resin molded products, and the present applicant has proposed that the impact strength of glass fiber reinforced resin molded products is higher than that of the E glass fiber. They have proposed glass fibers that can increase strength (see Patent Document 1).
  • the impact properties of the glass fiber-reinforced resin molded product are evaluated by the amount of impact energy absorbed at the time of breakage (hereinafter referred to as "shock absorption at time of breakage").
  • shock absorption at time of breakage the amount of impact energy absorbed at the time of breakage.
  • the glass fiber-reinforced resin molded product using glass fibers described in Patent Document 1 has a disadvantage in that, although it has a high impact absorption property at the time of breakage, it does not have sufficient impact resistance at a stage that does not lead to breakage.
  • glass fiber reinforced resin molded products with high shock absorption properties have a large amount of deformation (strain) upon impact, but glass fiber reinforced resin molded products with a large amount of deformation have low rigidity and are difficult to handle. There is this inconvenience.
  • the present invention eliminates such inconveniences and provides a glass fiber reinforced resin molded product that has both shock absorption at the time of breakage and impact resistance at a stage before breakage, as well as an excellent balance with ease of handling.
  • the purpose is to
  • the glass fiber reinforced resin molded article of the present invention has a fiber diameter D of the glass fibers contained in the glass fiber reinforced resin molded article in the range of 5.0 to 17.0 ⁇ m, and The linear expansion coefficient ⁇ of the fiber is in the range of 2.0 to 6.0 ppm/K, the tensile modulus E of the glass fiber is in the range of 58 to 92 GPa, and the glass fiber is The content C is in the range of 10.0 to 50.0% by mass, and the heat of crystallization Q of the glass fiber reinforced resin molded product is 30.0 to 60.0% with respect to the resin mass contained in the glass fiber reinforced resin molded product. 0 J/g, and is characterized in that D, ⁇ , E, C, and Q satisfy the following formula (1). 16.02 ⁇ Q ⁇ E/(D 1/3 ⁇ C 1/2 ⁇ 2 ) ⁇ 27.70 (1)
  • the glass fiber-reinforced resin molded product of the present invention has impact absorption properties at the time of breakage and impact resistance at a stage before breakage because D, ⁇ , E, C, and Q satisfy the above formula (1). It can be made to have an excellent balance with ease of use and ease of handling.
  • D, ⁇ , E, C, and Q preferably satisfy the following formula (2), more preferably satisfy the following formula (3). 18.74 ⁇ Q ⁇ E/(D 1/3 ⁇ C 1/2 ⁇ 2 ) ⁇ 21.74 (2) 20.24 ⁇ Q ⁇ E/(D 1/3 ⁇ C 1/2 ⁇ 2 ) ⁇ 21.54 (3)
  • the glass fiber-reinforced resin molded product of the present invention has impact absorption properties at the time of breakage and impact resistance at a stage before breakage because the above-mentioned D, ⁇ , E, C, and Q satisfy the above formula (2). It is possible to achieve a better balance between handling properties and handling properties.
  • the glass fiber reinforced resin molded product of the present invention has both shock absorption properties at the time of breakage and impact resistance at a stage before breakage, and has a balance with ease of handling. It can be made even better.
  • the resin is polyaryletherketone.
  • the fiber diameter D of the glass fibers contained in the glass fiber reinforced resin molded product is in the range of 5.0 to 17.0 ⁇ m, and the linear expansion coefficient ⁇ of the glass fiber is in the range of 5.0 to 17.0 ⁇ m.
  • the tensile modulus E of the glass fiber is in the range of 58 to 92 GPa, and the glass fiber content C with respect to the total amount of the glass fiber reinforced resin molded product is 10.0.
  • the heat of crystallization Q of the glass fiber reinforced resin molded product is in the range of 30.0 to 60.0 J/g based on the mass of resin contained in the glass fiber reinforced resin molded product.
  • D, ⁇ , E, C, and Q satisfy the following formula (1). 16.02 ⁇ Q ⁇ (E/ ⁇ 2 ) ⁇ /(D 1/3 ⁇ C 1/2 ) ⁇ 27.70 (1)
  • the glass fiber-reinforced resin molded product of this embodiment can be obtained, for example, by kneading glass fiber and thermoplastic resin in a twin-screw kneader and performing injection molding using the obtained molding raw material.
  • the glass fiber reinforced resin molded product of this embodiment can be produced using injection compression molding, two-color molding, blow molding, foam molding (including those using supercritical fluid), insert molding, and in-mold coating molding.
  • extrusion molding method extrusion molding method, sheet molding method, thermoforming method, rotational molding method, lamination molding method, press molding method, blow molding method, stamping molding method, infusion method, hand lay-up method, spray-up method, resin transfer molding
  • injection molding is preferred because it has excellent manufacturing efficiency.
  • the molding raw material is chopped strands, which are kneaded with the resin and then extruded from a nozzle to a predetermined length in the range of, for example, 1 to 50 mm. It is possible to use pellets processed into pellets by cutting them into lengths.
  • the chopped strand is a glass fiber formed by bundling a plurality of glass filaments and cut into lengths in the range of 1 to 25 mm. Note that the chopped strand is usually distributed as a plurality of glass fiber cut pieces cut as described above, housed in a bag-like package.
  • the roving is impregnated with a molten thermoplastic resin, cooled, and then processed into a pellet shape by cutting it into a predetermined length in the range of 1 to 50 mm, for example. It is also possible to use a
  • the roving is a glass fiber formed by bundling a plurality of glass filaments and continuously wound. Note that the roving is usually distributed in a state in which the roving has a length of 1000 m or more and is wound around a core material.
  • the thermoplastic resin is preferably polyaryletherketone.
  • the polyaryletherketone include polyetherketone (PEK), polyetheretherketone (PEEK), polyetherketoneketone (PEKK), polyetheretherketoneketone (PEEKK), etc. Particular preference is given to ether ether ketone (PEEK).
  • the glass fibers have a predetermined linear expansion coefficient and a predetermined tensile modulus.
  • the glass fiber is manufactured as follows.
  • a glass raw material (glass batch) is supplied to a melting furnace and melted at a temperature in the range of, for example, 1450 to 1600°C to obtain a glass batch (molten glass).
  • the glass batch is formulated to have the composition of a glass composition for glass fiber based on the components contained in the ore used as the glass raw material, the content of each component, and the amount of volatilization of each component during the melting process. .
  • the molten glass batch is drawn out from 1 to 20,000 nozzle tips of the bushing, which are controlled at a predetermined temperature, and rapidly cooled to form glass filaments.
  • the glass single fiber (glass filament) discharged from one nozzle tip or hole and cooled and solidified usually has a perfectly circular cross-sectional shape.
  • the nozzle tip has a non-circular shape and has a protrusion or notch that rapidly cools the molten glass
  • controlling the temperature conditions may cause the nozzle tip to have a non-circular shape (e.g. Glass filaments having a cross-sectional shape can be obtained.
  • the said cross-sectional shape is the shape of the cross section which cut
  • a sizing agent or binder is applied to the formed glass filament using an applicator, which is a coating device.
  • Glass fibers can then be obtained by focusing 1 to 20,000 glass filaments using a focusing shoe and winding them into a tube at high speed using a winder.
  • the composition of the glass composition for glass fibers forming the glass fibers is not particularly limited.
  • examples of the glass composition that the glass fiber can take include E glass composition, NE glass composition, etc., but NE glass composition is preferable.
  • the NE glass composition includes SiO 2 in a range of 48.0 to 62.0% by mass and B 2 O 3 in a range of 17.0 to 26.0% by mass, based on the total amount of glass fibers. and Al 2 O 3 in a range of 9.0 to 18.0% by mass, and may contain other components as the balance.
  • the other components include, but are not limited to, MgO, CaO, SrO, Li2O , Na2O , K2O , ZnO, F2 , Cl2 , Fe2O3 , etc. .
  • the linear expansion coefficient of the glass fiber decreases.
  • the glass composition of the glass fiber as the total content of SiO 2 and Al 2 O 3 relative to the total amount of the glass fiber decreases, the linear expansion coefficient of the glass fiber tends to increase.
  • the tensile modulus of the glass fiber decreases.
  • the tensile modulus of the glass fiber tends to increase as the content of B 2 O 3 with respect to the total amount of the glass fiber decreases.
  • the content of each component in the glass composition can be measured using an ICP emission spectrometer for Li, which is a light element. Further, the content of other elements can be measured using a wavelength dispersive X-ray fluorescence analyzer.
  • a glass batch is placed in a platinum crucible, held at a temperature of 1550° C. for 4 hours in an electric furnace, and melted with stirring to obtain homogeneous molten glass.
  • homogeneous molten glass is obtained by placing glass fibers in a platinum crucible and melting the glass fibers in an electric furnace at a temperature of 1600° C. for 4 hours while stirring.
  • the glass batch is prepared by mixing glass raw materials.
  • the glass fiber has an organic substance attached to the surface of the glass fiber, or when the glass fiber is mainly contained in the organic substance (resin) as a reinforcing material, It is heated in a muffle furnace for about 0.5 to 24 hours to remove organic substances before use.
  • the obtained molten glass is poured onto a carbon plate to produce a glass cullet, and then the glass cullet is crushed and powdered to obtain glass powder.
  • the glass powder is thermally decomposed with an acid, and then quantitatively analyzed using an ICP emission spectrometer.
  • Other elements are quantitatively analyzed using a wavelength dispersive X-ray fluorescence analyzer after the glass powder is formed into a disk shape using a press.
  • a calibration curve sample can be prepared based on the results measured by the fundamental parameter method, and the sample can be analyzed by the calibration curve method.
  • the content of each component in the calibration curve sample can be quantitatively analyzed using an ICP emission spectrometer.
  • the content and total amount of each component can be calculated by converting these quantitative analysis results into oxides, and the content (mass %) of each component described above can be determined from these values.
  • the glass fibers contained in the glass fiber reinforced resin molded product of this embodiment are used for the purpose of improving the adhesion between the glass fibers and the resin, improving the uniform dispersion of the glass fibers in the mixture of the glass fibers and the resin, etc.
  • the surface thereof may be coated with an organic substance.
  • organic substances include resins and silane coupling agents.
  • the organic substance may be a composition containing a lubricant, a surfactant, etc. in addition to a resin or a silane coupling agent.
  • the organic substance coats the glass fiber at a rate of 0.1 to 2.0% by mass, based on the mass of the glass fiber in a state not covered with the organic substance.
  • the coating of the glass fibers with the organic substance can be carried out, for example, in the manufacturing process of the glass fibers using a known method such as a roller type applicator, using the resin, the silane coupling agent, or the sizing agent containing a solution of the composition.
  • This can be carried out by applying a binder to glass fibers, and then drying the glass fibers coated with a solution of the resin, the silane coupling agent, or the composition.
  • the resins include urethane resins, epoxy resins, vinyl acetate resins, acrylic resins, modified polypropylenes, especially carboxylic acid-modified polypropylenes, copolymers of (poly)carboxylic acids, especially maleic acid, and unsaturated monomers, and the like. be able to.
  • silane coupling agent examples include aminosilane, chlorosilane, epoxysilane, mercaptosilane, vinylsilane, acrylicsilane, and cationic silane.
  • the silane coupling agents can be used alone or in combination of two or more.
  • aminosilane examples include ⁇ -aminopropyltriethoxysilane, N- ⁇ -(aminoethyl)- ⁇ -aminopropyltrimethoxysilane, N- ⁇ -(aminoethyl)-N'- ⁇ -(aminoethyl)- ⁇ - Examples include aminopropyltrimethoxysilane and ⁇ -anilinopropyltrimethoxysilane.
  • chlorosilane examples include ⁇ -chloropropyltrimethoxysilane and the like.
  • epoxysilane examples include ⁇ -glycidoxypropyltrimethoxysilane and ⁇ -(3,4-epoxycyclohexyl)ethyltrimethoxysilane.
  • Examples of mercaptosilane include ⁇ -mercaptotrimethoxysilane.
  • vinylsilane examples include vinyltrimethoxysilane, N- ⁇ -(N-vinylbenzylaminoethyl)- ⁇ -aminopropyltrimethoxysilane, and the like.
  • acrylic silane examples include ⁇ -methacryloxypropyltrimethoxysilane.
  • Examples of the cationic silane include N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane hydrochloride and N-phenyl-3-aminopropyltrimethoxysilane hydrochloride.
  • the lubricants include modified silicone oils, animal oils and hydrogenated products thereof, vegetable oils and hydrogenated products thereof, animal waxes, vegetable waxes, mineral waxes, condensates of higher saturated fatty acids and higher saturated alcohols, and polyethyleneimine. , polyalkylpolyamine alkylamide derivatives, fatty acid amides, and quaternary ammonium salts.
  • the lubricants can be used alone or in combination of two or more.
  • animal oil examples include beef tallow.
  • vegetable oils examples include soybean oil, coconut oil, rapeseed oil, palm oil, and castor oil.
  • animal waxes examples include beeswax and lanolin.
  • Examples of vegetable waxes include candelilla wax and carnauba wax.
  • mineral waxes examples include paraffin wax and montan wax.
  • condensates of higher saturated fatty acids and higher saturated alcohols include stearic acid esters such as lauryl stearate.
  • fatty acid amides include dehydrated condensates of polyethylene polyamines such as diethylenetriamine, triethylenetetramine, and tetraethylenepentamine and fatty acids such as lauric acid, myristic acid, palmitic acid, and stearic acid.
  • quaternary ammonium salt examples include alkyltrimethylammonium salts such as lauryltrimethylammonium chloride.
  • surfactant examples include nonionic surfactants, cationic surfactants, anionic surfactants, and amphoteric surfactants.
  • the surfactants can be used alone or in combination of two or more.
  • nonionic surfactants include ethylene oxide propylene oxide alkyl ether, polyoxyethylene alkyl ether, polyoxyethylene-polyoxypropylene-block copolymer, alkylpolyoxyethylene-polyoxypropylene-block copolymer ether, and polyoxyethylene fatty acid ester.
  • polyoxyethylene fatty acid monoester polyoxyethylene fatty acid diester, polyoxyethylene sorbitan fatty acid ester, glycerol fatty acid ester ethylene oxide adduct, polyoxyethylene castor oil ether, hydrogenated castor oil ethylene oxide adduct, alkylamine ethylene oxide adduct , fatty acid amide ethylene oxide adduct, glycerol fatty acid ester, polyglycerin fatty acid ester, pentaerythritol fatty acid ester, sorbitol fatty acid ester, sorbitan fatty acid ester, sucrose fatty acid ester, polyhydric alcohol alkyl ether, fatty acid alkanolamide, acetylene glycol, acetylene alcohol , an ethylene oxide adduct of acetylene glycol, an ethylene oxide adduct of acetylene alcohol, and the like.
  • cationic surfactants include alkyldimethylbenzylammonium chloride, alkyltrimethylammonium chloride, alkyldimethylethylammonium ethyl sulfate, higher alkylamine acetate, higher alkylamine hydrochloride, ethylene oxide adducts to higher alkylamines, and higher fatty acids. and polyalkylene polyamine, salts of esters of higher fatty acids and alkanolamines, salts of higher fatty acid amides, imidazoline type cationic surfactants, alkylpyridinium salts, and the like.
  • anionic surfactants include higher alcohol sulfate salts, higher alkyl ether sulfate salts, ⁇ -olefin sulfate salts, alkylbenzene sulfonates, ⁇ -olefin sulfonates, and reactions between fatty acid halides and N-methyltaurine. products, sulfosuccinic acid dialkyl ester salts, higher alcohol phosphate ester salts, higher alcohol ethylene oxide adduct phosphate ester salts, and the like.
  • amphoteric surfactant examples include amino acid type amphoteric surfactants such as alkylaminopropionic acid alkali metal salts, betaine type such as alkyl dimethyl betaine, imidazoline type amphoteric surfactants, and the like.
  • the fiber diameter D of the glass fiber is less than 5.0 ⁇ m, the glass fibers will be difficult to disperse in the resin during molding of the glass fiber reinforced resin molded product, and the glass fibers will be difficult to disperse in the resin.
  • the impact strength of reinforced resin molded products decreases.
  • the fiber diameter D of the glass fiber exceeds 17.0 ⁇ m, the total area of the interface between the glass fiber and the resin decreases, and the impact strength of the glass fiber reinforced resin molded product decreases.
  • the fiber diameter D of the glass fibers contained in the glass fiber reinforced resin molded product is preferably in the range of 5.5 to 13.0 ⁇ m, more preferably 6 ⁇ m. The range is .0 to 8.5 ⁇ m.
  • the fiber diameter D of the glass fiber means the diameter of the glass filament constituting the glass fiber, which usually has a circular cross-sectional shape.
  • the diameter of the glass filament can be measured in accordance with JIS R 3420:2013.
  • the fiber diameter D is the diameter of a circle having the same area as the cross-sectional shape. means.
  • the linear expansion coefficient ⁇ of the glass fiber is less than 2.0 ppm/K, there is a disadvantage that cracks are likely to develop upon impact. If it exceeds 6.0 ppm/K, there is a disadvantage that the strength of the glass fiber itself is low.
  • the linear expansion coefficient ⁇ of the glass fibers contained in the glass fiber reinforced resin molded product is preferably in the range of 2.8 to 4.4 ppm/K, more preferably is in the range of 3.1 to 4.0 ppm/K.
  • the linear expansion coefficient ⁇ of the glass fiber can be measured, for example, as follows.
  • the glass fiber reinforced resin molded product is heated, for example, in a muffle furnace at 300 to 650° C. for about 0.5 to 24 hours to decompose organic substances.
  • the remaining glass fibers are placed in a platinum crucible, held at a temperature of 1600° C. for 6 hours in an electric furnace, and melted with stirring to obtain homogeneous molten glass.
  • the platinum crucible containing the molten glass is taken out of the electric furnace, and the molten glass is cooled.
  • After knocking out the molten glass from the platinum crucible it was heated at a strain removal temperature (660 to 750°C) for 2 hours to remove distortion of the glass, and then cooled to room temperature (20 to 25°C) over 8 hours. Obtain glass chunks.
  • the obtained glass lump is processed into a 4 mm x 4 mm x 20 mm test piece using a cutting machine, for example, a diamond cutter and a polisher.
  • a cutting machine for example, a diamond cutter and a polisher.
  • the obtained test piece is heated at a temperature increase rate of 10° C./min.
  • thermomechanical analyzer manufactured by Hitachi High-Tech Science Co., Ltd.
  • measure the amount of elongation of the test piece at a temperature in the range of 50 to 200°C and calculate the coefficient of linear expansion from the amount of elongation. Measure the linear expansion coefficient ⁇ of the glass fiber.
  • the glass fiber reinforced resin molded product of this embodiment if the tensile modulus E of the glass fiber becomes small, the amount of deformation when an external force is applied becomes too large, and if it becomes large, the glass fiber reinforced resin molded product becomes brittle. There is a tendency. Therefore, in the glass fiber reinforced resin molded product of this embodiment, if the tensile modulus E of the glass fiber is less than 58 GPa, the handling properties of the glass fiber reinforced resin molded product deteriorate, and the tensile modulus E of the glass fiber deteriorates. If it exceeds 92 GPa, the impact properties of the glass fiber reinforced resin molded product tend to deteriorate.
  • the tensile modulus E of the glass fibers contained in the glass fiber reinforced resin molded article is preferably in the range of 60 to 69 GPa, more preferably in the range of 62 to 67 GPa. range.
  • the tensile modulus E of the glass fiber can be measured, for example, as follows.
  • the glass fiber reinforced resin molded product is heated, for example, in a muffle furnace at 300 to 650° C. for about 0.5 to 24 hours to decompose organic substances.
  • the remaining glass fibers are placed in a platinum crucible, held at a temperature of 1600° C. for 6 hours in an electric furnace, and melted with stirring to obtain homogeneous molten glass.
  • the obtained molten glass is poured onto a carbon plate to produce a glass cullet, and then the obtained glass cullet is placed into a small cylindrical platinum bushing that has one circular nozzle tip at the bottom of the container. .
  • the platinum bushing is heated to a predetermined temperature to melt the glass cullet and obtain molten glass so that the viscosity of the glass cullet becomes 1000 ⁇ 150 poise.
  • the molten glass discharged from the nozzle tip of the platinum bushing is wound up at a predetermined speed with a winding machine so that the glass fiber diameter is 13 ⁇ 2 ⁇ m, and cooled and solidified while being stretched, so that the glass fiber has a perfect circular cross section. Obtain a glass filament.
  • One glass filament (monofilament) between the nozzle tip of the platinum bushing and the winder is collected, and the glass filament in a state where deterioration due to contact and friction is suppressed as much as possible is collected as a sample for elastic modulus evaluation.
  • the obtained monofilament was placed in the long side direction of a mount having two gripping parts and two support parts, which will be described later, along a line connecting the centers of the short sides, and glued. Create.
  • the diameter of the obtained monofilament is measured using a scanning electron microscope (manufactured by Hitachi, Ltd., trade name: S-3400), and the cross-sectional area of the monofilament is calculated from the obtained diameter.
  • the two grips in the mount were placed on the upper and lower sides of a tensile testing machine (manufactured by A&D Co., Ltd., product name: desktop material testing machine STB-1225S), with the distance between the grips set at 50 mm. Set it on the grip.
  • the two support parts in the mount were cut out, and the grip part was connected only with the monofilament, and then a tensile test was conducted at a crosshead speed of 5 mm/min.
  • a tensile test was conducted at a crosshead speed of 5 mm/min.
  • the mount has a short side of 25 mm and a long side of 75 mm, and is provided with a cut-out part in the center of the inside of which the short side is 15 mm and the long side is 50 mm.
  • the cutout portion is configured such that the short side and long side of the mount are parallel to the short side and long side of the cutout portion, respectively.
  • a grip part that is set in a grip of a tensile testing machine is provided between the short side of the cutout part and the short side of the mount paper, and a grip part is provided between the long side of the cutout part and the long side of the mount paper.
  • a support part that connects and supports the two grip parts.
  • the glass fiber reinforced resin molded product of this embodiment if the glass fiber content C exceeds 50.0% by mass based on the total amount of the glass fiber reinforced resin molded product, the resin tends to become brittle, and the glass fiber reinforced resin molded product tends to become brittle. The impact properties of the product deteriorate. On the other hand, if the glass fiber content C is less than 10.0% by mass, sufficient impact strength cannot be obtained.
  • the glass fiber content C based on the total amount of the glass fiber reinforced resin molded product is preferably in the range of 20.0 to 45.0% by mass, and more preferably, It is in the range of 25.0 to 40.0% by mass.
  • the glass fiber content C in the glass fiber reinforced molded product of this embodiment can be calculated in accordance with JIS K 7052:1999.
  • the crystallization heat Q of the glass fiber reinforced resin molded product is less than 30.0 J/g or 60.0 J/g with respect to the resin mass contained in the glass fiber reinforced resin molded product. If it exceeds the range, the impact properties of the glass fiber reinforced resin molded product tend to deteriorate.
  • the crystallization heat Q of the glass fiber reinforced resin molded product is preferably 35.0 to 50.0 J/g relative to the resin mass contained in the glass fiber reinforced resin molded product. is within the range of
  • the heat of crystallization Q of the glass fiber reinforced resin molded product with respect to the resin mass contained in the glass fiber reinforced resin molded product can be determined, for example, as follows.
  • a glass fiber-reinforced resin molded product is cut into pieces of about 10 mg to prepare test pieces, and the mass of the test pieces is measured.
  • a differential scanning calorimeter for example, manufactured by NETZCH, trade name: DSC 3500 Sirius
  • the glass fiber reinforced resin molded product was heated to 370°C at a heating rate of 40°C/min under nitrogen purge, After being held at 370°C for 10 minutes, it is cooled to 200°C at a cooling temperature of 40°C/min to obtain a DSC curve.
  • the heat of crystallization (Q 0 ) for the total mass of the test piece is determined from the peak area in the obtained DSC curve.
  • the glass fibers included in the glass fiber reinforced resin molded article of this embodiment preferably have a number average fiber length in the range of 1 to 10,000 ⁇ m, for example. If the number average fiber length of the glass fibers is less than 1 ⁇ m, sufficient impact absorption and impact resistance may not be obtained in the glass fiber reinforced resin molded product. Furthermore, setting the number average fiber length of the glass fibers to more than 10,000 ⁇ m may cause breakage of the glass fibers, more specifically, the glass filaments constituting the glass fibers, during the manufacturing process of the glass fiber reinforced resin molded product. Therefore, it is difficult.
  • the number average fiber length of the glass fibers is preferably in the range of 50 to 3,000 ⁇ m, more preferably in the range of 65 to 1,800 ⁇ m, even more preferably in the range of 80 to 900 ⁇ m, and particularly preferably in the range of 95 to 900 ⁇ m. It is in the range of 600 ⁇ m, most preferably in the range of 100-300 ⁇ m.
  • glass fibers are usually formed by bundling a plurality of glass filaments, but the glass fibers included in the glass reinforced resin molded product of this embodiment are the same as those in the glass fiber reinforced resin molded product.
  • the bundles are unbundled and present in the form of glass filaments dispersed in the glass fiber reinforced resin molded product. Therefore, the number average fiber length of the glass fibers essentially means the number average fiber length of the glass filaments in the glass fiber reinforced resin molded product.
  • the number average fiber length of the glass fibers included in the glass fiber reinforced resin molded product of this embodiment can be measured as follows.
  • the glass fiber reinforced resin molded product is heated, for example, in a muffle furnace at 300 to 650° C. for about 0.5 to 24 hours to decompose organic substances.
  • the remaining glass filaments are transferred to a glass Petri dish and dispersed on the surface of the Petri dish using acetone.
  • the fiber length of 500 or more glass filaments dispersed on the surface of the petri dish is measured using a stereomicroscope, and the number average fiber length is calculated.
  • the glass fiber-reinforced resin molded product of this embodiment has impact absorption properties at the time of breakage and resistance at a stage before breakage because D, ⁇ , E, C, and Q satisfy the above formula (1). It can be made to have both impact resistance and excellent balance with handling properties.
  • the crystallization heat Q of the glass fiber reinforced resin molded product when the crystallization heat Q of the glass fiber reinforced resin molded product is small relative to the resin mass contained in the glass fiber reinforced resin molded product, the molecular weight of the resin tends to increase. The reinforcing fibers are easily broken during resin molding.
  • the heat of crystallization Q of the glass fiber reinforced resin molded product is large relative to the resin mass contained in the glass fiber reinforced resin molded product, the crystallization rate of the resin tends to be high and the molecular weight tends to be small. The resin tends to become brittle.
  • the above formula (1) is based on the impact properties of the glass fiber reinforced resin molded product of this embodiment due to breakage and dispersion of the glass fibers during molding, and the effects of the resin and the glass fibers themselves. It is presumed that this shows a balance between the impact characteristics and
  • the glass fiber reinforced resin molded product of the present embodiment has the above-mentioned D, ⁇ , E, C, and Q within the above-mentioned ranges and satisfies the above-mentioned formula (1), so that the glass fiber-reinforced resin molded product has good impact absorption properties at the time of breakage and a high resistance to breakage. It can be made to have both impact resistance at an early stage and an excellent balance with ease of handling. It is possible to have both shock absorption at the time of fracture, impact resistance at the stage before fracture, and a good balance with handling properties. /bending strength/bending strain" is 350 or more.
  • the unnotched Charpy impact strength is an index indicating the impact absorption property at the time of fracture.
  • bending strength and bending strain are indicators of the handling properties of glass fiber-reinforced resin molded products, but when they have high impact resistance and high shock absorption, bending strength and bending strain tend to increase.
  • shock absorption properties There is a trade-off relationship between impact properties and shock absorption properties and handling properties. Therefore, "toughness coefficient x unnotched Charpy impact strength/bending strength bending strain" is an index showing that the material has both impact resistance and impact absorption, and is well balanced with handling properties.
  • the unnotched Charpy impact strength was measured using a digital impact tester (Toyo Seiki Co., Ltd.) at a test temperature of 23°C for an A-type dumbbell test piece (4 mm thick) in accordance with JIS K 7164:2005.
  • a non-notched Charpy impact test was conducted in accordance with JIS K 7111-1:2012 using a DG-UB model manufactured by Seisakusho.
  • the bending strength, bending modulus, bending strength, and bending strain of the glass fiber reinforced resin molded product were determined by cutting both ends of the dumbbell test piece in accordance with JIS K 7171:2016.
  • a test piece (length 80 mm, width 10 mm, thickness 4 mm) is measured using a precision universal testing machine (manufactured by Shimadzu Corporation, trade name: Autograph AG-Xplus 50 kN) at a test temperature of 23°C.
  • D, ⁇ , E, C, and Q preferably satisfy the following formula (1a), more preferably satisfy the following formula (2), and still more preferably satisfy the following formula (1a). (3) is satisfied. 16.87 ⁇ Q ⁇ E/(D 1/3 ⁇ C 1/2 ⁇ 2 ) ⁇ 24.90 (1a) 18.74 ⁇ Q ⁇ E/(D 1/3 ⁇ C 1/2 ⁇ 2 ) ⁇ 21.74 (2) 20.24 ⁇ Q ⁇ E/(D 1/3 ⁇ C 1/2 ⁇ 2 ) ⁇ 21.54 (3)
  • the glass fiber reinforced resin molded product of this embodiment has the above-mentioned D, ⁇ , E, C, and Q within the above-mentioned ranges and satisfies the above-mentioned formula (2), so that the glass fiber-reinforced resin molded product has good impact absorption properties at the time of breakage and a high resistance to breakage. It can be made to have a better balance with impact resistance at a stage when the material is not in use, and also with ease of handling. It is possible to achieve a better balance between shock absorption at the time of fracture, impact resistance at a stage that does not result in fracture, and even better handling properties. It means that the value of "strength/bending strength/bending strain" is 370 or more.
  • the glass fiber reinforced resin molded product of this embodiment has the above-mentioned D, ⁇ , E, C, and Q within the above-mentioned ranges and satisfies the above-mentioned formula (3), so that the glass fiber-reinforced resin molded product has good impact absorption properties at the time of breakage and a high resistance to breakage. It is possible to achieve an even better balance between impact resistance and handling properties.
  • the combination of shock absorption at the time of fracture and impact resistance at the stage before fracture, as well as an even better balance with ease of handling, is the combination of "toughness coefficient x unnotched Charpy impact". It means that the value of "strength/bending strength/bending strain" is 400 or more.
  • the glass fiber reinforced resin molded product of this embodiment can be used for parts such as casings and motherboards, frames, speakers, and antennas of portable electronic devices such as smartphones, tablets, notebook computers, and mobile computers, switches, gears, and connectors. , motor parts, semiconductor/LCD manufacturing equipment parts, electrical and electronic parts such as insulation films and wire coating materials, automotive parts such as bearings, seal rings, gears, transmission parts, thrust washers, piston parts, and spindle nuts, bracket fasteners, and compartments. Examples include aircraft parts such as retainers, vent grilles, structural members, satellite parts, and 3D printer materials.
  • Example 1 In this example, first, 30.0% by mass (glass fiber content C) of glass fiber (manufactured by Nitto Boseki Co., Ltd., NE Glass Chopped Strand) based on the total amount and polyether of 70.0% by mass based on the total amount.
  • Ether ketone manufactured by Daicel Evonik Co., Ltd., product name: Vesta Keep L4000G (described as "PEEK L4000G” in Tables 1 and 2)
  • PEEK L4000G product name: TEM-26SS
  • the glass fiber has a linear expansion coefficient ⁇ of 3.3 ppm/K, a tensile modulus E of 64 GPa, and a fiber diameter D of 6.5 ⁇ m.
  • injection molding was performed using an injection molding machine (manufactured by Nissei Jushi Kogyo Co., Ltd., product name: NEX80-9E) at a mold temperature of 200°C and an injection temperature of 410°C.
  • a multipurpose test piece type A1 (thickness: 4 mm) according to JIS K 7139:2009 was prepared as a glass fiber reinforced resin molded article of this example.
  • the heat of crystallization Q of the glass fiber reinforced resin molded product was determined with respect to the resin mass contained in the glass fiber reinforced resin molded product by the method described above. Then, from the above D, ⁇ , E, C, and Q, the value of Q ⁇ E/(D 1/3 ⁇ C 1/2 ⁇ 2 ) was calculated.
  • Example 2 In this example, first, 40.0% by mass (glass fiber content C) of glass fibers with a fiber diameter D of 11 ⁇ m (manufactured by Nitto Boseki Co., Ltd., NE glass chopped strand) and 60.0% by mass of polyether ether ketone (manufactured by Daicel Evonik Co., Ltd., product name: Vesta Keep 2000G (indicated as "PEEK 2000G” in Tables 1 and 2)) was mixed in a twin-screw kneader (Shibaura Kikai Co., Ltd.).
  • the glass fiber reinforced resin of this example was prepared in exactly the same manner as in Example 1, except that the resin pellets were obtained by kneading them at a kneading temperature of 390°C and a screw rotation speed of 100 rpm.
  • a multipurpose test piece type A1 (thickness: 4 mm) according to JIS K 7139:2009 was produced as a molded product.
  • Example 3 In this example, first, 30.0% by mass (glass fiber content C) of glass fibers with a fiber diameter D of 11 ⁇ m (manufactured by Nitto Boseki Co., Ltd., NE glass chopped strand) and 70.0% by mass of polyetheretherketone (manufactured by Daicel Evonik Co., Ltd., product name: Vesta Keep 2000G (indicated as "PEEK 2000G” in Tables 1 and 2)) was mixed in a twin-screw kneader (Shibaura Machinery Co., Ltd.).
  • the glass fiber reinforced resin of this example was prepared in exactly the same manner as in Example 1, except that the resin pellets were obtained by kneading them at a kneading temperature of 390°C and a screw rotation speed of 100 rpm.
  • a multipurpose test piece type A1 (thickness: 4 mm) according to JIS K 7139:2009 was produced as a molded product.
  • Example 4 In this example, first, 20.0% by mass (glass fiber content C) of glass fibers with a fiber diameter D of 11 ⁇ m (manufactured by Nitto Boseki Co., Ltd., NE glass chopped strand) and 80.0% by mass of polyether ether ketone (manufactured by Daicel Evonik Co., Ltd., product name: Vesta Keep 2000G (indicated as "PEEK 2000G” in Tables 1 and 2)) was mixed in a twin-screw kneader (Shibaura Kikai Co., Ltd.).
  • the glass fiber reinforced resin of this example was prepared in exactly the same manner as in Example 1, except that the resin pellets were obtained by kneading them at a kneading temperature of 390°C and a screw rotation speed of 100 rpm.
  • a multipurpose test piece type A1 (thickness: 4 mm) according to JIS K 7139:2009 was produced as a molded product.
  • Comparative example 1 This comparative example is exactly the same as Example 2, except that glass fiber (E glass chopped strand, manufactured by Nittobo Co., Ltd.) having a linear expansion coefficient ⁇ of 5.5 ppm/K and a tensile modulus E of 75 GPa was used.
  • glass fiber E glass chopped strand, manufactured by Nittobo Co., Ltd.
  • a multipurpose test piece type A1 thickness: 4 mm
  • JIS K 7139:2009 JIS K 7139:2009 was produced.
  • Comparative example 2 This comparative example is the same as Example 2 except that glass fibers having a linear expansion coefficient ⁇ of 2.8 ppm/K, a tensile modulus E of 86 GPa, and a fiber diameter D of 9 ⁇ m based on the total amount of glass fibers were used.
  • a multipurpose test piece type A1 thickness: 4 mm
  • JIS K 7139:2009 was prepared as a glass fiber reinforced resin molded article of this comparative example.
  • the glass fiber manufactured by Nittobo Co., Ltd., E glass chopped strand
  • the glass fiber diameter D is 11 ⁇ m.
  • a multipurpose test piece type A1 (thickness: 4 mm) according to JIS K 7139:2009 was produced as a glass fiber reinforced resin molded product of this comparative example in the same manner as in Example 1 except that glass fiber was used. .
  • Comparative example 4 This comparative example is exactly the same as Example 1 except that glass fiber (E glass chopped strand, manufactured by Nittobo Co., Ltd.) having a linear expansion coefficient ⁇ of 5.5 ppm/K and a tensile modulus E of 75 GPa was used.
  • glass fiber E glass chopped strand, manufactured by Nittobo Co., Ltd.
  • a multipurpose test piece type A1 thickness: 4 mm
  • JIS K 7139:2009 JIS K 7139:2009 was produced.
  • Comparative example 5 This comparative example was completely the same as Example 1 except that glass fibers having a linear expansion coefficient ⁇ of 2.8 ppm/K, a tensile modulus E of 86 GPa, and a fiber diameter D of 11 ⁇ m were used.
  • a glass fiber reinforced resin molded product of a comparative example a multipurpose test piece type A1 (thickness: 4 mm) according to JIS K 7139:2009 was produced.
  • the glass fiber has a linear expansion coefficient ⁇ of 3.3 ppm/K, a tensile modulus E of 64 GPa, and a fiber diameter D of 6.5 ⁇ m.
  • a multipurpose test piece according to JIS K 7139:2009 was prepared as a glass fiber reinforced resin molded product of this comparative example using the same method as in Example 1 except that the resin pellets obtained in this comparative example were used.
  • Type A1 (thickness: 4 mm) was produced.
  • Comparative example 7 This comparative example is exactly the same as Comparative Example 6, except that glass fiber (E glass chopped strand, manufactured by Nittobo Co., Ltd.) having a linear expansion coefficient ⁇ of 5.5 ppm/K and a tensile modulus E of 75 GPa was used.
  • glass fiber E glass chopped strand, manufactured by Nittobo Co., Ltd.
  • a multipurpose test piece type A1 thickness: 4 mm
  • JIS K 7139:2009 JIS K 7139:2009 was produced.
  • the glass fiber has a linear expansion coefficient ⁇ of 3.3 ppm/K, a tensile modulus E of 64 GPa, and a fiber diameter D of 11 ⁇ m.
  • a multipurpose test piece according to JIS K 7139:2009 was prepared as a glass fiber reinforced resin molded product of this comparative example using the same method as in Example 1 except that the resin pellets obtained in this comparative example were used.
  • Type A1 (thickness: 4 mm) was produced.
  • Comparative example 9 This comparative example is exactly the same as Comparative Example 8, except that glass fiber (E glass chopped strand, manufactured by Nittobo Co., Ltd.) having a linear expansion coefficient ⁇ of 5.5 ppm/K and a tensile modulus E of 75 GPa was used.
  • glass fiber E glass chopped strand, manufactured by Nittobo Co., Ltd.
  • a multipurpose test piece type A1 thickness: 4 mm
  • the fiber diameter D of the glass fiber is in the range of 5.0 to 17.0 ⁇ m, and the linear expansion coefficient ⁇ of the glass fiber is 2.0 ⁇ m.
  • the tensile modulus E of the glass fiber is in the range of 58 to 92 GPa, and the glass fiber content C with respect to the total amount of the glass fiber reinforced resin molded product is in the range of 0 to 6.0 ppm/K.
  • the crystallization heat Q of the glass fiber reinforced resin molded product is in the range of 30.0 to 60.0 J/g based on the resin mass contained in the glass fiber reinforced resin molded product, and the It is clear that D, ⁇ , E, C, and Q satisfy the above formula (1).
  • the glass fiber-reinforced resin molded products of Examples 1 to 4 have both shock absorption properties at the time of breakage and impact resistance at the stage of non-breakage, and also have excellent balance with ease of handling.
  • the value of toughness coefficient x unnotched Charpy impact strength/bending strength bending strain is 350 or more, and the impact absorption property and resistance to breakage are higher than that of the glass fiber reinforced resin molded products of Comparative Examples 1 to 9. It is clear that it has both impact resistance at an early stage and also has an excellent balance with ease of handling.
  • the glass fiber reinforced resin molded product of Example 1 has exactly the same values of toughness coefficient x unnotched Charpy impact strength/bending strength bending strain except that the glass composition of the glass fiber is equivalent to E glass. It is 128% of the glass fiber reinforced resin molded product of Comparative Example 4 with the structure, and the impact absorption property at the time of breakage and the impact resistance at the stage before destruction are 128% of the glass fiber reinforced resin molded product of Comparative Example 4. It is clear that it has an excellent balance with both physical properties and ease of handling.
  • the glass fiber reinforced resin molded product of Example 2 has exactly the same values of toughness coefficient x unnotched Charpy impact strength/bending strength bending strain except that the glass composition of the glass fiber is equivalent to E glass. It is 146% of the glass fiber reinforced resin molded product of Comparative Example 1 with the structure, and has a higher impact absorption property at the time of breakage and impact resistance at a stage before breaking than the glass fiber reinforced resin molded product of Comparative Example 1. It is clear that it has an excellent balance with both physical properties and ease of handling.
  • the glass fiber reinforced resin molded product of Comparative Example 6 has exactly the same values of toughness coefficient x unnotched Charpy impact strength/bending strength bending strain except that the glass composition of the glass fiber is equivalent to E glass. It is clear that it is 118% of the glass fiber reinforced resin molded product of Comparative Example 7 having the following structure.
  • the glass fiber reinforced resin molded product of Comparative Example 8 has exactly the same values of toughness coefficient x unnotched Charpy impact strength/bending strength bending strain except that the glass composition of the glass fiber is equivalent to E glass. It is clear that it is 110% of the glass fiber reinforced resin molded product of Comparative Example 9 having the following structure.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Health & Medical Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Medicinal Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Organic Chemistry (AREA)
  • Materials Engineering (AREA)
  • Engineering & Computer Science (AREA)
  • Manufacturing & Machinery (AREA)
  • Inorganic Chemistry (AREA)
  • Reinforced Plastic Materials (AREA)
  • Compositions Of Macromolecular Compounds (AREA)
  • Manufacture Of Macromolecular Shaped Articles (AREA)
PCT/JP2023/003464 2022-04-15 2023-02-02 ガラス繊維強化樹脂成形品 Ceased WO2023199576A1 (ja)

Priority Applications (5)

Application Number Priority Date Filing Date Title
JP2024514812A JPWO2023199576A1 (cg-RX-API-DMAC7.html) 2022-04-15 2023-02-02
GB2410568.6A GB2629724A (en) 2022-04-15 2023-02-02 Glass fiber-reinforced resin molded product
KR1020247027855A KR20250007494A (ko) 2022-04-15 2023-02-02 유리 섬유 강화 수지 성형품
US18/730,844 US20250101191A1 (en) 2022-04-15 2023-02-02 Glass fiber-reinforced resin molded product
CN202380032168.8A CN118974145A (zh) 2022-04-15 2023-02-02 玻璃纤维强化树脂成型品

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2022-067868 2022-04-15
JP2022067868 2022-04-15

Publications (1)

Publication Number Publication Date
WO2023199576A1 true WO2023199576A1 (ja) 2023-10-19

Family

ID=88329581

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2023/003464 Ceased WO2023199576A1 (ja) 2022-04-15 2023-02-02 ガラス繊維強化樹脂成形品

Country Status (7)

Country Link
US (1) US20250101191A1 (cg-RX-API-DMAC7.html)
JP (1) JPWO2023199576A1 (cg-RX-API-DMAC7.html)
KR (1) KR20250007494A (cg-RX-API-DMAC7.html)
CN (1) CN118974145A (cg-RX-API-DMAC7.html)
GB (1) GB2629724A (cg-RX-API-DMAC7.html)
TW (1) TWI921639B (cg-RX-API-DMAC7.html)
WO (1) WO2023199576A1 (cg-RX-API-DMAC7.html)

Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US20170101338A1 (en) * 2013-07-15 2017-04-13 Ppg Industries Ohio, Inc. Glass compositions, fiberizable glass compositions, and glass fibers made therefrom
WO2020166518A1 (ja) * 2019-02-12 2020-08-20 日東紡績株式会社 ガラス繊維強化樹脂成形品
JP2021003899A (ja) * 2020-10-08 2021-01-14 日東紡績株式会社 ガラス繊維強化樹脂成形品
JP2021516206A (ja) * 2018-03-07 2021-07-01 エレクトリック グラス ファイバー アメリカ, エルエルシー ガラス組成物、繊維化可能なガラス組成物、およびそれから作成されたガラス繊維
WO2022034903A1 (ja) * 2020-08-14 2022-02-17 Agc株式会社 樹脂組成物、成形体、複合体及びその用途
WO2022254918A1 (ja) * 2021-05-31 2022-12-08 日東紡績株式会社 ガラス強化樹脂成形品

Family Cites Families (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2002013899A (ja) * 2000-06-30 2002-01-18 Tomy Co Ltd 空気銃玩具、銃身及び玉発射装置
JP2005187523A (ja) * 2003-12-24 2005-07-14 Nippon Oil Corp 排出装置用耐熱性frp部材およびこれを使用したfrp製排出装置
TW201428019A (zh) * 2012-10-01 2014-07-16 Sumitomo Bakelite Co 樹脂組成物、樹脂硬化物、透明複合體、顯示元件用基板及面光源用基板
CN109843973B (zh) * 2016-08-02 2021-12-03 索尔维特殊聚合物美国有限责任公司 包含低分子量芳香族化合物的聚(芳醚酮)(paek)组合物
JP7136389B2 (ja) * 2020-06-17 2022-09-13 昭和電工マテリアルズ株式会社 積層板、プリント配線板、半導体パッケージ及び積層板の製造方法

Patent Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US20170101338A1 (en) * 2013-07-15 2017-04-13 Ppg Industries Ohio, Inc. Glass compositions, fiberizable glass compositions, and glass fibers made therefrom
JP2021516206A (ja) * 2018-03-07 2021-07-01 エレクトリック グラス ファイバー アメリカ, エルエルシー ガラス組成物、繊維化可能なガラス組成物、およびそれから作成されたガラス繊維
WO2020166518A1 (ja) * 2019-02-12 2020-08-20 日東紡績株式会社 ガラス繊維強化樹脂成形品
WO2022034903A1 (ja) * 2020-08-14 2022-02-17 Agc株式会社 樹脂組成物、成形体、複合体及びその用途
JP2021003899A (ja) * 2020-10-08 2021-01-14 日東紡績株式会社 ガラス繊維強化樹脂成形品
WO2022254918A1 (ja) * 2021-05-31 2022-12-08 日東紡績株式会社 ガラス強化樹脂成形品

Also Published As

Publication number Publication date
TWI921639B (zh) 2026-04-11
CN118974145A (zh) 2024-11-15
TW202405078A (zh) 2024-02-01
US20250101191A1 (en) 2025-03-27
KR20250007494A (ko) 2025-01-14
GB202410568D0 (en) 2024-09-04
JPWO2023199576A1 (cg-RX-API-DMAC7.html) 2023-10-19
GB2629724A (en) 2024-11-06

Similar Documents

Publication Publication Date Title
EP3892596B1 (en) Glass fiber-reinforced resin molded article
US11827770B2 (en) Glass fiber-reinforced resin molded product
EP4249445B1 (en) Glass composition for glass fibers, glass fiber, and glass fiber-reinforced resin molded product
JP7636681B2 (ja) ガラス繊維強化樹脂板
EP4299541A1 (en) Glass composition for glass fibers, glass fiber, and glass fiber-reinforced resin molded article
TWI783728B (zh) 玻璃纖維強化樹脂板
JP2009143765A (ja) ガラス繊維集束剤、ガラス繊維とその製造方法及びガラス繊維強化熱可塑性樹脂
JP7856911B2 (ja) ガラス強化樹脂成形品
KR20250007494A (ko) 유리 섬유 강화 수지 성형품
US12139591B2 (en) Glass fiber-reinforced resin molded article
JP7393714B1 (ja) 扁平断面ガラス繊維、ガラス繊維強化樹脂組成物およびガラス繊維強化樹脂成形品
CN119365335A (zh) 金属-玻璃纤维强化热塑性树脂复合材料
EP3584273A1 (en) Reinforcing material and resin molded article

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 23787999

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2024514812

Country of ref document: JP

Kind code of ref document: A

ENP Entry into the national phase

Ref document number: 202410568

Country of ref document: GB

Kind code of ref document: A

Free format text: PCT FILING DATE = 20230202

WWE Wipo information: entry into national phase

Ref document number: 2410568.6

Country of ref document: GB

WWE Wipo information: entry into national phase

Ref document number: 18730844

Country of ref document: US

WWE Wipo information: entry into national phase

Ref document number: 202380032168.8

Country of ref document: CN

WWP Wipo information: published in national office

Ref document number: 2410568.6

Country of ref document: GB

NENP Non-entry into the national phase

Ref country code: DE

WWP Wipo information: published in national office

Ref document number: 18730844

Country of ref document: US

122 Ep: pct application non-entry in european phase

Ref document number: 23787999

Country of ref document: EP

Kind code of ref document: A1