WO2023190585A1 - 熱伝導性シート、その装着方法及び製造方法 - Google Patents

熱伝導性シート、その装着方法及び製造方法 Download PDF

Info

Publication number
WO2023190585A1
WO2023190585A1 PCT/JP2023/012649 JP2023012649W WO2023190585A1 WO 2023190585 A1 WO2023190585 A1 WO 2023190585A1 JP 2023012649 W JP2023012649 W JP 2023012649W WO 2023190585 A1 WO2023190585 A1 WO 2023190585A1
Authority
WO
WIPO (PCT)
Prior art keywords
thermally conductive
conductive sheet
silicone compound
alkyl
filler
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2023/012649
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
健太 黒尾
弘通 岩▲崎▼
大希 工藤
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sekisui Polymatech Co Ltd
Original Assignee
Sekisui Polymatech Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sekisui Polymatech Co Ltd filed Critical Sekisui Polymatech Co Ltd
Priority to CN202380022675.3A priority Critical patent/CN118715612A/zh
Priority to EP23780594.0A priority patent/EP4503119A4/en
Priority to JP2023562863A priority patent/JP7424714B1/ja
Priority to US18/840,172 priority patent/US20250163299A1/en
Priority to KR1020247027819A priority patent/KR20240168304A/ko
Publication of WO2023190585A1 publication Critical patent/WO2023190585A1/ja
Priority to JP2024002618A priority patent/JP2024032772A/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Images

Classifications

    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J5/00—Manufacture of articles or shaped materials containing macromolecular substances
    • C08J5/18—Manufacture of films or sheets
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10W—GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10
    • H10W40/00—Arrangements for thermal protection or thermal control
    • H10W40/10—Arrangements for heating
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09J—ADHESIVES; NON-MECHANICAL ASPECTS OF ADHESIVE PROCESSES IN GENERAL; ADHESIVE PROCESSES NOT PROVIDED FOR ELSEWHERE; USE OF MATERIALS AS ADHESIVES
    • C09J7/00—Adhesives in the form of films or foils
    • C09J7/30—Adhesives in the form of films or foils characterised by the adhesive composition
    • C09J7/35—Heat-activated
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B27/00—Layered products comprising a layer of synthetic resin
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B7/00—Layered products characterised by the relation between layers; Layered products characterised by the relative orientation of features between layers, or by the relative values of a measurable parameter between layers, i.e. products comprising layers having different physical, chemical or physicochemical properties; Layered products characterised by the interconnection of layers
    • B32B7/04—Interconnection of layers
    • B32B7/12—Interconnection of layers using interposed adhesives or interposed materials with bonding properties
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K3/00—Use of inorganic substances as compounding ingredients
    • C08K3/01—Use of inorganic substances as compounding ingredients characterized by their specific function
    • C08K3/013—Fillers, pigments or reinforcing additives
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K5/00—Use of organic ingredients
    • C08K5/54—Silicon-containing compounds
    • C08K5/541—Silicon-containing compounds containing oxygen
    • C08K5/5415—Silicon-containing compounds containing oxygen containing at least one Si—O bond
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K5/00—Use of organic ingredients
    • C08K5/54—Silicon-containing compounds
    • C08K5/541—Silicon-containing compounds containing oxygen
    • C08K5/5415—Silicon-containing compounds containing oxygen containing at least one Si—O bond
    • C08K5/5419—Silicon-containing compounds containing oxygen containing at least one Si—O bond containing at least one Si—C bond
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L83/00—Compositions of macromolecular compounds obtained by reactions forming in the main chain of the macromolecule a linkage containing silicon with or without sulfur, nitrogen, oxygen or carbon only; Compositions of derivatives of such polymers
    • C08L83/04—Polysiloxanes
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
    • C09D183/00—Coating compositions based on macromolecular compounds obtained by reactions forming in the main chain of the macromolecule a linkage containing silicon, with or without sulfur, nitrogen, oxygen, or carbon only; Coating compositions based on derivatives of such polymers
    • C09D183/04—Polysiloxanes
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09J—ADHESIVES; NON-MECHANICAL ASPECTS OF ADHESIVE PROCESSES IN GENERAL; ADHESIVE PROCESSES NOT PROVIDED FOR ELSEWHERE; USE OF MATERIALS AS ADHESIVES
    • C09J11/00—Features of adhesives not provided for in group C09J9/00, e.g. additives
    • C09J11/02—Non-macromolecular additives
    • C09J11/04—Non-macromolecular additives inorganic
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09J—ADHESIVES; NON-MECHANICAL ASPECTS OF ADHESIVE PROCESSES IN GENERAL; ADHESIVE PROCESSES NOT PROVIDED FOR ELSEWHERE; USE OF MATERIALS AS ADHESIVES
    • C09J5/00—Adhesive processes in general; Adhesive processes not provided for elsewhere, e.g. relating to primers
    • C09J5/06—Adhesive processes in general; Adhesive processes not provided for elsewhere, e.g. relating to primers involving heating of the applied adhesive
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09J—ADHESIVES; NON-MECHANICAL ASPECTS OF ADHESIVE PROCESSES IN GENERAL; ADHESIVE PROCESSES NOT PROVIDED FOR ELSEWHERE; USE OF MATERIALS AS ADHESIVES
    • C09J9/00—Adhesives characterised by their physical nature or the effects produced, e.g. glue sticks
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09K—MATERIALS FOR MISCELLANEOUS APPLICATIONS, NOT PROVIDED FOR ELSEWHERE
    • C09K5/00—Heat-transfer, heat-exchange or heat-storage materials, e.g. refrigerants; Materials for the production of heat or cold by chemical reactions other than by combustion
    • C09K5/08—Materials not undergoing a change of physical state when used
    • C09K5/14—Solid materials, e.g. powdery or granular
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10W—GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10
    • H10W40/00—Arrangements for thermal protection or thermal control
    • H10W40/20—Arrangements for cooling
    • H10W40/25—Arrangements for cooling characterised by their materials
    • H10W40/251—Organics
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10W—GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10
    • H10W40/00—Arrangements for thermal protection or thermal control
    • H10W40/20—Arrangements for cooling
    • H10W40/25—Arrangements for cooling characterised by their materials
    • H10W40/257—Arrangements for cooling characterised by their materials having a heterogeneous or anisotropic structure, e.g. powder or fibres in a matrix, wire mesh or porous structures
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B32—LAYERED PRODUCTS
    • B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
    • B32B2307/00—Properties of the layers or laminate
    • B32B2307/30—Properties of the layers or laminate having particular thermal properties
    • B32B2307/302—Conductive
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G77/00—Macromolecular compounds obtained by reactions forming a linkage containing silicon with or without sulfur, nitrogen, oxygen or carbon in the main chain of the macromolecule
    • C08G77/04—Polysiloxanes
    • C08G77/12—Polysiloxanes containing silicon bound to hydrogen
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G77/00—Macromolecular compounds obtained by reactions forming a linkage containing silicon with or without sulfur, nitrogen, oxygen or carbon in the main chain of the macromolecule
    • C08G77/04—Polysiloxanes
    • C08G77/20—Polysiloxanes containing silicon bound to unsaturated aliphatic groups
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J2383/00—Characterised by the use of macromolecular compounds obtained by reactions forming in the main chain of the macromolecule a linkage containing silicon with or without sulfur, nitrogen, oxygen, or carbon only; Derivatives of such polymers
    • C08J2383/04—Polysiloxanes
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K3/00—Use of inorganic substances as compounding ingredients
    • C08K3/02—Elements
    • C08K3/08—Metals
    • C08K2003/0812—Aluminium
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K3/00—Use of inorganic substances as compounding ingredients
    • C08K3/18—Oxygen-containing compounds, e.g. metal carbonyls
    • C08K3/20—Oxides; Hydroxides
    • C08K3/22—Oxides; Hydroxides of metals
    • C08K2003/2227—Oxides; Hydroxides of metals of aluminium
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K2201/00—Specific properties of additives
    • C08K2201/001—Conductive additives
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09J—ADHESIVES; NON-MECHANICAL ASPECTS OF ADHESIVE PROCESSES IN GENERAL; ADHESIVE PROCESSES NOT PROVIDED FOR ELSEWHERE; USE OF MATERIALS AS ADHESIVES
    • C09J2203/00—Applications of adhesives in processes or use of adhesives in the form of films or foils
    • C09J2203/326—Applications of adhesives in processes or use of adhesives in the form of films or foils for bonding electronic components such as wafers, chips or semiconductors
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09J—ADHESIVES; NON-MECHANICAL ASPECTS OF ADHESIVE PROCESSES IN GENERAL; ADHESIVE PROCESSES NOT PROVIDED FOR ELSEWHERE; USE OF MATERIALS AS ADHESIVES
    • C09J2301/00—Additional features of adhesives in the form of films or foils
    • C09J2301/40—Additional features of adhesives in the form of films or foils characterized by the presence of essential components
    • C09J2301/408—Additional features of adhesives in the form of films or foils characterized by the presence of essential components additives as essential feature of the adhesive layer
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09J—ADHESIVES; NON-MECHANICAL ASPECTS OF ADHESIVE PROCESSES IN GENERAL; ADHESIVE PROCESSES NOT PROVIDED FOR ELSEWHERE; USE OF MATERIALS AS ADHESIVES
    • C09J2301/00—Additional features of adhesives in the form of films or foils
    • C09J2301/40—Additional features of adhesives in the form of films or foils characterized by the presence of essential components
    • C09J2301/414—Additional features of adhesives in the form of films or foils characterized by the presence of essential components presence of a copolymer

Definitions

  • the present invention relates to a thermally conductive sheet, and for example, to a thermally conductive sheet that is used by being placed between a heat generating element and a heat radiating element.
  • heat radiators such as heat sinks are generally used to radiate heat generated from heat generating elements such as semiconductor elements and mechanical parts. It is known that a thermally conductive sheet is placed between a heat generating element and a heat radiating element for the purpose of increasing the efficiency of heat transfer to the heat radiating element.
  • Patent Document 1 discloses a heat dissipation sheet that includes at least an alkyl group-introduced silicone oil, an ⁇ -olefin, and a thermally conductive filler, is putty-like at room temperature, and softens and becomes fluid when heated.
  • thermally conductive sheet a thermally conductive sheet using polymer gel is also known.
  • Patent Document 2 describes a heat dissipating sheet made of a composition containing a polymer gel, a compound that is solid or paste-like at room temperature and becomes liquid when heated, and a thermally conductive filler, which softens when heated.
  • a heat-softening heat dissipating sheet is disclosed.
  • Patent Document 3 discloses a thermally conductive sheet including a thermally conductive resin layer, the thermally conductive resin layer comprising a binder resin containing wax and a thermally conductive filler dispersed in the binder resin.
  • thermoly conductive sheet containing a silicone gel is used as a binder resin in a thermally conductive sheet containing.
  • the phase change sheets disclosed in Patent Documents 1 to 3 above and thermally conductive sheets using polymer gels such as silicone gels have high flexibility, so they have good followability to heat radiators and heating elements. This makes it possible to improve heat conduction performance.
  • thermally conductive sheets often have an organic polymer having a crosslinked structure as a matrix, and in that case, it is known that due to the characteristics of the organic polymer, the sheet expands when the temperature changes and the temperature rises. Further, generally, each member (substrate, heating element, heat radiating element, etc.) within an electronic device also expands to a certain extent at high temperatures. Therefore, when a thermally conductive sheet is used, for example, installed between a heating element and a heat radiating element, the expansion of each member at high temperatures increases the load on the heating element and heat radiating element, which can cause various problems. It can be. Further, in recent years, as electronic devices have become smaller, the rigidity of each member within the electronic devices has been set lower, and small loads have become a concern.
  • an object of the present invention is to provide a thermally conductive sheet that has excellent thermal conductivity, suppresses expansion at high temperatures, and can reduce the load on a heating element, a heat radiating element, and the like.
  • the present invention includes a binder component that is a mixture of a silicone matrix (A) and an alkyl silicone compound (B), and a thermally conductive filler (C) that is dispersed in the binder component. It has been discovered that the above problems can be solved by a thermally conductive sheet in which the content of the alkyl silicone compound (B) is in a specific range and the expansion coefficient X is in a certain range as measured by a thermomechanical analyzer (TMA). completed. That is, the present invention provides the following [1] to [11].
  • a binder component that is a mixture of a silicone matrix (A) and an alkyl silicone compound (B), and a thermally conductive filler (C) dispersed in the binder component,
  • the content is 2.0 to 20 parts by mass based on a total of 100 parts by mass of the silicone matrix (A) and the alkyl silicone compound (B), and the measurement is performed at a heating rate of 2°C/min and a compressive load of 0.01N.
  • a thermally conductive sheet having an expansion coefficient X of -2.0% or more and less than 0% as measured by a thermomechanical analyzer (TMA) at a temperature of 30 to 80°C.
  • thermally conductive sheet according to any one of [1] to [4] above, wherein the thermally conductive filler (C) has a volumetric filling rate of 30 to 85% by volume.
  • 0.1 to 18 parts by mass of a compatible substance (D) is contained based on a total of 100 parts by mass of the silicone matrix (A) and the alkyl silicone compound (B), [1] to [5] The thermally conductive sheet according to any one of the above.
  • a heat radiating member comprising the thermally conductive sheet according to any one of [1] to [6] above and a heat radiator, and the thermally conductive sheet is attached to the surface of the heat radiator.
  • a binder component that is a mixture of a silicone matrix (A) and an alkyl silicone compound (B), and a thermally conductive filler (C) dispersed in the binder component,
  • the content is 2.0 to 20 parts by mass based on a total of 100 parts by mass of the silicone matrix (A) and the alkyl silicone compound (B), and the measurement is performed at a heating rate of 2°C/min and a compressive load of 0.01N.
  • TMA thermomechanical analyzer
  • thermoly conductive sheet that has excellent thermal conductivity, suppresses expansion at high temperatures, and can reduce the load on a heating element, a heat radiating element, and the like.
  • FIG. 2 is a diagram illustrating a measuring device that measures thermal resistance.
  • the thermally conductive sheet of the present invention comprises a binder component which is a mixture of a silicone matrix (A) and an alkyl silicone compound (B), and a thermally conductive filler (C) dispersed in the binder component,
  • the content of the silicone compound (B) is 2.0 to 20 parts by mass based on the total of 100 parts by mass of the silicone matrix (A) and the alkyl silicone compound (B)
  • the heating rate is 2°C/min
  • the compression is
  • the expansion coefficient X measured by a thermomechanical analyzer (TMA) under the conditions of a load of 0.01N and a measurement temperature of 30 to 80°C is -2.0% or more and less than 0%.
  • the thermally conductive sheet of the present invention has excellent thermal conductivity and can suppress expansion when used at high temperatures.
  • the thermally conductive sheet of the present invention has an expansion coefficient X of -2.0 as measured by a thermomechanical analyzer (TMA) under the conditions of a compressive load of 0.01 N, a measurement temperature of 30 to 80°C, and a temperature increase rate of 2°C/min. It is 0% or more and less than 0%.
  • TMA thermomechanical analyzer
  • the expansion coefficient X exceeds 0%, high-temperature expansion cannot be suppressed, and the load on the heating element, heat radiating element, etc. becomes large. If the expansion coefficient It becomes difficult for the silicone compound to be uniformly dispersed, and the two are likely to separate, causing pump-out.
  • the thermally conductive sheet tends to become brittle at temperatures below the melting point of the alkyl silicone compound. Furthermore, the thermal resistance value of the thermally conductive sheet tends to vary.
  • a large expansion coefficient means a magnitude toward a positive numerical value side. For example, between 0% and -2.0%, -2.0% means that "the expansion rate is smaller" or "the expansion can be suppressed".
  • the expansion coefficient X is preferably -1.5% or more and -0.01% or less, more preferably -1. It is 2% or more and -0.3% or less, more preferably -1.0% or more and -0.5% or less.
  • the expansion coefficient X can be adjusted to a desired value by adjusting the type and amount of the alkyl silicone compound (B), which will be described later, contained in the thermally conductive sheet.
  • the alkyl silicone compound (B) can also be adjusted by the hardness of the silicone matrix, the shape and amount of the thermally conductive filler, and the amount and volatilization amount of the compatible substance (D). More specifically, in order to adjust the expansion coefficient It is possible to employ methods such as increasing the filling amount of the thermally conductive filler, or blending a compatible substance (D) so that the compatible substance remains in the thermally conductive sheet.
  • thermally conductive filler As the thermally conductive filler and orienting it in a predetermined direction, it is possible to adjust the expansion coefficient in the predetermined direction so that it does not become large. Furthermore, from the perspective of increasing the flexibility and thermal conductivity of the thermally conductive sheet, it is important to keep the filling amount of the thermally conductive filler within the range described below, avoid increasing the hardness of the silicone matrix too much, and incorporate an alkyl silicone compound. It is preferable to adjust the expansion coefficient X within the above range by adjusting the amount.
  • the expansion coefficient X in the present invention means the expansion coefficient in the thickness direction of the thermally conductive sheet, and is measured by a thermomechanical analyzer (TMA) as follows. First, the thermally conductive sheet is compressed at room temperature (23° C.) with a compressive load of 0.01N. The thickness of the thermally conductive sheet at this time is defined as the initial thickness (mm). Next, with the compressive load still applied, the temperature was raised from 30 °C to 80 °C at a temperature increase rate of 2 °C/min, and the expansion coefficient (%) at 30 °C and the expansion coefficient (%) at 80 °C were determined, respectively.
  • the expansion coefficient at 30°C is determined as follows from the thickness (mm) of the thermally conductive sheet at 30°C and the initial thickness (mm).
  • the silicone matrix (A) is preferably a silicone that does not have fluidity at either room temperature (23°C) or high temperature (80°C). Since the silicone matrix (A) does not have fluidity, it can ensure the shape retention of the thermally conductive sheet at room temperature and high temperature. Further, as the silicone matrix (A) of the present invention, for example, silicone rubber may be used. By using silicone rubber, it can be easily compressed and deformed, making it easier to assemble between the heat generating element and the heat radiating element. Further, since certain compression characteristics can be imparted to the thermally conductive sheet, reliability can be improved.
  • the silicone used for the silicone matrix (A) may be either a condensation reaction type or an addition reaction type. Reactive type is preferred.
  • the silicone matrix (A) can be obtained, for example, by curing the curable silicone composition (A1).
  • the curable silicone composition (A1) may consist of, for example, a base agent and a curing agent.
  • the curable silicone composition (A1) is composed of an alkenyl group-containing organopolysiloxane as a main component and a hydrogen organopolysiloxane as a curing agent, from the viewpoint that it is easy to highly fill the thermally conductive filler. It is preferable to contain.
  • the curable silicone composition (A1) is preferably in a liquid state before curing. Since the curable silicone composition (A1) is liquid before curing, it is easy to highly fill the thermally conductive filler, and furthermore, the alkyl silicone compound (B) can be dispersed in the curable silicone composition (A1). It becomes easier to do so.
  • liquid refers to something that is liquid at room temperature (23° C.) and under 1 atmosphere.
  • silicone matrix (A) it is preferable to use a three-dimensionally crosslinked silicone matrix as the silicone matrix (A) in order to ensure the shape retention of the thermally conductive sheet.
  • a three-dimensionally crosslinked silicone matrix for example, in the case of an addition reaction type, curing containing an alkenyl group-containing organopolysiloxane having at least three or more alkenyl groups in one molecule, or a hydrogen organopolysiloxane having at least three or more hydrogens added to silicon atoms.
  • the silicone composition (A1) may be cured.
  • the content of the silicone matrix (A) may be, for example, about 15 to 70% by volume, preferably 17 to 50% by mass, and more preferably 20 to 39% by mass, based on the total amount of the thermally conductive sheet.
  • the thermally conductive sheet of the present invention contains 2.0 to 20 parts by mass of the alkyl silicone compound (B) based on a total of 100 parts by mass of the silicone matrix (A) and the alkyl silicone compound (B). If the content of the alkyl silicone compound (B) is less than 2.0 parts by mass, the thermally conductive sheet will tend to expand at high temperatures, increasing the load on the heating element and heat radiating element, and causing problems. Often. In addition, the rigidity of the thermally conductive sheet tends to be low at room temperature, and it tends to stretch when attached to a heat generating element and a heat radiating element, resulting in poor handling properties.
  • the alkyl silicone compound (B) may bleed out on the surface of the thermally conductive sheet, or it may be difficult to uniformly disperse the silicone matrix and the alkyl silicone compound (B). As a result, the two become separated and pump-out is likely to occur. Furthermore, the thermal resistance value of the thermally conductive sheet tends to vary. In addition, the thermally conductive sheet tends to become hard at room temperature, and when it is attached to a heat generating element and a heat radiating element, cracks and cracks are likely to occur, resulting in poor handling properties.
  • the content of the alkyl silicone compound (B) is preferably 2.5 parts by mass or more, and 4 parts by mass or more with respect to the total of 100 parts by mass of the silicone matrix (A) and the alkyl silicone compound (B). It is more preferably 8 parts by mass or more, further preferably 18 parts by mass or less, and more preferably 15 parts by mass or less.
  • the silicone matrix (A) is formed from a curable silicone composition (A1) described below. Therefore, in the mixed composition described below, the content of the alkyl silicone compound (B) is higher than the content of the alkyl silicone compound (B) based on the total of 100 parts by mass of the curable silicone composition (A1) and the alkyl silicone compound (B). ) is the same as the content of The contents of the thermally conductive filler (C), anisotropic filler, and non-anisotropic filler described later are also the same.
  • the binder component is preferably composed of a silicone matrix (A) and an alkyl silicone compound (B), but as long as it does not impede the effects of the present invention, a resin component other than the silicone matrix (A) or an alkyl silicone compound ( Plasticizers other than B) may be contained as binder components.
  • the alkyl silicone compound (B) used in the present invention may be a compound that is liquid at room temperature, or a compound that melts when heated to a certain temperature (for example, a temperature higher than 23 °C and lower than 80 °C).
  • a certain temperature for example, a temperature higher than 23 °C and lower than 80 °C.
  • the melting point of the alkyl silicone compound (B) is preferably 80°C or lower, more preferably 70°C or lower, still more preferably 60°C or lower, and even more preferably is below 50°C.
  • the alkyl silicone compound (B) is preferably solid at room temperature and under 1 atmosphere. Since it is solid at room temperature, it can be easily handled, and when the cutting process described below is performed at a temperature near room temperature, a thermally conductive sheet can be easily obtained by having a predetermined rigidity. Therefore, the melting point of the alkyl silicone compound is preferably higher than room temperature (23°C), more preferably 30°C or higher, and even more preferably 35°C or higher.
  • the melting point of the alkyl silicone compound (B) is preferably higher than 23°C and lower than 80°C, more preferably higher than 30°C and lower than 70°C, still more preferably higher than 35°C and lower than 60°C. More preferably, the temperature is 35°C or higher and 50°C or lower.
  • the melting point of the alkyl silicone compound is the temperature of the endothermic peak of the DTA curve measured using thermogravimetric differential thermal analysis (TGDTA) at a heating rate of 1° C./min. Furthermore, when the alkyl silicone compound is a mixture, the melting point is the maximum endothermic peak within the above temperature range.
  • the alkyl silicone compound (B) is not compatible with the silicone matrix (A), and that the binder component has a sea-island structure in which the silicone matrix (A) is the sea component and the alkyl silicone compound (B) is the island component. be done. Because the binder component has a sea-island structure, the alkyl silicone compound (B) continues to be retained by the silicone matrix (A) even if it softens, melts, or lowers its viscosity during heating, increasing flexibility while preventing pump-out. It can be suppressed. In addition, since the silicone matrix (A) constitutes the sea component, the thermally conductive sheet has a predetermined rebound resilience, so it can be assembled stably without forming an air layer between the heating element or the heat radiating element. be able to.
  • alkyl silicone compound examples include compounds having a polysiloxane skeleton in the main chain and an alkyl group.
  • the alkyl group is an alkyl group bonded to a silicon atom, and preferably contains an alkyl group having 8 or more carbon atoms.
  • an alkyl silicone compound represented by the following formula (1) is preferable.
  • R represents an alkyl group having 8 or more carbon atoms
  • m and n are integers such that m:n is in the range of 100:0 to 50:50.
  • m+n is an integer of 20 or more and 1000 or less.
  • the alkyl group having 8 or more carbon atoms may be a linear alkyl group or a branched alkyl group, but is preferably a linear alkyl group.
  • the number of carbon atoms in the alkyl group is preferably in the range of 8 to 26, more preferably in the range of 12 to 22 carbon atoms.
  • R is an alkyl group having 8 or more carbon atoms
  • the melting point of the alkyl silicone compound can be prevented from becoming too low.
  • R is an alkyl group having 26 or less carbon atoms
  • the range indicated by "-" means a range from the lower limit numerical value or more to the upper limit numerical value or less written before and after "-".
  • R is not particularly limited, but is preferably a dodecyl group, a tetradecyl group, a pentadecyl group, a hexadecyl group, a heptadecyl group, an octadecyl group, a nonadecyl group, an icosyl group, a henicyl group, a docosyl group, etc., and more preferably an octadecyl group. be.
  • the alkyl silicone compound has properties similar to so-called hard resins at temperatures below the melting point, and as m:n approaches 50:50, the properties become wax-like. .
  • the thermally conductive sheet becomes hard to a certain extent, making it easier to improve handleability.
  • alkyl silicone compound may be other than the compound represented by the above formula (1), and may be, for example, an alkyl silicone compound having a substituent other than an alkyl group.
  • the thermally conductive sheet of the present invention further includes a thermally conductive filler (C).
  • the thermally conductive filler (C) is preferably dispersed in and retained in the binder component, which is a mixture of the silicone matrix (A) and the alkyl silicone compound (B).
  • the thermally conductive filler preferably contains an anisotropic filler oriented in the thickness direction of the thermally conductive sheet. This makes it easier for the thermally conductive sheet to increase its thermal conductivity. Orientation in the thickness direction makes it difficult to increase the compressibility, but in the present invention, the compressibility in the thickness direction can be increased by dispersing the alkyl silicone compound (B) in the silicone matrix (A).
  • anisotropic filler when the anisotropic filler is oriented in the thickness direction, its long axis direction does not need to be strictly parallel to the thickness direction, and even if the long axis direction is slightly inclined to the thickness direction, It shall be oriented in the thickness direction.
  • an anisotropic filler whose long axis direction is tilted by less than 20 degrees is considered an anisotropic filler oriented in the thickness direction, and such an anisotropic filler has a large If it is a portion (for example, more than 60%, preferably more than 80% of the total number of anisotropic fillers), it shall be oriented in the thickness direction.
  • the content of the thermally conductive filler (C) is preferably 150 to 3000 parts by mass, more preferably 200 to 2000 parts by mass, based on a total of 100 parts by mass of the silicone matrix (A) and the alkyl silicone compound (B). , more preferably 300 to 1000 parts by mass.
  • the thermally conductive filler (C) is preferably 150 to 3000 parts by mass, more preferably 200 to 2000 parts by mass, based on a total of 100 parts by mass of the silicone matrix (A) and the alkyl silicone compound (B). , more preferably 300 to 1000 parts by mass.
  • the volume filling rate of the thermally conductive filler with respect to the total amount of the thermally conductive sheet is preferably 30 to 85% by volume, more preferably 50 to 83% by volume, and still more preferably 61 to 80% by volume. .
  • the volumetric filling rate is preferably 30 to 85% by volume, more preferably 50 to 83% by volume, and still more preferably 61 to 80% by volume.
  • Anisotropic fillers are fillers that have anisotropy in shape and can be oriented.
  • Examples of the anisotropic filler include fibrous materials and scaly materials.
  • the anisotropic filler has a high aspect ratio, specifically, an aspect ratio of more than 2, and preferably an aspect ratio of 5 or more. By making the aspect ratio larger than 2, it becomes easier to orient the anisotropic filler in one direction such as the thickness direction, and it becomes easier to increase the thermal conductivity of the thermally conductive sheet in one direction such as the thickness direction. Further, the upper limit of the aspect ratio is not particularly limited, but is practically 100.
  • the aspect ratio is the ratio of the length in the long axis direction to the length in the short axis direction of an anisotropic filler, and for fiber materials, it means fiber length/fiber diameter, and for scaly materials, means the length/thickness of the scaly material in the longitudinal direction.
  • the content of the anisotropic filler in the thermally conductive sheet is preferably 10 to 500 parts by mass, and 30 to 300 parts by mass based on the total of 100 parts by mass of the silicone matrix (A) and the alkyl silicone compound (B). parts by weight, and even more preferably from 50 to 250 parts by weight.
  • the content of the anisotropic filler is preferably 10 to 500 parts by mass, and 30 to 300 parts by mass based on the total of 100 parts by mass of the silicone matrix (A) and the alkyl silicone compound (B). parts by weight, and even more preferably from 50 to 250 parts by weight.
  • the average fiber length thereof is preferably 10 to 500 ⁇ m, more preferably 20 to 350 ⁇ m, and still more preferably 50 to 300 ⁇ m.
  • the average fiber length is 10 ⁇ m or more, the anisotropic fillers come into proper contact with each other inside the thermally conductive sheet, ensuring a heat transfer path and improving the thermal conductivity of the thermally conductive sheet.
  • the average fiber length is set to 500 ⁇ m or less, the bulk of the anisotropic filler becomes low and it becomes possible to fill the binder component with a high degree of filling.
  • the average fiber length of the fibrous material is shorter than the thickness of the thermally conductive sheet.
  • the above average fiber length can be calculated by observing the anisotropic filler with a microscope. More specifically, for example, the fiber length of 50 arbitrary anisotropic fillers can be measured using an electron microscope or an optical microscope, and the average value (arithmetic average value) can be taken as the average fiber length. can.
  • the average particle size thereof is preferably 10 to 400 ⁇ m, more preferably 15 to 300 ⁇ m, and even more preferably 20 to 200 ⁇ m.
  • the average particle size is preferably 10 ⁇ m or more, the anisotropic fillers in the thermally conductive sheet are likely to come into contact with each other, a heat transfer path is secured, and the thermal conductivity of the thermally conductive sheet is improved.
  • the average particle size is 400 ⁇ m or less, the bulk of the thermally conductive sheet becomes low, and it becomes possible to highly fill the anisotropic filler in the binder component.
  • the average particle size of the scaly material can be calculated by observing the anisotropic filler with a microscope and using the major axis as the diameter. More specifically, for example, using an electron microscope or an optical microscope, the long axis of 50 arbitrary anisotropic fillers can be measured, and the average value (arithmetic average value) can be taken as the average particle size. .
  • the anisotropic filler may be a known thermally conductive material, but if it is oriented by magnetic field orientation as will be described later, it may be diamagnetic. On the other hand, if the material is oriented by flow orientation or if no anisotropic filler is oriented, diamagnetic properties may not be provided.
  • Specific examples of anisotropic fillers include carbon fibers or carbon-based materials such as scaly carbon powder, metal materials such as metal fibers, metal oxides, boron nitride, metal nitrides, metal carbides, Examples include metal hydroxide, polyparaphenylene benzoxazole fiber, and the like.
  • carbon-based materials are preferred because they have a low specific gravity and good dispersibility in the binder component, and graphitized carbon materials with high thermal conductivity are particularly preferred.
  • the graphitized carbon material has diamagnetic properties because the graphite surfaces are aligned in a predetermined direction.
  • boron nitride is also preferable as the anisotropic filler. Although boron nitride is not particularly limited, it is preferably used as a scaly material.
  • the scale-like boron nitride may or may not be agglomerated, but it is preferable that some or all of it is not agglomerated. Note that boron nitride and the like also have diamagnetic properties because their crystal planes are aligned in a predetermined direction.
  • the anisotropic filler is not particularly limited, but has a thermal conductivity of generally 30 W/m ⁇ K or more, preferably 60 W/m ⁇ K, in the direction in which it has anisotropy (that is, the major axis direction). m ⁇ K or more, more preferably 100 W/m ⁇ K or more, still more preferably 200 W/m ⁇ K or more.
  • the upper limit of the thermal conductivity of the anisotropic filler is not particularly limited, but is, for example, 2000 W/m ⁇ K or less. Thermal conductivity can be measured by a laser flash method or the like.
  • anisotropic filler may be used alone, or two or more types may be used in combination.
  • anisotropic fillers having at least two different average particle sizes or average fiber lengths may be used as anisotropic fillers.
  • anisotropic fillers of different sizes small anisotropic fillers are inserted between relatively large anisotropic fillers, allowing the anisotropic fillers to be densely packed into the binder component. It is thought that it is possible to improve the heat conduction efficiency.
  • the carbon fiber used as the anisotropic filler is preferably graphitized carbon fiber.
  • flaky carbon powder flaky graphite powder is preferable.
  • the anisotropic filler it is also preferable to use graphitized carbon fiber and flaky graphite powder in combination.
  • Graphitized carbon fiber has graphite crystal planes that are continuous in the fiber axis direction, and has high thermal conductivity in the fiber axis direction. Therefore, by aligning the fiber axis direction in a predetermined direction, the thermal conductivity in a specific direction can be increased.
  • the flaky graphite powder has graphite crystal planes that are continuous in the in-plane direction of the scale surface, and has high thermal conductivity in that in-plane direction. Therefore, by aligning one side of the scales in a predetermined direction, the thermal conductivity in a specific direction can be increased.
  • the graphitized carbon fiber and flake graphite powder preferably have a high degree of graphitization.
  • graphitized carbon materials such as the graphitized carbon fibers and flaky graphite powder described above
  • those obtained by graphitizing the following raw materials can be used.
  • Examples include fused polycyclic hydrocarbon compounds such as naphthalene, PAN (polyacrylonitrile), fused heterocyclic compounds such as pitch, etc., but in particular graphitized mesophase pitch with a high degree of graphitization, polyimide, and polybenzazole should be used. is preferred.
  • mesophase pitch the pitch is oriented in the fiber axis direction due to its anisotropy in the spinning process described below, and graphitized carbon fibers having excellent thermal conductivity in the fiber axis direction can be obtained.
  • mesophase pitch is used in graphitized carbon fibers
  • mesophase pitch may be used alone or in combination with other raw materials.
  • mesophase pitch alone that is, graphitized carbon fiber with a mesophase pitch content of 100%, from the viewpoints of high thermal conductivity, spinnability, and quality stability.
  • Graphitized carbon fibers may be those that are sequentially subjected to spinning, infusibility, and carbonization, and that are graphitized after being crushed or cut to a predetermined particle size, or those that are graphitized after being carbonized, then crushed or cut, and then graphitized. can.
  • the condensation reaction and cyclization reaction proceed more easily during the graphitization process on the surface newly exposed by the pulverization, so the degree of graphitization is increased and heat conduction is further improved.
  • Graphitized carbon fibers with improved properties can be obtained.
  • the average fiber length of the graphitized carbon fiber is preferably 10 to 500 ⁇ m, more preferably 20 to 350 ⁇ m, and even more preferably 50 to 300 ⁇ m. Further, the aspect ratio of the graphitized carbon fiber is more than 2, preferably 5 or more, as described above.
  • the thermal conductivity of the graphitized carbon fiber is not particularly limited, but the thermal conductivity in the fiber axis direction is preferably 400 W/m ⁇ K or more, more preferably 800 W/m ⁇ K or more.
  • the anisotropic filler may or may not be exposed on the sheet surface, but is preferably exposed.
  • the sheet surface of the thermally conductive sheet can be made into a non-adhesive surface by exposing the anisotropic filler.
  • the thermally conductive sheet is the main surface of the sheet, and the anisotropic filler may be exposed on only one of both surfaces of the sheet, or the anisotropic filler may be exposed on both surfaces. May be exposed. Since the surface of the thermally conductive sheet is non-adhesive, it becomes possible to slide the sheet when it is assembled into electronic equipment, etc., thereby improving the ease of assembly.
  • the thermally conductive filler (C) in the present invention may contain a non-anisotropic filler, or the above-described anisotropic filler and non-anisotropic filler may be used together.
  • the non-anisotropic filler in combination with the anisotropic filler oriented in one direction, the non-anisotropic filler is interposed in the gap between the oriented anisotropic fillers, and the thermal conductivity can be further increased.
  • a non-anisotropic filler is a filler that does not substantially have anisotropy in shape, and can be used under an environment in which an anisotropic filler is oriented in a predetermined direction, such as under the generation of magnetic lines of force or under the action of shearing force, which will be described later. Also, it is a filler that is not oriented in its predetermined direction.
  • the aspect ratio of the non-anisotropic filler is 2 or less, preferably 1.5 or less.
  • a non-anisotropic filler having such a low aspect ratio is used in combination with an anisotropic filler, it is more likely to be placed in the gap between the anisotropic fillers, and the thermal conductivity can be improved. Further, by setting the aspect ratio to 2 or less, it is possible to prevent the viscosity of the mixed composition described below from increasing and to achieve high filling.
  • non-anisotropic filler examples include metals, metal oxides, metal nitrides, metal hydroxides, carbon materials, oxides other than metals, nitrides, and carbides. Further, the shape of the non-anisotropic filler may be spherical, irregularly shaped powder, or the like. Examples of non-anisotropic fillers include metals such as aluminum, copper, and nickel; examples of metal oxides include aluminum oxide such as alumina, magnesium oxide, and zinc oxide; examples of metal nitrides include aluminum nitride. can do. Examples of metal hydroxides include aluminum hydroxide. Further, examples of the carbon material include spherical graphite.
  • oxides, nitrides, and carbides other than metals include quartz, boron nitride, and silicon carbide.
  • aluminum oxide and aluminum are preferred because they have high thermal conductivity and are easily available in spherical shapes.
  • the non-anisotropic filler one type of the above-mentioned fillers may be used alone, or two or more types may be used in combination.
  • the average particle size of the non-anisotropic filler is, for example, 0.1 to 200 ⁇ m.
  • the average particle size of the non-anisotropic filler is preferably 0.1 to 50 ⁇ m, more preferably 0.5 to 35 ⁇ m, and 1 to 15 ⁇ m. It is more preferable that By setting the average particle size to 50 ⁇ m or less, even when used together with an anisotropic filler, problems such as disordering of the orientation of the anisotropic filler are less likely to occur.
  • the average particle size is set to 0.1 ⁇ m or more, the specific surface area of the non-anisotropic filler does not become larger than necessary, and even if a large amount is added, the viscosity of the mixed composition does not easily increase. It becomes easier to highly fill the oriented filler.
  • the non-anisotropic filler for example, non-anisotropic fillers having at least two mutually different average particle sizes may be used.
  • the average particle size of the non-anisotropic filler is preferably 0.1 to 200 ⁇ m, more preferably 0.5 to 100 ⁇ m, and even more preferably 1 to 70 ⁇ m.
  • the average particle size of the non-anisotropic filler can be measured by observing with an electron microscope or the like. More specifically, for example, using an electron microscope or an optical microscope, measure the particle size of 50 arbitrary non-anisotropic fillers, and use the average value (arithmetic average value) as the average particle size. I can do it.
  • the content of the non-anisotropic filler is preferably 50 to 2,500 parts by mass, and 100 to 1,500 parts by mass, based on a total of 100 parts by mass of the silicone matrix (A) and the alkyl silicone compound (B).
  • the amount is more preferably 200 to 750 parts by mass.
  • the thermal conductivity of the thermally conductive sheet can be improved.
  • the non-anisotropic filler is appropriately dispersed in the binder component, and the effect of increasing thermal conductivity depending on the content can be obtained. Further, it is also possible to prevent the viscosity of the mixed composition from increasing more than necessary.
  • the mass ratio of the content of the non-anisotropic filler to the content of the anisotropic filler is not particularly limited, but is preferably from 0.5 to 5, more preferably from 1 to 3. It is preferably 1.1 to 2.5. By setting the mass ratio within the above range, the non-anisotropic filler is appropriately filled between the anisotropic fillers and an efficient heat transfer path can be formed. Thermal conductivity of can be further improved.
  • the binder component may further contain various additives within a range that does not impair its function as a thermally conductive sheet.
  • the additive include at least one selected from dispersants, coupling agents, adhesives, flame retardants, antioxidants, colorants, antisettling agents, and the like.
  • a curing catalyst that accelerates curing may be added as an additive.
  • the curing catalyst include platinum-based catalysts.
  • a compatible substance (D) may be blended into the mixed composition. The compatible substance (D) volatilizes during the process of manufacturing the thermally conductive sheet and does not need to remain in the thermally conductive sheet, but at least a part of the blended compatible substance (D) remains. Good too.
  • the thermally conductive sheet of the present invention preferably has a compressibility of 15% or more at 40 psi.
  • the compression ratio of the thermally conductive sheet is 15% or more, it has high flexibility when heated, improves followability to a heat generating element or a heat radiating element during use, and has good thermal conductivity.
  • the compression ratio is preferably 18% or more, more preferably 20% or more, from the viewpoint of increasing flexibility during use and improving thermal conductivity. Further, the compression ratio is preferably 50% or less. When the compression ratio is 50% or less, handling properties and reliability are easily improved, assembly into electronic equipment and cutting processing are also facilitated, and pump-out and the like are less likely to occur. From these viewpoints, the compression ratio is more preferably 40% or less, and even more preferably 38% or less. Compressibility is measured by the method described in Examples.
  • the thickness of the thermally conductive sheet is not particularly limited, and may be set appropriately depending on the shape and use of the electronic device in which the thermally conductive sheet is mounted, and is, for example, in the range of 0.1 to 5 mm. Good. Further, from the viewpoint of ease of use in small electronic devices, etc., the thickness of the thermally conductive sheet is preferably 0.1 to 3 mm, more preferably 0.1 to 1 mm.
  • the thermally conductive sheet of the present invention can be manufactured, for example, by a manufacturing method comprising the following steps X and Y.
  • Step X Step of mixing at least the curable silicone composition (A1), the alkyl silicone compound (B), the thermally conductive filler (C), and the compatible substance (D) to obtain a mixed composition.
  • Step Y Step of curing the mixed composition obtained in Step X by heating. Each step will be described in detail below.
  • a mixed composition is obtained by mixing a compatible substance (D) in addition to the curable silicone composition (A1), the alkyl silicone compound (B), and the thermally conductive filler (C).
  • the compatible substance (D) is a substance that is compatible with or dissolves in the alkyl silicone compound (B) and the curable silicone composition (A1).
  • the alkyl silicone compound (B) has low compatibility with the curable silicone composition (A1), it can be uniformly mixed into the curable silicone composition (A1) by using the compatible substance (D). Therefore, the alkyl silicone compound (B) is evenly mixed in the silicone matrix (A) obtained by curing the curable silicone composition (A1).
  • compatible refers to when the compatible substance (D) and the alkyl silicone compound (B), or the compatible substance (D) and the curable silicone composition (A1) are mixed in the ratio actually used. A state in which two phases do not separate.
  • dissolution refers to the solid state when the compatible substance (D) and the alkyl silicone compound (B), or the compatible substance (D) and the curable silicone composition (A1) are mixed in the ratio actually used. The state in which there is no residue left on the surface.
  • step A mixed composition may be obtained by appropriately mixing the thermally conductive filler (C), the compatible substance (D), and other optionally added components in any order.
  • the curable silicone composition (A1) is composed of, for example, a main agent and a curing agent; in such a case, the main agent, a curing agent, an alkyl silicone compound (B), a thermally conductive filler (C),
  • a mixed composition may be obtained by mixing the compatible substance (D) and other components optionally added as necessary in any order.
  • the form of the mixed composition may be either a one-part type or a two-part type formed by combining the first agent and the second agent.
  • the two-component type is one in which a first agent and a second agent are mixed to obtain a mixed composition at the time of use. More specifically, the two-component mixed composition is one in which the first part contains an alkenyl group-containing organopolysiloxane (main ingredient), and the second part contains a hydrogen organopolysiloxane (curing agent). The second agent may further contain an alkenyl group-containing organopolysiloxane. Moreover, in one embodiment of a two-component mixed composition, a curing catalyst is contained in the first part. In this case, the alkyl silicone compound (B), the thermally conductive filler (C), and the compatible substance (D) may be contained in either the first part or the second part; Preferably, it is included.
  • the alkyl silicone compound (B) is preferably dissolved in the compatible substance (D) and then mixed with the curable silicone composition (A1) and other components.
  • the mixture of the alkyl silicone compound (B) and the compatible substance (D), the curable silicone composition (A1) (or the main ingredient and the curing agent), the thermally conductive filler (C), and if necessary A mixed composition may be obtained by mixing other optionally added components in any order.
  • the alkyl silicone compound (B) can be mixed more uniformly in the silicone matrix (A).
  • the heating temperature is preferably higher than the melting point of the compatible substance (D), and for example, the compatible substance (D) may be heated to 40° C. or higher to melt.
  • the upper limit of the heating temperature can be set to a temperature at which the thermally conductive silicone does not substantially harden during the mixing process when the base resin and the curing agent are mixed.
  • the temperature can be set at a temperature at which the compatible substances (D) are difficult to volatilize, for example, by heating to 80°C or lower to dissolve them. Good too.
  • the state in which the silicone matrix (A) and the alkyl silicone compound (B) are mixed is a transparent or slightly cloudy homogeneous mixture due to the presence of the compatible substance (D).
  • the compatible substance (D) is not included, the solid alkyl silicone compound is dispersed or the liquid alkyl silicone compound is separated into two layers.
  • the compatible substance (D) used in the present invention is preferably a substance that dissolves in the alkyl silicone compound (B) and is compatible with the curable silicone composition (A1).
  • the compatible substance (D) is preferably a substance that is liquid at room temperature (23° C.) and 1 atmosphere.
  • the compatible substance (D) is a component that volatilizes by heating at about 50 to 180° C. in Step Y, for example, as described later.
  • the content ratio of the thermally conductive filler (C) in the thermally conductive sheet can be increased.
  • the viscosity of the mixed composition is reduced by containing the compatible substance (D). Therefore, it becomes easier to increase the blending amount of the thermally conductive filler (C), and furthermore, it becomes easier to orient the anisotropic filler in a predetermined direction by magnetic field orientation, which will be described later.
  • the compatible substance (D) examples include alkoxysilane compounds, hydrocarbon solvents, and alkoxysiloxane compounds. These compounds have high solubility or compatibility with the alkyl silicone compound (B) and the curable silicone composition (A1). Dispersibility can be improved. Thereby, the alkyl silicone compound (B) is appropriately dispersed in the thermally conductive sheet as well, making it easier to ensure shape retention, reliability, flexibility at high temperatures, and the like.
  • the compatible substances (D) may be used alone or in combination of two or more.
  • the compatible substance (D) it is preferable to use an alkoxysilane compound.
  • an alkoxysilane compound By using an alkoxysilane compound, the surface of the thermally conductive sheet obtained by curing is free from bubbles and has a good appearance.
  • the alkoxysilane compound used as the compatible substance (D) one to three of the four bonds possessed by the silicon atom (Si) are bonded to an alkoxy group, and the remaining bonds are bonded to an organic substituent. It is a compound with a structure. By having an alkoxy group and an organic substituent, the alkoxysilane compound can improve the dispersibility of the alkyl silicone compound (B) in the curable silicone composition (A1).
  • alkoxy group contained in the alkoxysilane compound examples include methoxy group, ethoxy group, protoxy group, butoxy group, pentoxy group, and hexatoxy group.
  • the alkoxysilane compound may be contained in the curable silicone composition (A1) as a dimer.
  • alkoxysilane compounds having at least one of a methoxy group and an ethoxy group are preferred.
  • the number of alkoxy groups that the alkoxysilane compound has is preferably 2 or 3, and is 3 from the viewpoint of compatibility and solubility with the curable silicone composition (A1) and the alkyl silicone compound (B). It is more preferable.
  • the alkoxysilane compound is preferably at least one selected from trimethoxysilane compounds, triethoxysilane compounds, dimethoxysilane compounds, and diethoxysilane compounds.
  • Examples of the functional groups included in the organic substituent of the alkoxysilane compound include an acryloyl group, an alkyl group, a carboxyl group, a vinyl group, a methacrylic group, an aromatic group, an amino group, an isocyanate group, an isocyanurate group, an epoxy group, Examples include hydroxyl group and mercapto group.
  • a platinum catalyst as a curing catalyst for the curable silicone composition (A1), it is preferable to select and use an alkoxysilane compound that hardly affects the curing reaction of the organopolysiloxane.
  • the organic substituent of the alkoxysilane compound when using an addition reaction type organopolysiloxane using a platinum catalyst, the organic substituent of the alkoxysilane compound must not contain an amino group, an isocyanate group, an isocyanurate group, a hydroxyl group, or a mercapto group. is preferred.
  • the alkoxysilane compound is an alkylalkoxysilane compound having an alkyl group bonded to a silicon atom, that is, an alkyloxysilane compound having an alkyl group as an organic substituent.
  • it contains a silane compound. Therefore, dialkyldialkoxysilane compounds and alkyltrialkoxysilane compounds are preferable, and among them, alkyltrialkoxysilane compounds are preferable.
  • the number of carbon atoms in the alkyl group bonded to the silicon atom is preferably 1 to 16, for example.
  • the number of carbon atoms in the alkyl group is preferably 6 or more, and preferably 8 or more, from the viewpoint of improving the dispersibility of the alkylsilicone compound. More preferably, the number of carbon atoms is 12 or less, and more preferably 10 or less.
  • the number of carbon atoms in the alkyl group may be 1 or more; The following is preferable, 6 or less is more preferable, and 4 or less is still more preferable.
  • alkyl group-containing alkoxysilane compounds include methyltrimethoxysilane, dimethyldimethoxysilane, diethyldimethoxysilane, trimethylmethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, Di-n-propyldimethoxysilane, di-n-propyldiethoxysilane, isobutyltrimethoxysilane, isobutyltriethoxysilane, isobutyltrimethoxysilane, isobutyltriethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane , methylcyclohexyldimethoxysilane, methylcyclohexyldiethoxysilane, n-octyltri
  • alkyl group-containing alkoxysilane compounds from the viewpoint of improving the dispersibility of the alkyl silicone compound (B), n-decyltrimethoxysilane, dimethyldimethoxysilane, and n-octyltriethoxysilane are more preferable, and the alkyl silicone compound ( From the viewpoint of solubility with B), n-decyltrimethoxysilane and n-octyltriethoxysilane are even more preferred.
  • the alkoxysiloxane compound used as the compatible substance (D) has two or more siloxane bonds and has a structure in which an alkoxy group is bonded to at least one silicon atom.
  • the alkoxysiloxane compound has a structure in which an organic substituent is bonded to at least one silicon atom among the silicon atoms constituting the siloxane bond.
  • the alkoxysiloxane compound can improve the dispersibility of the alkyl silicone compound (B) by having an alkoxy group and an organic substituent.
  • alkoxy group and organic substituent that the alkoxysiloxane compound has include those exemplified in the explanation of the alkoxysilane compound above, and from the viewpoint of improving the dispersibility of the alkyl silicone compound (B), it is preferable to have at least an alkyl group. is preferred.
  • alkoxysiloxane compound examples include methylmethoxysiloxane oligomer, methylphenylmethoxysiloxane oligomer, methylepoxymethoxysiloxane oligomer, methylmercaptomethoxysiloxane oligomer, and methylacryloylmethoxysiloxane oligomer.
  • One type or two or more types of alkoxysiloxane compounds can be used.
  • hydrocarbon solvent used as the compatible substance (D) examples include aromatic hydrocarbon solvents.
  • aromatic hydrocarbon solvents are preferred from the viewpoint of compatibility with the curable silicone composition (A1).
  • aromatic hydrocarbon solvent include aromatic hydrocarbon solvents having about 6 to 10 carbon atoms, such as toluene, xylene, mesitylene, ethylbenzene, propylbenzene, butylbenzene, t-butylbenzene, etc. , preferably toluene, xylene, etc.
  • the content of the compatible substance (D) is preferably 6 to 60 parts by mass based on a total of 100 parts by mass of the curable silicone composition (A1) and the alkyl silicone compound (B).
  • the amount is 6 parts by mass or more, the uniformity of mixing the alkyl silicone compound (B) with the curable silicone composition (A1) can be sufficiently improved.
  • the content of the compatible substance (D) is more preferably 10 to 50 parts by mass, and even more preferably 15 to 45 parts by mass.
  • the alkyl silicone compound (B) is not mixed uniformly, the alkyl silicone compound remains undissolved, resulting in, for example, a solid alkyl silicone compound being dispersed.
  • Such dispersed solids may exhibit properties as a filler in the mixed composition. That is, the undissolved solids become part of the filler that increases the viscosity, and as a result, it may become difficult to increase the amount of the thermally conductive filler.
  • the content of the compatible substance (D) is preferably greater than the content of the alkyl silicone compound (B).
  • the compatible substance (D) may not be contained in the thermally conductive sheet, but may be contained in the thermally conductive sheet in an amount smaller than the content in the mixed composition. Further, when the thermally conductive sheet contains the compatible substance (D), it is preferable that 2 to 30% by mass of the compatible substance (D) blended into the mixed composition remains. .
  • the content of the compatible substance (D) in the thermally conductive sheet is 0.1 to 18 parts by mass based on the total of 100 parts by mass of the silicone matrix (A) and the alkyl silicone compound (B). The amount is preferably 0.3 to 15 parts by weight, more preferably 1 to 10 parts by weight. When the compatible substance (D) is within the above range, the flexibility of the thermally conductive sheet can be improved.
  • components other than the compatible substance (D) in the mixed composition i.e., curable silicone composition (A1), alkyl silicone compound (B), thermally conductive filler (C), other additives, etc.
  • curable silicone composition (A1), alkyl silicone compound (B), thermally conductive filler (C), other additives, etc. A detailed description of is given above.
  • the contents of the alkyl silicone compound (B) and the thermally conductive filler (C) in the mixed composition are also as described above.
  • the content of each component is based on the total of 100 parts by mass of the silicone matrix (A) and the alkyl silicone compound (B), but in the mixed composition, the curable silicone composition The amount is based on a total of 100 parts by mass of (A1) and the alkyl silicone compound (B).
  • Step Y is a step of curing the mixed composition by heating.
  • the temperature at which the mixed composition is heated is not particularly limited as long as the curable silicone composition (A1) can be cured by heating, and may be higher than room temperature (23°C), but preferably at a temperature of 50°C or higher. It is best to heat it.
  • the heating temperature is not particularly limited, but may be a temperature that does not cause thermal deterioration of the thermally conductive sheet and the mixed composition, and is, for example, 180°C or lower, preferably 150°C or lower.
  • the mixed composition may be heated in one step, or may be heated in two or more steps.
  • the heating is carried out in two or more stages, it is sufficient that the heating temperature is within the above range in at least one of the stages, but it is preferable that the heating temperature is within the above range in all stages. Further, the total heating time is, for example, about 10 minutes to 3 hours. Moreover, when carrying out in two or more stages, it is preferable to semi-cure the mixed composition in the first stage, and completely harden the mixed composition by heating in the second and subsequent stages.
  • the mixed composition is preferably formed into a predetermined shape such as a block shape or a sheet shape, and then heated and cured.
  • the mixed composition contains an anisotropic filler as the thermally conductive filler (C)
  • it is preferable that the anisotropic filler is oriented in one direction and then cured by heating.
  • the anisotropic filler can be oriented by a magnetic field orientation method or a flow orientation method, but it is preferably oriented by a magnetic field orientation method.
  • the mixed composition is injected into a mold or the like and then placed in a magnetic field to orient the anisotropic filler along the magnetic field. Then, it is preferable to obtain an oriented molded article by curing the curable silicone composition (A1). The mixed composition may be cured under the heating conditions described above.
  • the oriented molded product is preferably in the form of a block, but may be in the form of a sheet. By making it into a sheet, the oriented molded product can be used as a thermally conductive sheet as it is without slicing. On the other hand, by forming the filler into a block shape, the orientation of the anisotropic filler can be improved.
  • a release film may be placed inside the mold at a portion that comes into contact with the mixed composition.
  • the release film for example, a resin film with good releasability or a resin film whose one side has been subjected to release treatment with a release agent or the like is used.
  • a release film By using a release film, the oriented molded product can be easily released from the mold.
  • the viscosity of the mixed composition used in the magnetic field orientation method is preferably 10 to 300 Pa ⁇ s in order to achieve magnetic field orientation.
  • the thermally conductive filler (C) becomes difficult to settle.
  • the fluidity becomes good, the anisotropic filler is appropriately oriented by the magnetic field, and problems such as taking too much time for orientation do not occur.
  • the viscosity is the viscosity measured using a rotational viscometer (Brookfield Viscometer DV-E, spindle SC4-14) at 25° C. and a rotational speed of 10 rpm.
  • the viscosity of the mixed composition may be less than 10 Pa ⁇ s.
  • examples of the magnetic field line generation source for applying magnetic lines of force include superconducting magnets, permanent magnets, electromagnets, etc., but superconducting magnets are preferred because they can generate a magnetic field with high magnetic flux density.
  • the magnetic flux density of the magnetic field generated from these magnetic field line sources is preferably 1 to 30 Tesla. When the magnetic flux density is 1 Tesla or more, it becomes possible to easily orient the above-mentioned anisotropic filler made of carbon material or the like. Further, by setting the value to 30 Tesla or less, it becomes possible to manufacture it practically.
  • a shearing force is applied to the mixed composition to produce a primary sheet in which anisotropic fillers are oriented along the plane direction. More specifically, in the fluid orientation method, first, the mixed composition prepared in Step X is flattened and stretched while applying a shearing force to form a sheet (primary sheet). By applying a shearing force, the anisotropic filler can be oriented in the shearing direction.
  • a sheet forming means for example, the mixed composition is coated on the base film using a coating applicator such as a bar coater or a doctor blade, or by extrusion molding or discharge from a nozzle, and then the mixed composition is coated as necessary.
  • the thickness of the primary sheet is preferably about 50 to 5000 ⁇ m.
  • the anisotropic filler is oriented in one direction along the plane of the sheet.
  • the mixed composition used in the flow orientation method has a relatively high viscosity so that shearing forces are applied when it is stretched into a sheet. Specifically, the viscosity of the mixed composition is preferably 3 to 500 Pa ⁇ s.
  • the primary sheet may be used as it is as a thermally conductive sheet without being made into a block, as will be described later.
  • the primary sheets are adhered to each other using heat press, etc., while being cured by heating if necessary, to create a laminated block (block-shaped).
  • An oriented molded body) may also be formed.
  • the primary sheets when forming a laminated block, may be stacked after irradiating vacuum ultraviolet rays on at least one of the surfaces of the primary sheets to be stacked on each other. By overlapping the primary sheets with the surfaces irradiated with vacuum ultraviolet rays interposed therebetween, the primary sheets can be firmly adhered to each other.
  • the mixed composition when irradiating vacuum ultraviolet rays, may be completely cured when producing the primary sheet, and when the primary sheets are stacked to form a laminated block, it is cured by heating etc. There's no need. Even in the fluid orientation method, the mixed composition is preferably cured under the heating conditions described above.
  • the obtained oriented molded body is cut by slicing or the like perpendicular to the direction in which the anisotropic filler is oriented, and then formed into a sheet shape. It is good to use it as a body.
  • the slicing may be performed using, for example, a shear blade.
  • the tips of the anisotropic filler are exposed from the binder component on each cut surface.
  • the sheet-like molded product obtained by cutting may be used as a thermally conductive sheet as it is, or may be further subjected to other treatments.
  • each surface, which is a cut surface may be polished.
  • the surface may be polished using, for example, abrasive paper.
  • the thermally conductive sheet of the present invention is used inside electronic devices and the like. Specifically, the thermally conductive sheet is interposed between two members and used to conduct heat from one member to the other member. Specifically, the thermally conductive sheet is interposed between the heat generating element and the heat radiating element, conducts heat generated by the heat generating element to the heat radiating element, and radiates the heat from the heat radiating element.
  • the heating element include various electronic components such as a CPU, a power semiconductor, and a power supply used inside an electronic device.
  • Examples of the heat sink include a heat sink, a heat pump, and a metal casing of an electronic device.
  • the thermally conductive sheet is preferably used with both surfaces in close contact with the heating element and the heat radiating element, respectively, and compressed.
  • the thermally conductive sheet of the present invention comprises a binder component which is a mixture of a silicone matrix (A) and an alkyl silicone compound (B), and a thermally conductive filler (C) dispersed in the binder component.
  • the content of the alkyl silicone compound (B) is 2.0 to 20 parts by mass based on the total of 100 parts by mass of the silicone matrix (A) and the alkyl silicone compound (B), and the compressive load is 0.01 N.
  • the expansion coefficient X measured by a thermomechanical analyzer (TMA) at a measurement temperature of 30 to 80°C and a heating rate of 2°C/min is -2.0% or more and less than 0%.
  • the thermally conductive sheet of the present invention can be stably mounted between two members (between the first and second members) by a mounting method having the following steps 1 to 3.
  • Step 1 Placing the thermally conductive sheet on the surface of the first member
  • Step 2 Heating the thermally conductive sheet
  • Step 3 The opposite side of the thermally conductive sheet from the first member side
  • the first and second members are Although not particularly limited, it is preferable that one side is a heat generating body and the other side is a heat radiating body.
  • the detailed explanation of the heating element and the heat radiating element is as above.
  • Step 1 a thermally conductive sheet is placed on the surface of the first member.
  • the method of arranging the thermally conductive sheet is not particularly limited, but it is preferable to arrange the thermally conductive sheet so that one surface thereof is in contact with the first member. In this method, as described later, it is preferable to perform step 2 after step 1. In that case, the thermally conductive sheet is placed on the surface of the first member in a firm state before heating, so that the workability of step 1 is improved.
  • Step 2 the thermally conductive sheet is heated.
  • Step 2 may be performed after Step 1, before Step 1, or in parallel with Step 1, but Step 2 may be performed after Step 1 as described above. preferable. That is, in step 2, it is preferable to heat the thermally conductive sheet placed on the surface of the first member.
  • the thermally conductive sheet is preferably heated to a temperature equal to or higher than the melting point of the alkyl silicone compound (B). Therefore, the thermally conductive sheet is preferably heated to a temperature higher than room temperature (23°C), but the alkyl silicone compound (B) is reliably melted and the thermally conductive sheet is From the viewpoint of increasing flexibility, it is preferably heated to 50°C or higher, more preferably 60°C or higher, even more preferably 70°C or higher. In addition, from the viewpoint of preventing the thermally conductive sheet from being heated more than necessary, the thermally conductive sheet may be heated to 100°C or lower, preferably 90°C or lower, more preferably 85°C or lower. Good. In step 2, when the thermally conductive sheet is heated to a temperature higher than the melting point of the alkyl silicone compound (B), the first and second members are heated through the melted alkyl silicone compound (B) by applying pressure in step 3. can be easily fixed.
  • the heating method for the thermally conductive sheet is not particularly limited, and the thermally conductive sheet may be heated by a heating device such as an infrared heater, a hot air heater, or a heat transfer heater.
  • a heating device such as an infrared heater, a hot air heater, or a heat transfer heater.
  • the phase change sheet is generally softened or melted by the heating of a heating element constituting either the first or second member, but in this mounting method, the thermally conductive sheet is
  • the body is heated by a heating device separate from the body before being sandwiched between the first and second members. According to this aspect, it becomes possible to fix the thermally conductive sheet to the first and second members before using the electronic device. Therefore, it becomes possible to assemble the thermally conductive sheet by compressing it with a designed compression ratio.
  • Step 3 a second member is placed on the opposite side of the first member side of the thermally conductive sheet, and the thermally conductive sheet is pressurized to create a space between the first and second members. Assemble the thermally conductive sheet.
  • step 3 it is preferable to further dispose a second member on the thermally conductive sheet disposed on the surface of the first member, so that the thermally conductive sheet covers the surfaces of the first and second members. It becomes a state of being caught in between.
  • step 3 may be performed in parallel with step 2, it is preferably performed after step 2. Therefore, in step 3, it is preferable to further arrange the second member on the thermally conductive sheet that has been placed on the surface of the first member and has already been heated.
  • step 1, step 2, and step 3 it is more preferable to perform step 1, step 2, and step 3 in this order. Performing each step in this order improves workability.
  • the thermally conductive sheet sandwiched between the first and second members in step 3 has been heated in step 2, and therefore in step 3, in the heated state, it is further pressed in the thickness direction. It is good.
  • the pressurization may be performed, for example, by further pressing the thermally conductive sheet sandwiched between the first and second members in the thickness direction by the first and second members.
  • the heat conductive sheet is pressurized in step 3
  • the temperature becomes higher than the melting point of the alkyl silicone compound (B), and the alkyl silicone compound (B) is melted, so the molten alkyl silicone compound (B) ) is preferably used to fix the thermally conductive sheet to the first and second members.
  • the thermally conductive sheet of the present invention has a certain level of flexibility in a heated state, it can be made to follow the first and second members by applying pressure in step 3. Therefore, even if the first and second members have irregularities, the thermally conductive sheet can be brought into close contact with the first and second members to prevent the thermal resistance from increasing. Furthermore, the thermally conductive sheet can be assembled without applying high stress to the first and second members. Furthermore, the thermally conductive sheet retains its shape even when heated, so even when used in a compressed state, pump-out is suppressed and reliability is improved. Furthermore, since the thermally conductive sheet has a certain stiffness before heating, workability during assembly can be improved.
  • the present invention also provides a heat radiating member comprising the above-described thermally conductive sheet and a heat radiator, and in which the heat conductive sheet is attached to the surface of the heat radiator.
  • a heat radiating member can be obtained, for example, by arranging a heat conductive sheet on the surface of a heat radiator and fixing the heat conductive sheet to the surface of the heat radiator.
  • the thermally conductive sheet is preferably fixed to the surface of the heat sink by heating to a temperature equal to or higher than the melting point of the alkyl silicone compound (B) and applying pressure. At this time, the thermally conductive sheet may be placed on the surface of the heat radiator after being heated, or may be heated after being placed on the surface of the heat radiator.
  • the heat conductive sheet can be attached between the heat dissipating body and the heat generating body.
  • the mounting method is preferably carried out by a method comprising steps 2 and 3 described above, and since the details are as described above, they will be omitted.
  • thermally conductive sheets obtained in the present examples and comparative examples were evaluated by the following method.
  • the thermal resistance value was measured by the method shown below using a thermal resistance measuring device as shown in FIG. Specifically, for each sample, a test piece S having a size of 30 mm x 30 mm was prepared for this test. Each test piece S was attached to a copper block 22 with a measurement surface of 25.4 mm x 25.4 mm and whose side surfaces were covered with a heat insulating material 21, sandwiched between upper copper blocks 23, and a pressure of 20 psi ( A load of 0.138 MPa) was applied.
  • the lower copper block 22 is in contact with the heater 24.
  • the upper copper block 23 is covered with a heat insulating material 21 and connected to a heat sink 25 with a fan.
  • the thermally conductive sheet was cut into a size of 10 mm x 10 mm, and the compressibility was measured when compressed at 40 psi (0.276 MPa) in an 80° C. environment. Specifically, a test piece is sandwiched between a pedestal with a flat surface measuring 10 mm x 10 mm and a presser that presses in parallel, and the thickness T2 when the test piece is compressed at 0.276 MPa is measured. The compression ratio [100 ⁇ (T1-T2)/T1] with respect to the thickness T1 was calculated. In addition, the compressibility was measured in the same manner as above except that the pressure was changed to 20 psi.
  • the expansion coefficient X was measured as follows using a thermomechanical analyzer (TMA, "TMA-60” manufactured by Shimadzu Corporation). A thermally conductive sheet (size ⁇ 6 mm, thickness 0.3 mm) was compressed at room temperature (23° C.) with a compressive load of 0.01 N. The thickness of the thermally conductive sheet at this time was defined as the initial thickness (mm). Next, with the compressive load still applied, the temperature was raised from 30 °C to 80 °C at a temperature increase rate of 2 °C/min, and the expansion coefficient (%) at 30 °C and the expansion coefficient (%) at 80 °C were determined, respectively. The expansion coefficient X in the present invention was determined using the following formula.
  • Expansion rate X (%) Expansion rate (%) at 80°C - Expansion rate (%) at 30°C
  • the expansion coefficient at 30°C was determined as follows from the thickness (mm) of the thermally conductive sheet at 30°C and the initial thickness (mm).
  • the expansion coefficient at 80°C was determined from the thickness (mm) of the thermally conductive sheet at 80°C and the initial thickness (mm) as follows.
  • Expansion rate (%) at 30°C 100 x [(thickness at 30°C - initial thickness)/initial thickness]
  • Expansion rate (%) at 80°C 100 x [(thickness at 80°C - initial thickness)/initial thickness]
  • Adhesion force (tensile shear strength) was measured according to the tensile shear test of JIS K6850:1999.
  • a thermally conductive sheet (length 20 mm, width 20 mm, thickness 0.2 mm) produced by the method of each example and comparative example was placed between two aluminum sheets (length 30 mm, width 100 mm, thickness 0.012 mm). I got caught. At this time, the aluminum sheets were arranged so that their tips overlapped each other with a length of 25 mm x 25 mm. Then, a test sample was prepared by pressure bonding for 3 minutes at a temperature of 80° C. and a pressure of 20 psi.
  • Adhesion was evaluated as follows based on the measured adhesion force (Mpa). A: Adhesion force is 1.4 MPa or more B: Adhesion force is 1.0 MPa or more and less than 1.4 MPa C: Adhesion force is 0.4 MPa or more and less than 1.0 MPa D: Adhesion force is 0.3 MPa or more and less than 1.0 MPa. Less than 4MPaE: Adhesion force is less than 0.3MPa
  • C The thermally conductive sheet becomes too hard at room temperature (23° C.) and tends to crack when attached to each member (heat generating element, heat radiating element, etc.).
  • D The rigidity of the thermally conductive sheet is extremely low at room temperature (23° C.) and tends to stretch when attached to each member (heat generating element, heat radiating element, etc.).
  • E The thermally conductive sheet becomes too hard at room temperature (23° C.) and breaks when attached to each member (heat generating element, heat radiating element, etc.).
  • Example 1 Polyoctadecylmethylsiloxane (melting point (Tm): 50°C) as the alkyl silicone compound (B) and n-decyltrimethoxysilane as the compatible substance (D) were mixed at 23°C according to the blending amounts shown in Table 1.
  • a mixture was obtained in which the alkyl silicone compound (B) was dissolved in the compatible substance (D).
  • the obtained mixture a silicone base agent (alkenyl group-containing organopolysiloxane) as a curable silicone composition (A1), a silicone curing agent (hydrogen organopolysiloxane), and a catalyst (platinum-based catalyst) are uniformly mixed.
  • the thermally conductive filler (C) was mixed according to the amount shown in Table 1 to obtain a mixed composition.
  • the thermally conductive filler (C) includes aluminum powder (spherical, average particle size 3 ⁇ mm, aspect ratio 1 to 1.5, thermal conductivity 236 W/m ⁇ K) and aluminum oxide as non-anisotropic fillers.
  • a powder sintered, average particle size 0.5 ⁇ m, aspect ratio 1, thermal conductivity 32 W/m ⁇ K was used.
  • scale graphite powder (average particle size 40 ⁇ m, aspect ratio 10, thermal conductivity 550 W/m ⁇ K), graphitized carbon fiber 1 (average fiber length 77 ⁇ m, aspect ratio 8, thermal conductivity 1200 W) /m ⁇ K) and graphitized carbon fiber 2 (average fiber length 150 ⁇ m, aspect ratio 15, thermal conductivity 900 W/m ⁇ K) were used.
  • the volume filling rate of the thermally conductive filler (C) in each Example and Comparative Example was 66 volume %.
  • the melting point is the temperature at the endothermic peak of the DTA curve measured by thermogravimetric differential thermal analysis (TGDTA, "DTG-60" manufactured by Shimadzu Corporation) at a heating rate of 1° C./min.
  • the above mixed composition is injected into a mold whose thickness is set to be sufficiently larger than that of the thermally conductive sheet, and an 8T magnetic field is applied in the thickness direction to form an anisotropic filler in the thickness direction.
  • the curable silicone composition (A1) was cured by heating at 80° C. for 60 minutes to obtain a block-shaped oriented molded product.
  • the block-shaped oriented molded body is sliced into sheets using a shear blade to obtain a sheet-shaped molded body in which the anisotropic filler is exposed, and then heated at 150°C for 2 hours. Then, a sheet-like molded product was obtained.
  • Example 2 to 4 A thermally conductive sheet was obtained in the same manner as in Example 1, except that the amounts of each component were changed to those listed in Table 1. Each evaluation was performed on the obtained thermally conductive sheet. The results are shown in Table 1.
  • Example 1 was carried out in the same manner as in Example 1, except that a thermally conductive sheet was produced using a mixed composition obtained by mixing each component according to the formulation shown in Table 1 without using the alkyl silicone compound (B). Table 1 shows the evaluation results of the thermally conductive sheet obtained in Comparative Example 1.
  • the thermally conductive sheets of Examples 1 to 4 are thermally conductive sheets that satisfy the requirements of the present invention, are difficult to expand, have a rating of "C” or higher regarding the magnitude of the load due to expansion, and are It was also found that it was difficult to put a load on the heat sink.
  • the handling properties were also evaluated as "C” or higher, indicating that problems caused by the addition of the alkyl silicone compound were unlikely to occur. Furthermore, the thermal resistance value was low and the thermal conductivity was excellent.
  • the thermally conductive sheets obtained in each example were relatively rigid sheets at room temperature lower than the melting point of the alkyl silicone compound (B), so the thermally conductive sheets were obtained by slicing as described above. It was easy to handle.
  • the thermally conductive sheets of Comparative Examples 1 and 2 have a lower content of alkyl silicone compound than the amount stipulated in the present invention, and are therefore easy to expand, and the evaluation regarding the magnitude of the load due to expansion is D or E, and it was found that it is easy to put a load on the heating element, heat radiating element, etc. Furthermore, the thermal resistance value was high and the thermal conductivity was poor.
  • the content of the alkyl silicone compound (B) exceeded 20 parts by mass based on the total of 100 parts by mass of the silicone matrix (A) and the alkyl silicone compound (B). .
  • the thermally conductive sheet became too hard at room temperature (23° C.), causing cracks when attached to each member (heat generating element, heat radiating element, etc.), resulting in poor handling properties.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Organic Chemistry (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Polymers & Plastics (AREA)
  • Health & Medical Sciences (AREA)
  • Medicinal Chemistry (AREA)
  • Engineering & Computer Science (AREA)
  • Materials Engineering (AREA)
  • Manufacturing & Machinery (AREA)
  • Inorganic Chemistry (AREA)
  • Physics & Mathematics (AREA)
  • Combustion & Propulsion (AREA)
  • Thermal Sciences (AREA)
  • Wood Science & Technology (AREA)
  • Life Sciences & Earth Sciences (AREA)
  • Compositions Of Macromolecular Compounds (AREA)
  • Cooling Or The Like Of Semiconductors Or Solid State Devices (AREA)
  • Cooling Or The Like Of Electrical Apparatus (AREA)
  • Manufacture Of Macromolecular Shaped Articles (AREA)
  • Adhesive Tapes (AREA)
  • Adhesives Or Adhesive Processes (AREA)
PCT/JP2023/012649 2022-03-29 2023-03-28 熱伝導性シート、その装着方法及び製造方法 Ceased WO2023190585A1 (ja)

Priority Applications (6)

Application Number Priority Date Filing Date Title
CN202380022675.3A CN118715612A (zh) 2022-03-29 2023-03-28 导热性片、其组装方法和制造方法
EP23780594.0A EP4503119A4 (en) 2022-03-29 2023-03-28 THERMOCONDUCTIVE SHEET, ITS INSTALLATION METHOD AND ITS MANUFACTURING METHOD
JP2023562863A JP7424714B1 (ja) 2022-03-29 2023-03-28 熱伝導性シート、その装着方法及び製造方法
US18/840,172 US20250163299A1 (en) 2022-03-29 2023-03-28 Thermally-conductive sheet, method for installing same, and method for manufacturing same
KR1020247027819A KR20240168304A (ko) 2022-03-29 2023-03-28 열전도성 시트, 그 장착 방법 및 제조 방법
JP2024002618A JP2024032772A (ja) 2022-03-29 2024-01-11 熱伝導性シート、その装着方法及び製造方法

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2022-054381 2022-03-29
JP2022054381 2022-03-29

Publications (1)

Publication Number Publication Date
WO2023190585A1 true WO2023190585A1 (ja) 2023-10-05

Family

ID=88201806

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2023/012649 Ceased WO2023190585A1 (ja) 2022-03-29 2023-03-28 熱伝導性シート、その装着方法及び製造方法

Country Status (7)

Country Link
US (1) US20250163299A1 (cg-RX-API-DMAC7.html)
EP (1) EP4503119A4 (cg-RX-API-DMAC7.html)
JP (2) JP7424714B1 (cg-RX-API-DMAC7.html)
KR (1) KR20240168304A (cg-RX-API-DMAC7.html)
CN (1) CN118715612A (cg-RX-API-DMAC7.html)
TW (1) TW202348729A (cg-RX-API-DMAC7.html)
WO (1) WO2023190585A1 (cg-RX-API-DMAC7.html)

Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2000327917A (ja) * 1999-05-24 2000-11-28 Fuji Kobunshi Kogyo Kk 熱伝導性・電気絶縁性シリコーン組成物
JP2002234952A (ja) * 2001-02-08 2002-08-23 Fuji Kobunshi Kogyo Kk 熱軟化放熱シート及びこれを用いた放熱シート
JP2004331835A (ja) * 2003-05-08 2004-11-25 Fuji Polymer Industries Co Ltd 放熱シート
WO2022137762A1 (ja) * 2020-12-23 2022-06-30 積水ポリマテック株式会社 熱伝導性シート、その装着方法及び製造方法
WO2022163192A1 (ja) * 2021-01-29 2022-08-04 積水ポリマテック株式会社 熱伝導性シート、その装着方法及び製造方法

Family Cites Families (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2001291807A (ja) 2000-04-10 2001-10-19 Three M Innovative Properties Co 熱伝導性シート
US20040094293A1 (en) * 2001-04-23 2004-05-20 Kunihiko Mita Heat radiating member
US20050222323A1 (en) * 2002-04-11 2005-10-06 Xiao-Qi Zhou Thermally conductive coating compositions, methods of production and uses thereof
WO2006023860A2 (en) * 2004-08-23 2006-03-02 General Electric Company Thermally conductive composition and method for preparing the same
JP4993135B2 (ja) * 2008-07-08 2012-08-08 信越化学工業株式会社 熱伝導性シリコーン組成物

Patent Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2000327917A (ja) * 1999-05-24 2000-11-28 Fuji Kobunshi Kogyo Kk 熱伝導性・電気絶縁性シリコーン組成物
JP2002234952A (ja) * 2001-02-08 2002-08-23 Fuji Kobunshi Kogyo Kk 熱軟化放熱シート及びこれを用いた放熱シート
JP2004331835A (ja) * 2003-05-08 2004-11-25 Fuji Polymer Industries Co Ltd 放熱シート
WO2022137762A1 (ja) * 2020-12-23 2022-06-30 積水ポリマテック株式会社 熱伝導性シート、その装着方法及び製造方法
WO2022163192A1 (ja) * 2021-01-29 2022-08-04 積水ポリマテック株式会社 熱伝導性シート、その装着方法及び製造方法

Non-Patent Citations (1)

* Cited by examiner, † Cited by third party
Title
See also references of EP4503119A4 *

Also Published As

Publication number Publication date
KR20240168304A (ko) 2024-11-29
CN118715612A (zh) 2024-09-27
TW202348729A (zh) 2023-12-16
JPWO2023190585A1 (cg-RX-API-DMAC7.html) 2023-10-05
JP7424714B1 (ja) 2024-01-30
EP4503119A4 (en) 2026-04-01
JP2024032772A (ja) 2024-03-12
EP4503119A1 (en) 2025-02-05
US20250163299A1 (en) 2025-05-22

Similar Documents

Publication Publication Date Title
CN116075547B (zh) 导热性片、其安装方法及制造方法
KR101261064B1 (ko) 열 전도성 조성물 및 그의 제조 방법
JP6884456B1 (ja) 熱伝導性シート及びその製造方法
TWI807053B (zh) 熱傳導性片
TW202029430A (zh) 導熱性片
WO2022163192A1 (ja) 熱伝導性シート、その装着方法及び製造方法
WO2022210419A1 (ja) 熱伝導性シートの製造方法
JP7424714B1 (ja) 熱伝導性シート、その装着方法及び製造方法
JP2022121447A (ja) 熱伝導性シート、その装着方法及び製造方法
JP7424713B1 (ja) 熱伝導性シート
WO2024225391A1 (ja) 熱伝導性シート
TW202505717A (zh) 導熱性片及其製造方法
TW202502554A (zh) 導熱性片及其製造方法
WO2024204754A1 (ja) 熱伝導性シート及びその製造方法
WO2023080234A1 (ja) 熱伝導性シート
JP2025146817A (ja) 熱伝導性樹脂組成物

Legal Events

Date Code Title Description
WWE Wipo information: entry into national phase

Ref document number: 2023562863

Country of ref document: JP

121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 23780594

Country of ref document: EP

Kind code of ref document: A1

WWE Wipo information: entry into national phase

Ref document number: 202380022675.3

Country of ref document: CN

WWE Wipo information: entry into national phase

Ref document number: 18840172

Country of ref document: US

WWE Wipo information: entry into national phase

Ref document number: 2023780594

Country of ref document: EP

NENP Non-entry into the national phase

Ref country code: DE

ENP Entry into the national phase

Ref document number: 2023780594

Country of ref document: EP

Effective date: 20241029

WWP Wipo information: published in national office

Ref document number: 18840172