WO2023167287A1 - 還元剤およびガスの製造方法 - Google Patents

還元剤およびガスの製造方法 Download PDF

Info

Publication number
WO2023167287A1
WO2023167287A1 PCT/JP2023/007870 JP2023007870W WO2023167287A1 WO 2023167287 A1 WO2023167287 A1 WO 2023167287A1 JP 2023007870 W JP2023007870 W JP 2023007870W WO 2023167287 A1 WO2023167287 A1 WO 2023167287A1
Authority
WO
WIPO (PCT)
Prior art keywords
reducing agent
oxygen carrier
ratio
carbon dioxide
oxygen
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2023/007870
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
理沙 櫻井
昂嗣 滝沢
圭祐 飯島
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sekisui Chemical Co Ltd
Original Assignee
Sekisui Chemical Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sekisui Chemical Co Ltd filed Critical Sekisui Chemical Co Ltd
Priority to JP2024504752A priority Critical patent/JPWO2023167287A1/ja
Publication of WO2023167287A1 publication Critical patent/WO2023167287A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
    • B01J23/00—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00
    • B01J23/70—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00 of the iron group metals or copper
    • B01J23/76—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00 of the iron group metals or copper combined with metals, oxides or hydroxides provided for in groups B01J23/02 - B01J23/36
    • B01J23/83—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00 of the iron group metals or copper combined with metals, oxides or hydroxides provided for in groups B01J23/02 - B01J23/36 with rare earths or actinides
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01B—NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C
    • C01B32/00—Carbon; Compounds thereof
    • C01B32/40—Carbon monoxide
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01F—COMPOUNDS OF THE METALS BERYLLIUM, MAGNESIUM, ALUMINIUM, CALCIUM, STRONTIUM, BARIUM, RADIUM, THORIUM, OR OF THE RARE-EARTH METALS
    • C01F17/00—Compounds of rare earth metals
    • C01F17/20—Compounds containing only rare earth metals as the metal element
    • C01F17/206—Compounds containing only rare earth metals as the metal element oxide or hydroxide being the only anion
    • C01F17/224—Oxides or hydroxides of lanthanides
    • C01F17/235—Cerium oxides or hydroxides
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01F—COMPOUNDS OF THE METALS BERYLLIUM, MAGNESIUM, ALUMINIUM, CALCIUM, STRONTIUM, BARIUM, RADIUM, THORIUM, OR OF THE RARE-EARTH METALS
    • C01F17/00—Compounds of rare earth metals
    • C01F17/30—Compounds containing rare earth metals and at least one element other than a rare earth metal, oxygen or hydrogen, e.g. La4S3Br6
    • C01F17/32—Compounds containing rare earth metals and at least one element other than a rare earth metal, oxygen or hydrogen, e.g. La4S3Br6 oxide or hydroxide being the only anion, e.g. NaCeO2 or MgxCayEuO
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01G—COMPOUNDS CONTAINING METALS NOT COVERED BY SUBCLASSES C01D OR C01F
    • C01G49/00—Compounds of iron

Definitions

  • the present invention relates to a reducing agent and a method for producing a gas, and more particularly to a reducing agent that can be used in chemical looping, and a method for producing a gas using such a reducing agent.
  • a chemical looping method is used to convert (synthesize) carbon monoxide from carbon dioxide.
  • the chemical looping method referred to here divides the reverse water gas shift reaction into two reactions, a reduction reaction with hydrogen and a reaction of producing carbon monoxide from carbon dioxide, and divides these reactions into oxygen carrier (for example, It is a method of bridging with a metal oxide: MO x ) (see the formula below).
  • MO x-1 represents a state in which part or all of the metal oxide has been reduced.
  • a reducing agent that reduces carbon dioxide upon contact to produce a carbon value.
  • This reducing agent contains cerium (Ce) and iron (Fe) and contains an oxygen carrier with oxygen ion conductivity.
  • the ratio of the chroma a * to the lightness L* of the oxygen carrier (a * /L * -oxygen carrier ) obtained by the colorimetric test satisfies the relationship of 0.01 or more.
  • the reducing agent of the present invention is used in producing a product gas containing carbon monoxide (carbon value) by reducing carbon dioxide by contacting a raw material gas containing carbon dioxide with the reducing agent (i.e. , used in the gas production method of the present invention). Also, the reducing agent oxidized by contact with carbon dioxide can be reduced (regenerated) by contact with a reducing gas containing hydrogen (reducing substance).
  • a raw material gas and a reducing gas are alternately passed through a reaction tube (reaction vessel) filled with the reducing agent of the present invention, thereby converting carbon dioxide into carbon monoxide by the reducing agent, Regeneration of the reducing agent in an oxidized state by the reducing gas is performed.
  • the reducing agent of the present invention contains an oxygen carrier with oxygen ion conductivity.
  • the oxygen carrier is a compound that can cause reversible oxygen deficiency, and the oxygen element itself is deficient due to reduction. It refers to a compound that shows the action of depriving carbon dioxide of oxygen element and reducing it.
  • the oxygen carrier in the present invention is a compound containing cerium (Ce) and iron (Fe), preferably a metal oxide. In such an oxygen carrier, the synergistic effect of Ce and Fe promotes the production of carbon monoxide from carbon dioxide.
  • the ratio of the chroma a * to the lightness L * of the oxygen carrier (a * /L * -oxygen carrier ) obtained by the colorimetric test satisfies the relationship of 0.01 or more.
  • the timing of the colorimetry test is before the reducing agent is used for reaction with gas, that is, immediately after the reducing agent is produced.
  • the form of the colorimetric object to be subjected to the colorimetric test may be powder, or may be a molded body obtained by granulating powder. In the case of powder, the smaller the gaps between the particles and the irregularities on the surface of the particles, the higher the colorimetric accuracy, which is preferable.
  • the molded body can be produced by, for example, tableting, tumbling granulation, extrusion molding, or the like.
  • the size of the molded body is set according to the size of the field of view of the colorimetry unit of the colorimetry device. For example, when the colorimetric visual field is 6 mm ⁇ , the size of the molded body is set to 10 mm ⁇ or more.
  • CIE L * a * b * (CIELAB) is a color space formulated by the International Commission on Illumination (CIE).
  • CIE International Commission on Illumination
  • the colorimetric test can be performed according to JIS Z 8722:2009.
  • the ratio (a * /L * ) obtained by performing a colorimetric test on the reducing agent is directly used as the ratio (a * /L * -oxygen carrier ).
  • the above ratio (a * /L * -oxygen carrier ) is the ratio of the reducing agent and the binder obtained by a colorimetric test. It can be calculated by the following formula (1) based on the ratio (a * /L * -reducing agent ) and the ratio (a * /L * -binder ) of chroma a * to lightness L * of each preferable.
  • Ratio (a * /L * -oxygen carrier ) [ratio (a * /L * -reducing agent )-ratio (a * /L * -binder ) x ratio of binder to reducing agent]/oxygen to reducing agent Percentage of careers (1)
  • the oxygen carrier ratio (a * /L * -oxygen carrier ) can be measured relatively easily and accurately. It is preferable to set the same colorimetric test conditions for the reducing agent and the binder.
  • L * takes a relatively small value and a * takes a positive value.
  • Fe exists as an Fe 2 O 3 phase when it cannot completely dissolve inside the crystal of the oxygen carrier (cerium oxide) (that is, when it is in a non-dissolution state).
  • the reducing agent as a whole has a lower L * than when it does not contain the Fe 2 O 3 phase.
  • the present inventors' studies have revealed that the value of a* is small and a * tends to take a positive value.
  • the ratio (a * /L * -oxygen carrier ) is 0.01 or more, it can be determined that Fe is sufficiently dissolved inside the crystal of the oxygen carrier (cerium oxide). Therefore, interaction between Ce and Fe becomes easier in the oxygen carrier, and the conversion efficiency from carbon dioxide to carbon monoxide can be improved.
  • the above ratio (a * /L * -oxygen carrier ) may be 0.01 or more, but is preferably 0.1 or more and 1.2 or less, and satisfies the relationship of 0.35 or more and 1 or less. is more preferable, more preferably 0.45 or more and 1 or less, and particularly preferably 0.45 or more and 0.7 or less. If the above ratio (a * /L * -oxygen carrier ) satisfies such a relationship, Fe is necessary and sufficiently solid-soluted inside the crystal of the oxygen carrier, and the interaction between Ce and Fe is enhanced. it is conceivable that. As a result, the synergistic effect of Ce and Fe further promotes the production of carbon monoxide from carbon dioxide.
  • the lightness L * of the reducing agent obtained by the colorimetric test is more preferably 10 or more and 90 or less, more preferably 10 or more and 70 or less, and even more preferably 20 or more and 50 or less. 30 or more and 45 or less is particularly preferable. It is considered that a reducing agent having a lightness L * not too low prevents the generation or increase of the Fe 2 O 3 phase (non-dissolved phase) in the oxygen carrier (reducing agent). Therefore, destabilization of the reducing agent due to sintering of the non-dissolved phase is preferably suppressed.
  • the oxygen carrier further comprises a transition element other than cerium (Ce) and iron (Fe). Including the additional transition element in the oxygen carrier allows the oxygen element to move in and out of the oxygen carrier more smoothly.
  • the ratio (molar ratio) of the molar amount of cerium to the total molar amount of the metal elements contained in the oxygen carrier is not particularly limited, but is preferably 0.6 or more, more preferably 0.65 or more. More preferably, it is 0.7 or more. In addition, the upper limit of the molar ratio is usually 0.98 or less.
  • the ratio (molar ratio) of the molar amount of cerium and iron to the total molar amount of the metal elements contained in the oxygen carrier is not particularly limited, but is preferably 0.8 or more, and is 0.85 or more. is more preferable, and 0.9 or more is even more preferable.
  • the upper limit of the molar ratio is usually 0.98 or less.
  • the transition element is at least one element belonging to the 4th and 5th periods of the periodic table.
  • Such elements have ionic radii relatively close to those of Ce and Fe, and thus can prevent or suppress the instability of oxygen carrier crystals due to the difference in ionic radii.
  • Specific examples of transition elements include scandium (Sc), chromium (Cr), manganese (Mn), nickel (Ni), copper (Cu), zirconium (Zr), and niobium (Nb). These transition elements can be used singly or in combination of two or more.
  • the transition element is preferably Mn and/or Zr, more preferably Zr.
  • the reducing agent of the present invention may be composed of an oxygen carrier alone, or may be composed of an oxygen carrier and a binder that binds the oxygen carrier together.
  • the latter embodiment includes an embodiment in which oxygen carrier fine particles are bound with a binder (carrier).
  • the shape retention of the reducing agent can be further enhanced, and the specific surface area of the reducing agent can be easily adjusted.
  • the ratio of the binder to 100 parts by mass of the reducing agent is preferably 90 parts by mass or less, more preferably 80 parts by mass or less, and 70 parts by mass or less. It is more preferable that the content is 50 parts by mass or less.
  • the ratio of the binder contained in the reducing agent can be measured by ICP mass spectrometry or the like.
  • a reducing agent containing such a binder can be produced by mixing the oxygen carrier and the binder using, for example, a mortar or a mixer/kneader.
  • the binder may be solid (powder) or liquid (sol). In the latter case, it becomes solid by firing as described later.
  • alumina sol is used as the binder and becomes solid alumina after firing.
  • the reducing agent can be produced by extruding a paste obtained by kneading an oxygen carrier and a binder through a die.
  • the reducing agent is obtained by mixing an oxygen carrier and a binder with a mixer and then granulating while spraying a spray liquid (water), or by spraying an oxygen carrier containing a binder. It can be produced by granulating while spraying a liquid (water + binder).
  • the reducing agent can be produced by mixing an oxygen carrier and a binder in a mixer and then tableting.
  • the oxygen carrier can be produced using a sol-gel method, a coprecipitation method, a solid-phase method, a hydrothermal synthesis method, or the like, which will be described later.
  • the strength can be improved by firing the granules obtained by granulation.
  • the granules are fired at a temperature of preferably 300° C. or higher and 1200° C. or lower, more preferably 700° C. or higher and 1000° C. or lower, for preferably 1 hour or more and 24 hours or less, more preferably 1.5 hours or more and 20 hours or less. It is recommended to do this at the time of Excessive particle growth of the reducing agent can also be prevented by firing under the above firing conditions.
  • the temperature should be raised at a rate of 1° C./min or more and 20° C./min or less, preferably 2° C./min or more and 10° C./min or less until the firing temperature is reached.
  • the growth of the reducing agent particles can be promoted, and cracking of the crystals (particles) can be avoided.
  • the binder is not particularly limited as long as it is a compound that is difficult to denature depending on contact with the raw material gas, reaction conditions, etc., but for example, inorganic materials such as oxides, nitrides, oxynitrides, and carbides, Examples include carbon materials (graphite, graphene, etc.).
  • the binder is preferably an oxide, and an oxide containing at least one of magnesium (Mg), titanium (Ti), zirconium (Zr), aluminum (Al) and silicon (Si). more preferably aluminum oxide. These oxides are preferable because they are highly stable against heat and tend to stably bind oxygen carrier fine particles.
  • the packing density of the reducing agent is preferably 4 g/mL or less, more preferably 0.5 g/mL or more and 3 g/mL or less, and even more preferably 1 g/mL or more and 2.5 g/mL or less. . If the packing density is too low, the gas passing speed becomes too fast, and the contact time between the reducing agent and the raw material gas and the reducing gas is shortened. As a result, the efficiency of conversion of carbon dioxide to carbon monoxide by the reducing agent and the efficiency of regeneration of the reducing agent in the oxidized state by the reducing gas tend to decrease. On the other hand, if the packing density is too high, the gas passing speed becomes too slow, making it difficult for the reaction to proceed or requiring a long time to produce the product gas.
  • the pore volume of the reducing agent is preferably 0.1 cm 3 /g or more, more preferably 1 cm 3 /g or more and 30 cm 3 /g or less, and 5 cm 3 /g or more and 20 cm 3 /g or less. is more preferred. If the pore volume is too small, it becomes difficult for the raw material gas and the reducing gas to enter the inside of the reducing agent. As a result, the contact area between the reducing agent and the raw material gas and the reducing gas is reduced, and the efficiency of conversion of carbon dioxide to carbon monoxide by the reducing agent and the efficiency of regeneration of the reducing agent in the oxidized state by the reducing gas tend to decrease. On the other hand, even if the pore volume exceeds the upper limit, no further increase in the effect can be expected, and the mechanical strength tends to decrease depending on the type of reducing agent.
  • the shape of the reducing agent is not particularly limited, it is preferably granular, for example. If it is granular, it is easy to adjust the filling density of the reducing agent to the above range.
  • "granular" is a concept including powdery, particulate, lumpy, pellet-like, etc., and its shape may be any of spherical, plate-like, polygonal, crushed, columnar, needle-like, scale-like, etc. .
  • the average particle size of the reducing agent is preferably 1 ⁇ m or more and 5 mm or less, more preferably 10 ⁇ m or more and 1 mm or less, and even more preferably 20 ⁇ m or more and 0.5 mm or less. With a reducing agent having such an average particle size, it is easy to adjust the packing density within the above range.
  • the average particle size means the average value of the particle sizes of arbitrary 200 reducing agents in one field observed with an electron microscope.
  • the "particle size” means the maximum length among the distances between two points on the contour line of the reducing agent.
  • the maximum length of the distance between two points on the contour line of the end face is defined as the "particle diameter”.
  • the average particle size is, for example, in the form of lumps, and means the average particle size of the secondary particles when the primary particles are agglomerated.
  • the BET specific surface area of the reducing agent is preferably 1 m 2 /g or more and 500 m 2 /g or less, more preferably 3 m 2 /g or more and 450 m 2 /g or less, and 5 m 2 /g or more and 400 m 2 /g. More preferably: When the BET specific surface area is within the above range, it becomes easier to improve the conversion efficiency of carbon dioxide to carbon monoxide by the reducing agent.
  • the oxygen capacity of the reducing agent is increased in a wide range from low temperature (about 400 ° C.) to high temperature (about 850 ° C.). state can be maintained. That is, the reducing agent of the present invention can efficiently convert carbon dioxide to carbon monoxide over a wide temperature range, and can be efficiently reduced by a hydrogen-containing reducing gas.
  • the oxygen capacity of the reducing agent at 400° C. is preferably 0.5 to 40% by mass, more preferably 1.5 to 30% by mass. If the oxygen capacity of the reducing agent at low temperatures is within the above range, it means that the oxygen capacity is sufficiently high even at temperatures (650 ° C. or higher) during actual operation, and the conversion efficiency of carbon dioxide to carbon monoxide is high. It can be said that it is an extremely high reducing agent.
  • the method for producing the reducing agent is not particularly limited, and examples thereof include a sol-gel method, a coprecipitation method, a solid phase method, a hydrothermal synthesis method and the like.
  • the reducing agent can be produced as follows. First, an aqueous solution is prepared by dissolving a salt of a metal element that constitutes a reducing agent (when using the inorganic binder, the salt of the element that constitutes the inorganic binder may be included) in water. Then, after gelling the aqueous solution, it is dried and baked.
  • the reducing agent of the present invention can be easily and reliably produced by the so-called sol-gel method.
  • acidic water adjusted to be acidic with citric acid, acetic acid, malic acid, tartaric acid, hydrochloric acid, nitric acid, or a mixture thereof may be used.
  • salts of metal elements include nitrates, sulfates, chlorides, hydroxides, carbonates, and composites thereof. Of these, nitrates are preferred. Moreover, you may use a hydrate for the salt of a metal element as needed.
  • the gel is dried at a temperature of preferably 20° C. to 200° C., more preferably 50° C. to 150° C., preferably 0.5 hours to 20 hours, more preferably 1 hour to 15 hours. do it. By drying in this manner, the gel can be dried uniformly.
  • the gel is baked at a temperature of preferably 300° C. or higher and 1200° C. or lower, more preferably 700° C. or higher and 1000° C. or lower, for preferably 1 hour or more and 24 hours or less, more preferably 1.5 hours or more and 20 hours or less.
  • the gel preferably becomes an oxide upon calcination, but can be easily converted to a reducing agent by calcination under the above calcination conditions. Further, if the firing is performed under the above firing conditions, excessive particle growth of the reducing agent can be prevented.
  • the temperature should be raised at a rate of 1° C./min to 20° C./min, preferably at a rate of 2° C./min to 10° C./min until the firing temperature is reached. As a result, the growth of the reducing agent particles can be promoted, and cracking of the crystals (particles) can be avoided.
  • the reducing agent of the present invention can be used, for example, in the chemical looping method, as described above.
  • the reducing agent of the present invention can be used for the application of reducing carbon dioxide by contact to produce carbon monoxide (carbon valuables). More specifically, a reduction reaction of carbon dioxide and a reduction reaction of a reducing agent are preferably performed, and the reducing agent is used so as to circulate between the reduction reaction of carbon dioxide and the reduction reaction of the reducing agent. is preferred.
  • a reducing gas containing other reducing substances is used in the reduction reaction of the reducing agent.
  • the reducing agent of the present invention is preferably used for so-called reverse water gas shift reaction.
  • the reverse water gas shift reaction is a reaction that produces carbon monoxide and water from carbon dioxide and hydrogen.
  • the reverse water gas shift reaction is divided into a reducing reaction of the reducing agent (first process) and a reducing reaction of carbon dioxide (second process).
  • the reaction is represented by the formula (A)
  • the reduction reaction of carbon dioxide is represented by the following formula (B).
  • x is usually 2. That is, in the reduction reaction of the reducing agent, hydrogen, which is one type of reducing substance, is oxidized to produce water. In addition, in the reduction reaction of carbon dioxide, carbon monoxide, which is a type of carbon valuables, is produced by reducing carbon dioxide.
  • the reaction temperature in the reduction reaction of the reducing agent may be any temperature at which the reduction reaction can proceed.
  • the lower limit of the reaction temperature is 300°C or higher, 350°C or higher, 400°C or higher, 450°C or higher, 500°C or higher, 550°C or higher, 600°C or higher, 650°C or higher, 700°C or higher, 750°C or higher, 800°C or higher. can be Within this temperature range, the reduction reaction of the reducing agent can proceed efficiently.
  • the upper limit of the reaction temperature can be 1050° C. or less, 1000° C. or less, 950° C. or less, 900° C. or less, or 850° C. or less. By setting the upper limit of the reaction temperature within the above range, economic efficiency can be improved.
  • the lower limit and the upper limit can be arbitrarily combined to define the range of the reaction temperature.
  • the amount of hydrogen (reducing gas) brought into contact with the reducing agent in an oxidized state is preferably 1 mmol or more and 50 mmol or less, more preferably 2.5 mmol or more and 35 mmol or less, with respect to 1 g of the reducing agent. more preferably 5 mmol or more and 20 mmol or less.
  • the reducing agent of the present invention has a high hydrogen utilization rate because the oxygen element enters and exits smoothly. Therefore, the reducing agent of the present invention is sufficiently reduced (regenerated) with a small amount of hydrogen. Therefore, it contributes to the reduction of the energy required for hydrogen production, and thus the reduction of carbon dioxide generated when the energy is obtained.
  • the hydrogen utilization rate (%) is the ratio of the amount (number of moles) of generated carbon monoxide to the amount (number of moles) of hydrogen brought into contact with 1 g of the reducing agent, expressed as a percentage.
  • a reversible amount of oxygen deficiency is generated in the reducing agent at a predetermined rate.
  • This specific ratio is preferably 1.6% or more, more preferably 2% or more, and further preferably 2.5% or more with respect to the mass of the oxygen carrier contained in the reducing agent. preferable.
  • the conversion of carbon dioxide to carbon monoxide can be further promoted by creating oxygen defects at such a rate.
  • the upper limit of the oxygen deficiency amount is not particularly limited, it is usually about 10%.
  • the amount of oxygen deficiency can be determined by the method described in Examples below.
  • the reaction temperature in the reduction reaction of carbon dioxide may be a temperature at which the reduction reaction can proceed.
  • the lower limit of the reaction temperature is 300°C or higher, 350°C or higher, 400°C or higher, 450°C or higher, 500°C or higher, 550°C or higher, 600°C or higher, 650°C or higher, 700°C or higher, 750°C or higher, 800°C or higher.
  • the upper limit of the reaction temperature can be 1050° C. or less, 1000° C. or less, 950° C. or less, 900° C. or less, or 850° C. or less.
  • the reducing agent can reduce carbon dioxide to carbon monoxide with high efficiency even at low temperatures
  • the reduction reaction of carbon dioxide can be set to a relatively low temperature.
  • the upper limit of the reaction temperature within the above range, it is possible not only to facilitate utilization of waste heat, but also to further improve economic efficiency.
  • the lower limit and the upper limit can be arbitrarily combined to define the range of the reaction temperature.
  • the amount of carbon dioxide brought into contact with the reducing agent is preferably 1 mmol or more and 50 mmol or less, more preferably 2.5 mmol or more and 30 mmol or less, relative to 1 g of the reducing agent. More preferably, it is 5 mmol or more and 20 mmol or less.
  • the reducing agent of the present invention facilitates entry and exit of oxygen element. Therefore, the reducing agent of the present invention has a high conversion efficiency of carbon dioxide to carbon monoxide (that is, a large amount of carbon monoxide is produced), and from this point of view also contributes to the reduction of carbon dioxide.
  • the reducing agent can be regenerated with a small amount of hydrogen.
  • the amount of carbon monoxide produced in the reducing agent of the present invention is preferably about 0.3 mmol or more and 1 mmol or less per 1 g of the reducing agent.
  • the reduced product (carbon valuables) obtained by the reduction reaction of carbon dioxide contains carbon monoxide, but may contain substances other than carbon monoxide, and carbon monoxide and other substances It may be a mixture with Specific examples of other substances include, for example, methane. It is preferable that the reduced product such as carbon monoxide obtained by the carbon dioxide reduction reaction is further converted into an organic substance or the like by microbial fermentation or the like. Microbial fermentation includes anaerobic fermentation. Organic substances obtained include methanol, ethanol, acetic acid, butanol, derivatives thereof, mixtures thereof, and C5 or higher compounds such as isoprene.
  • the reduced products such as carbon monoxide may be converted into C1 to C20 compounds including hydrocarbons and alcohols conventionally synthesized by petrochemicals by metal oxides.
  • Specific compounds obtained include methane, ethane, propylene, methanol, ethanol, propanol, acetaldehyde, diethyl ether, acetic acid, butyric acid, diethyl carbonate, butadiene, and the like.
  • the reducing agent of the present invention preferably has the following properties. That is, when a reducing agent is filled at a height of 40 cm in a stainless steel reaction tube with an inner diameter of 8 mm and a pressure gauge is arranged in the flow channel, and nitrogen gas with a concentration of 100% by volume is passed at 30 mL / min, The pressure rise in 10 minutes is preferably 0.03 MPaG or less, more preferably 0.01 MPaG or less. A reducing agent exhibiting such characteristics can be judged to satisfy the above ranges in packing density and pore volume, and can sufficiently increase the conversion efficiency of carbon dioxide to carbon monoxide.
  • a reducing agent with high conversion efficiency of carbon dioxide to carbon monoxide is determined by a simple analytical method called a colorimetric test, and a reducing agent with such high characteristics and this reducing agent are used.
  • a method for producing gas can be provided.
  • a reducing agent that reduces carbon dioxide by contact to produce a carbon value contains cerium (Ce) and iron (Fe), contains an oxygen carrier with oxygen ion conductivity, and performs a colorimetric test
  • the reducing agent according to (1) above further contains a binder that binds the oxygen carrier, and the ratio (a * /L * -oxygen carrier ) is obtained by the colorimetric test.
  • transition element is at least one of elements belonging to the 4th period and the 5th period of the periodic table.
  • the reducing agent oxidized by contact with carbon dioxide is reduced by contact with a reducing gas containing hydrogen. , reducing agent.
  • the reducing agent is cerium ( Ce) and iron (Fe)
  • the ratio of chroma a * to lightness L * of the oxygen carrier obtained by a colorimetric test (a * /L * - A method for producing a gas that satisfies the relationship that oxygen carrier ) is 0.01 or more.
  • the method for producing a reducing agent and gas of the present invention may have any other configuration added to the above embodiments, and may be replaced with any configuration that performs similar functions. Well, part of the configuration may be omitted.
  • a gas containing hydrogen was described as a representative example of the reducing gas.
  • the reducing gas includes a hydrocarbon (eg, methane, ethane, acetylene, etc.) as a reducing substance instead of or in addition to hydrogen. and ammonia can also be used.
  • Example 1 Production of reducing agent (Example 1) First, as precursors of the reducing agent, cerium (III) nitrate hexahydrate (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd., purity: 98.0%) and zirconium nitrate dihydrate (FUJIFILM Wako Pure Chemical Industries, Ltd. Industrial Co., Ltd., purity: 97.0%) and iron (III) nitrate nonahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity: 99.9%) were weighed in predetermined amounts. .
  • cerium (III) nitrate hexahydrate manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd., purity: 98.0
  • zirconium nitrate dihydrate FUJIFILM Wako Pure Chemical Industries, Ltd. Industrial Co., Ltd., purity: 97.0
  • iron (III) nitrate nonahydrate manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., purity
  • citric acid manufactured by Fuji Film Wako Pure Chemical Industries, Ltd., purity: 99.5%
  • aqueous citric acid solution 6.06 g was weighed and dissolved in 96 mL of deionized water to obtain an aqueous citric acid solution.
  • the above precursor metal nitrate
  • the Ce:Zr:Fe (molar ratio) in the precursor aqueous solution was set to 0.6:0.08:0.32.
  • 2.15 g of ethylene glycol manufactured by Fuji Film Wako Pure Chemical Industries, Ltd., purity: 99.5%
  • a temperature of 80° C. was maintained with continuous stirring until a viscous gel was formed. After that, the gel was transferred to a drying oven. Drying of the gel was performed at 120° C. for 5 hours.
  • the resulting swollen lumps of organic and inorganic compounds were pulverized, heated from room temperature to 450° C. at a rate of 8° C./min, and then calcined at 450° C. for 4 hours. After that, the temperature was further raised to 950° C. at a rate of 8° C./min, and then fired at 950° C. for 8 hours. Finally, the fired agglomerates were finely pulverized mechanically to obtain the desired reducing agent consisting solely of the oxygen carrier.
  • the reducing agent was granular.
  • Example 2 A reducing agent was obtained in the same manner as in Example 1, except that the Ce:Zr:Fe (molar ratio) in the aqueous precursor solution was changed to 0.8:0.15:0.05.
  • Example 3 A reducing agent was obtained in the same manner as in Example 1, except that the Ce:Zr:Fe (molar ratio) in the aqueous precursor solution was changed to 0.9:0.07:0.03.
  • Example 4 A reducing agent was obtained by mixing 90 parts by mass of the oxygen carrier obtained in Example 2 and 10 parts by mass of aluminum oxide (binder) in a mortar.
  • Example 5 Cerium oxide (manufactured by Kojundo Chemical Co., Ltd.), manganese (IV) oxide (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) and iron oxide (III) (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) and were weighed out in predetermined amounts. The molar ratio of cerium oxide, manganese oxide and iron oxide was 0.94:0.04:0.02. Into a zirconia container, weighed particles of each oxide, 100 mL of deionized water, and zirconia beads of 4 mm ⁇ were added.
  • Example 6 A reducing agent was obtained in the same manner as in Example 5, except that the grinding time in the ball mill was changed to 4 hours.
  • Example 7 A reducing agent was obtained by mixing 30 parts by mass of the oxygen carrier obtained in Example 2 and 70 parts by mass of aluminum oxide (binder) in a mortar.
  • Example 8 Predetermined amounts of cerium oxide (manufactured by Kojundo Chemical Co., Ltd.) and iron (III) oxide (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) were weighed. The molar ratio of cerium oxide and iron oxide was 0.6:0.4. Lightened particles of each oxide were added to a mortar and mixed and ground with a pestle.
  • the substrate After raising the temperature from room temperature to 450° C. at a rate of 8° C./min in an air atmosphere, the substrate was fired at 450° C. for 4 hours. After that, the temperature was further raised to 950° C. at a rate of 8° C./min, and then fired at 950° C. for 8 hours. Finally, the fired agglomerates were finely pulverized mechanically to obtain the desired reducing agent consisting solely of the oxygen carrier. (Comparative example 1) A reducing agent was obtained by tableting cerium oxide alone. The packing densities of the reducing agents obtained in Examples 1 to 8 were 2 g/mL or more and 2.5 g/mL or less.
  • the metal composition in the reducing agent (metal oxide) was analyzed and identified by ICP emission spectrometry using argon gas using SPECTRO ARCOS manufactured by AMETEK.
  • a measurement solution was prepared by the following method. 50 to 100 mg of a reducing agent was dissolved in 100 mL of 1% nitric acid to 1% hydrofluoric acid, and the obtained solution was further diluted 10 times. Table 1 shows the results (molar ratios of metal elements) of the analysis of the measurement solution.
  • Colorimetric test A colorimetric color difference meter (manufactured by Nippon Denshoku Industries Co., Ltd., "ZE6000" was calibrated in accordance with JIS Z 8722: 2009. After that, the particles of each reducing agent were uniformly spread in a test cell for powder, A colorimetric test was performed. In addition, the measurement conditions in the colorimetry test are as follows. Calibration: Standard thin plate Measurement conditions: Light source D65, field of view 10°C Number of measurements: 3 measurements Color specifications: L * , a * , b *
  • the average value of the lightness L * and the chroma a * obtained from the three measurements was obtained, and the ratio (a * /L * ) was calculated from the average value of the chroma a * to the average value of L*. .
  • this value was taken as the ratio (a * /L * -oxygen carrier ).
  • the above values were taken as the ratio (a * /L * -reducing agent ), and the binders were separately subjected to a colorimetric test.
  • the ratio (a * /L * -oxygen carrier ) was calculated by the following equation (1).
  • the ratio of the binder contained in the reducing agent was measured by ICP mass spectrometry or the like.
  • Ratio (a * /L * -oxygen carrier ) [ratio (a * /L * -reducing agent )-ratio (a * /L * -binder ) x ratio of binder to reducing agent]/oxygen to reducing agent Percentage of careers (1)
  • Amount of oxygen deficiency The amount of oxygen deficiency of the reducing agent was measured using thermogravimetry (TG). The difference between the mass reduced by the reducing agent hydrogen and the mass increased by carbon dioxide is divided by the mass of the oxygen carrier contained in the charged reducing agent. , 100 to obtain the amount of oxygen deficiency (%). Specifically, first, a sample container was filled with 100 mg of a reducing agent. Next, the temperature was raised to 850° C. at 10° C./min while flowing helium.
  • a mixed gas of hydrogen and helium (10% by volume of hydrogen) was flowed at 100 mL/min for 10 minutes to reduce the reducing agent. After 10 minutes, helium gas was flowed at 100 mL/min for 30 minutes for gas exchange. The weight of the reducing agent at this time is defined as "A”.
  • a mixed gas of carbon dioxide and helium (10% by volume of carbon dioxide) was flowed at 100 mL/min for 10 minutes to oxidize the reducing agent. After 10 minutes, helium gas was flowed at 100 mL/min for 30 minutes for gas exchange. The weight of the reducing agent at this time is defined as "B”.
  • the amount of oxygen deficiency (%) was determined by (BA/mass of oxygen carrier contained in reducing agent) ⁇ 100.
  • Amount of carbon monoxide produced (amount of CO produced)
  • a quartz reaction tube having an inner diameter of 4 mm was prepared and filled with a cylindrical reducing agent formed to have a long diameter of 3 mm so that the layer height was 30 mm.
  • the amount of carbon monoxide produced is from 0.001 mmol or more per second to 0.001 mmol or less. It was defined as a value obtained by dividing the total amount of carbon monoxide produced by the weight (g) of the reducing agent.
  • the ⁇ S part (detection part) was used after being calibrated under the following conditions. That is, using a mass flow controller calibrated with carbon dioxide, with a discharge full scale of 10 mL / min or 50 mL / min, a flow rate accuracy of ⁇ 1.0%, and a repeatability of ⁇ 0.2%, carbon dioxide is Plot the detected signal intensity when flowing at 2, 3 mL / min, and use the least squares method to approximate the calibration curve with a straight line passing through the origin . Signal strength was adjusted. Based on this, the detected amount (the amount of carbon dioxide produced per second) was calculated with respect to the detected signal intensity of carbon dioxide. Also, carbon monoxide was similarly calibrated by the following procedure.
  • the reducing agent of each example produced a larger amount of carbon monoxide than the reducing agent of Comparative Example 1, which was cerium oxide alone. Further, the amount of carbon monoxide produced can be adjusted by adjusting the ratio (a * /L * -oxygen carrier ) by changing the types and ratios of the metal elements constituting the reducing agent (oxygen carrier). did it.
  • the oxygen carrier contained in the reducing agent of each example had a larger amount of oxygen deficiency than the cerium oxide alone constituting the reducing agent of Comparative Example 1. This result is in good agreement with the high conversion efficiency of carbon dioxide to carbon monoxide.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Organic Chemistry (AREA)
  • Inorganic Chemistry (AREA)
  • Life Sciences & Earth Sciences (AREA)
  • Geology (AREA)
  • Engineering & Computer Science (AREA)
  • Materials Engineering (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Catalysts (AREA)
PCT/JP2023/007870 2022-03-03 2023-03-02 還元剤およびガスの製造方法 Ceased WO2023167287A1 (ja)

Priority Applications (1)

Application Number Priority Date Filing Date Title
JP2024504752A JPWO2023167287A1 (cg-RX-API-DMAC7.html) 2022-03-03 2023-03-02

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2022-032781 2022-03-03
JP2022032781 2022-03-03

Publications (1)

Publication Number Publication Date
WO2023167287A1 true WO2023167287A1 (ja) 2023-09-07

Family

ID=87883855

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2023/007870 Ceased WO2023167287A1 (ja) 2022-03-03 2023-03-02 還元剤およびガスの製造方法

Country Status (2)

Country Link
JP (1) JPWO2023167287A1 (cg-RX-API-DMAC7.html)
WO (1) WO2023167287A1 (cg-RX-API-DMAC7.html)

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2024203959A1 (ja) * 2023-03-24 2024-10-03 積水化学工業株式会社 還元剤およびガスの製造方法

Citations (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2012512127A (ja) * 2008-12-17 2012-05-31 セリオン テクノロジー インコーポレイテッド 燃料添加剤含有格子操作二酸化セリウムナノ粒子
WO2018221357A1 (ja) * 2017-06-01 2018-12-06 日揮触媒化成株式会社 セリア系複合微粒子分散液、その製造方法及びセリア系複合微粒子分散液を含む研磨用砥粒分散液
WO2021192872A1 (ja) * 2020-03-25 2021-09-30 積水化学工業株式会社 還元剤およびガスの製造方法

Patent Citations (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2012512127A (ja) * 2008-12-17 2012-05-31 セリオン テクノロジー インコーポレイテッド 燃料添加剤含有格子操作二酸化セリウムナノ粒子
WO2018221357A1 (ja) * 2017-06-01 2018-12-06 日揮触媒化成株式会社 セリア系複合微粒子分散液、その製造方法及びセリア系複合微粒子分散液を含む研磨用砥粒分散液
WO2021192872A1 (ja) * 2020-03-25 2021-09-30 積水化学工業株式会社 還元剤およびガスの製造方法

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2024203959A1 (ja) * 2023-03-24 2024-10-03 積水化学工業株式会社 還元剤およびガスの製造方法

Also Published As

Publication number Publication date
JPWO2023167287A1 (cg-RX-API-DMAC7.html) 2023-09-07

Similar Documents

Publication Publication Date Title
JP7464738B2 (ja) アンモニア分解触媒
Rao et al. Surface and catalytic properties of Cu–Ce–O composite oxides prepared by combustion method
Zhang et al. Low-temperature catalytic oxidation of benzene over nanocrystalline Cu–Mn composite oxides by facile sol–gel synthesis
Zhong et al. Influence of preparation methods on the physicochemical properties and catalytic performance of Mn-Ce catalysts for lean methane combustion
US7807600B2 (en) Catalyst for acrylonitrile synthesis
CN104379255B (zh) 甲醇制造用催化剂及其制造方法以及甲醇的制造方法
Gigantino et al. Thermochemical energy storage via isothermal carbonation-calcination cycles of MgO-stabilized SrO in the range of 1000–1100 C
Jensen et al. FT-IR characterization of supported Ni-catalysts: Influence of different supports on the metal phase properties
US10226758B2 (en) Method for preparing catalyst used for preparing chlorine, catalyst and method for preparing chlorine
CN103908959B (zh) Ce‑Zr复合氧化铝材料及其制备方法
Chen et al. Preparation and characterization of a novel solid base catalyst hydroxyapatite loaded with strontium
WO2023167288A1 (ja) 還元剤およびガスの製造方法
CN105050714A (zh) 用于在二氧化碳存在下重整烃的含六铝酸镍的催化剂
Rocha et al. Physical and chemical properties of nanosized powders of gadolinia-doped ceria prepared by the cation complexation technique
Pecchi et al. Catalytic oxidation of soot over alkaline niobates
EP4129920A1 (en) Reducing agent, and method for producing gas
JP2011078947A (ja) アンモニア分解触媒、及びアンモニアの分解方法
WO2021192872A1 (ja) 還元剤およびガスの製造方法
Albaladejo-Fuentes et al. Tailoring the properties of BaTi0. 8Cu0. 2O3 catalyst selecting the synthesis method
Chai et al. Simple preparation of ZnO superstructures self-assembled by hexagonal prisms and their superb catalytic activity in the pyrolysis of ammonium perchlorate
Zhang et al. Hydrothermal synthesis and catalytic performance of single-crystalline La2− xSrxCuO4 for methane oxidation
Sato et al. Rapid oxygen storage and release with Brownmillerite-structured Ca2AlMnO5
WO2022167967A1 (en) Mixed metal oxide catalyst containing tantalum for odh of ethane
WO2022186319A1 (ja) 還元剤、ガスの製造方法および変換効率増加方法
EP4219403A1 (en) Oxygen carrier, method for producing oxygen carrier, and method for producing gas

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 23763544

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2024504752

Country of ref document: JP

Kind code of ref document: A

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 23763544

Country of ref document: EP

Kind code of ref document: A1