WO2017110986A1 - 表面調整剤、並びに、皮膜付きマグネシウム材又はマグネシウム合金材、及びそれらの製造方法 - Google Patents

表面調整剤、並びに、皮膜付きマグネシウム材又はマグネシウム合金材、及びそれらの製造方法 Download PDF

Info

Publication number
WO2017110986A1
WO2017110986A1 PCT/JP2016/088312 JP2016088312W WO2017110986A1 WO 2017110986 A1 WO2017110986 A1 WO 2017110986A1 JP 2016088312 W JP2016088312 W JP 2016088312W WO 2017110986 A1 WO2017110986 A1 WO 2017110986A1
Authority
WO
WIPO (PCT)
Prior art keywords
magnesium
film
dicalcium phosphate
chemical conversion
magnesium alloy
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2016/088312
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
幸宏 上田
涼子 桂谷
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nihon Parkerizing Co Ltd
Original Assignee
Nihon Parkerizing Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nihon Parkerizing Co Ltd filed Critical Nihon Parkerizing Co Ltd
Priority to KR1020187018842A priority Critical patent/KR20180083433A/ko
Priority to EP16878873.5A priority patent/EP3396020B1/en
Priority to CN201680074828.9A priority patent/CN108368613A/zh
Priority to JP2017558250A priority patent/JP6407453B2/ja
Priority to US16/064,511 priority patent/US20190003058A1/en
Priority to KR1020197036954A priority patent/KR102178613B1/ko
Publication of WO2017110986A1 publication Critical patent/WO2017110986A1/ja
Anticipated expiration legal-status Critical
Priority to US16/922,072 priority patent/US11725287B2/en
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C22/00—Chemical surface treatment of metallic material by reaction of the surface with a reactive liquid, leaving reaction products of surface material in the coating, e.g. conversion coatings, passivation of metals
    • C23C22/05—Chemical surface treatment of metallic material by reaction of the surface with a reactive liquid, leaving reaction products of surface material in the coating, e.g. conversion coatings, passivation of metals using aqueous solutions
    • C23C22/06—Chemical surface treatment of metallic material by reaction of the surface with a reactive liquid, leaving reaction products of surface material in the coating, e.g. conversion coatings, passivation of metals using aqueous solutions using aqueous acidic solutions with pH less than 6
    • C23C22/07—Chemical surface treatment of metallic material by reaction of the surface with a reactive liquid, leaving reaction products of surface material in the coating, e.g. conversion coatings, passivation of metals using aqueous solutions using aqueous acidic solutions with pH less than 6 containing phosphates
    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C22/00—Chemical surface treatment of metallic material by reaction of the surface with a reactive liquid, leaving reaction products of surface material in the coating, e.g. conversion coatings, passivation of metals
    • C23C22/78—Pretreatment of the material to be coated
    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C22/00—Chemical surface treatment of metallic material by reaction of the surface with a reactive liquid, leaving reaction products of surface material in the coating, e.g. conversion coatings, passivation of metals
    • C23C22/05—Chemical surface treatment of metallic material by reaction of the surface with a reactive liquid, leaving reaction products of surface material in the coating, e.g. conversion coatings, passivation of metals using aqueous solutions
    • C23C22/06—Chemical surface treatment of metallic material by reaction of the surface with a reactive liquid, leaving reaction products of surface material in the coating, e.g. conversion coatings, passivation of metals using aqueous solutions using aqueous acidic solutions with pH less than 6
    • C23C22/07—Chemical surface treatment of metallic material by reaction of the surface with a reactive liquid, leaving reaction products of surface material in the coating, e.g. conversion coatings, passivation of metals using aqueous solutions using aqueous acidic solutions with pH less than 6 containing phosphates
    • C23C22/08—Orthophosphates
    • C23C22/22—Orthophosphates containing alkaline earth metal cations
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01B—NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C
    • C01B25/00—Phosphorus; Compounds thereof
    • C01B25/16—Oxyacids of phosphorus; Salts thereof
    • C01B25/26—Phosphates
    • C01B25/32—Phosphates of magnesium, calcium, strontium, or barium
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
    • C01P2004/00—Particle morphology
    • C01P2004/60—Particles characterised by their size
    • C01P2004/62—Submicrometer sized, i.e. from 0.1-1 micrometer

Definitions

  • the present invention relates to a surface conditioner used for surface treatment of a magnesium material or a magnesium alloy material to be applied before chemical conversion treatment, and also includes a surface treatment step using the surface conditioner and a magnesium material with a coating including a chemical conversion treatment step. Or it relates to the manufacturing method of a magnesium alloy material. Furthermore, the present invention relates to a magnesium material or a magnesium alloy material having a film containing crystalline particles of dicalcium phosphate.
  • Magnesium materials and magnesium alloy materials (which mean metal materials containing magnesium as a main component; hereinafter, magnesium materials, magnesium alloy materials, etc. are referred to as “magnesium-containing metal materials”) are low specific gravity, tough and Since it is excellent in recyclability, it is widely used as various industrial parts materials such as automobiles, bicycles, fishing gears, home appliances (notebook computers, mobile phones, etc.).
  • the magnesium-containing metal material is a metal that is easily corroded among the metals in practical use. Therefore, chemical conversion treatment is performed to impart corrosion resistance to the magnesium-containing metal material.
  • Patent Document 1 discloses that a magnesium alloy cast product subjected to a predetermined treatment is (1) an acidic aqueous solution having a pH of 2 to 6 containing orthophosphoric acid and predetermined metal ions, or (2) predetermined fluorine.
  • a method for surface treatment of a magnesium alloy is disclosed, which includes a step of bringing a compound into contact with an acidic aqueous solution having a pH of 2 to 6 containing a predetermined metal oxyacid compound.
  • Patent Document 2 the surface of a magnesium alloy that has been subjected to a predetermined etching treatment and whose aluminum content is 7.5% by mass or less is used using a solution containing calcium ions, manganese ions, and phosphate ions.
  • a method for forming a chemical conversion film of a magnesium alloy including a step of chemical conversion treatment is disclosed.
  • the present invention solves the above-described problems, and provides a technique that enables a chemical conversion film having excellent adhesion and corrosion resistance to be formed on a magnesium-containing metal material and use of the technique. .
  • the present inventors have performed surface conditioning treatment before chemical conversion treatment using a surface conditioning agent containing dicalcium phosphate particles having a specific particle diameter.
  • the present inventors have found that a chemical conversion film having excellent adhesion and corrosion resistance can be formed on a magnesium-containing metal material, and have completed the present invention.
  • the present invention (1) containing dicalcium phosphate particles, D 50 of the second calcium phosphate particles is 0.1 ⁇ m or more and 0.8 ⁇ m or less, A surface conditioner wherein the dicalcium phosphate is monetite and / or brushite; (2) contacting the surface conditioner according to (1) above with a magnesium material or a magnesium alloy material; Contacting the surface treatment agent containing phosphate ions and calcium ions with the magnesium material or magnesium alloy material contacted with the surface conditioning agent; A method for producing a coated magnesium material or magnesium alloy material, comprising: (3) On the surface of the magnesium material or magnesium alloy material, it has a film containing crystalline particles of dicalcium phosphate, The average particle size of the crystalline particles of the dicalcium phosphate is 0.7 ⁇ m or more and 25 ⁇ m or less, and the standard deviation of the particle size distribution is 5 or less, A coated magnesium material or magnesium alloy material, wherein the dicalcium phosphate is monetite and / or brushite; Etc.
  • the surface conditioner which is an embodiment of the present invention, a magnesium-containing metal material with a film, and a manufacturing method thereof will be described in detail.
  • the surface conditioner according to the embodiment of the present invention is a pretreatment agent for efficiently forming a chemical conversion film containing calcium phosphate on a magnesium-containing metal material.
  • the surface conditioner contains dicalcium phosphate particles having a specific particle size. Using such a surface conditioner, the above-mentioned chemical conversion film having excellent adhesion and corrosion resistance is formed by performing the surface condition treatment before the chemical conversion treatment with the surface treatment agent containing phosphate ions and calcium ions. Can do.
  • the surface conditioner according to the present embodiment may contain components other than the dicalcium phosphate particles as long as the effects of the present invention are exhibited, but may be composed only of a solvent and dicalcium phosphate particles.
  • Dicalcium phosphate particles Dicalcium phosphate is also called calcium monohydrogen phosphate. Dihydrate calcium (CaHPO 4 ) and dihydrate (CaHPO 4 .2H 2 O) exist in dicalcium phosphate, and the anhydrous hydrate is called monetite, and the dihydrate is called brushite.
  • the surface conditioner according to the present embodiment only needs to contain at least one of monetite or brushite, and may contain both. Moreover, when both are included, the content ratio is not specifically limited.
  • the dicalcium phosphate may be crystalline dicalcium phosphate or amorphous dicalcium phosphate, but usually crystalline dicalcium phosphate is used. Moreover, the dicalcium phosphate may use a commercially available thing, and may manufacture it from a phosphoric acid raw material and a calcium raw material.
  • the method for producing dicalcium phosphate can be obtained, for example, by reacting a calcium raw material such as calcium carbonate or calcium hydroxide with a phosphoric acid aqueous solution and adjusting the pH to 4-5. At this time, monetite is obtained by setting the reaction temperature to at least 80 ° C. or higher, and brushite is obtained by setting the reaction temperature to at least 60 ° C. or lower. In addition, monetite may be obtained even if it is less than 80 degreeC, and brushite may be obtained even if it exceeds 60 degreeC.
  • Dicalcium phosphate particles its D 50 is usually 0.1 ⁇ m or more, may also be 0.2 ⁇ m or more, may be 0.3 ⁇ m or more.
  • the upper limit is usually 0.8 ⁇ m or less, may be 0.6 ⁇ m or less, and may be 0.5 ⁇ m or less.
  • a chemical conversion film having excellent adhesion and corrosion resistance is formed by performing the chemical conversion treatment thereafter. can do.
  • the second calcium phosphate particles, the D 90 of is usually 0.15 ⁇ m or more, it may also be 0.2 ⁇ m or more, may be 0.3 ⁇ m or more.
  • the upper limit is usually 1.5 ⁇ m or less, may be 1.2 ⁇ m or less, and may be 1.0 ⁇ m or less.
  • D 50 and D 90 represent the particle diameters located at 50% by volume and 90% by volume, respectively, when the cumulative curve of the particles is obtained with the total volume of dicalcium phosphate particles in the surface conditioning agent as 100%.
  • the particle size distribution of the dicalcium phosphate particles in the surface conditioner is, for example, analyzed for the intensity of light scattered from the particles irradiated with laser light and the diffraction image generated on the focal plane by collecting the light with a lens. Can be obtained.
  • the particle diameter located in 50 volume% and 90 volume% can be calculated
  • the diameter of the dicalcium phosphate particles can be adjusted by a conventional method such as a wet pulverization method. More specifically, it can be adjusted by pulverizing a mixture of water, a dispersant, and dicalcium phosphate particles with a bead mill.
  • the mass concentration of the dicalcium phosphate particles in the mixture is not particularly limited, but is preferably 5 to 50 wt%.
  • Dispersant examples include monosaccharides or polysaccharides or derivatives thereof; orthophosphoric acid, polyphosphoric acid or salts thereof, or organic phosphonic acid compounds or salts thereof; vinyl acetate polymers or derivatives thereof, or vinyl acetate.
  • Water-soluble polymer compound comprising a copolymer of a polymerizable monomer and vinyl acetate; Formula: H 2 C ⁇ C (R 1 ) —COOR 2 (wherein R 1 is H or CH 3 , R 2 is H, C is an alkyl group of 1 to 5 or a hydroxyalkyl group of C is 1 to 5) or at least one selected from ⁇ , ⁇ unsaturated carboxylic acid monomers, And a polymer or copolymer obtained by polymerizing 50% by weight or less of a monomer copolymerizable with the monomer.
  • Examples of basic saccharides of the monosaccharides or polysaccharides or derivatives thereof include, for example, fructose, tagatose, psicose, sulbose, erythrose, threose, ribose, arabinose, xylose, lyxose, allose, altrose, glucose, mannose, growth, Examples include idose, galactose, talose and the like.
  • the hydroxyl group of the basic constituent saccharide is NO 2
  • Monosaccharides obtained by etherification with substituents such as CH 3 , C 2 H 4 OH, CH 2 CH (OH) CH 3 , CH 2 COOH, and homopolysaccharides containing monosaccharides substituted with the above substituents in the structure Or heteropolysaccharides can also be used. Further, several types of monosaccharides, polysaccharides, and derivatives thereof may be used in combination.
  • the saccharides When the saccharides are classified, they may be classified as monosaccharides, small saccharides, and polysaccharides depending on the degree of hydrolysis.
  • polysaccharides that produce two or more monosaccharides by hydrolysis A saccharide that itself is not further hydrolyzed was designated as a monosaccharide.
  • D-monosaccharide, L-monosaccharide and light-irradiating property (+ Any combination of,-) can be used.
  • sodium salts or ammonium salts of the monosaccharides, polysaccharides, and derivatives thereof may be used.
  • it when it is difficult to make water soluble in the above structure, it may be used after dissolving in an organic solvent having compatibility with water in advance.
  • Orthophosphoric acid is orthophosphoric acid.
  • polyphosphoric acid for example, pyrophosphoric acid, triphosphoric acid, trimetaphosphoric acid, tetrametaphosphoric acid, hexametaphosphoric acid or its sodium salt, ammonium salt and the like can be used.
  • organic phosphonic acid compound for example, aminotrimethylenephosphonic acid, 1-hydroxyethylidene-1,1-diphosphonic acid, ethylenediaminetetramethylenephosphonic acid, diethylenetriaminepentamethylenephosphonic acid or a sodium salt thereof can be used. it can.
  • Examples of the vinyl acetate polymer or derivatives thereof include polyvinyl alcohol which is a saponified product of vinyl acetate polymer, cyanoethylated polyvinyl alcohol obtained by cyanoethylating polyvinyl alcohol with acrylonitrile, and formalized polyvinyl obtained by acetalizing polyvinyl alcohol with formalin.
  • Alcohol, urethanized polyvinyl alcohol obtained by urethanizing polyvinyl alcohol with urea, and water-soluble polymer compounds obtained by introducing a carboxyl group, a sulfone group, an amide group, or the like into polyvinyl alcohol can be used.
  • water-soluble means the property that a substance of 0.1 g or more dissolves in 100 g of water at 25 ° C., or the property that the mixture of the material and water is transparent (the same applies hereinafter). ).
  • acrylic acid, crotonic acid, maleic anhydride etc. can be used, for example.
  • the vinyl acetate polymer or a derivative thereof or a copolymer of a monomer copolymerizable with vinyl acetate and vinyl acetate can sufficiently exhibit the effects of the present invention as long as it is water-soluble. Therefore, the effect is not affected by the degree of polymerization and the introduction rate of functional groups.
  • One kind of vinyl acetate polymer or its derivatives and copolymers may be used, or two or more kinds may be used in combination.
  • Examples of the monomer represented by the above formula include methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, pentyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, methacrylic acid.
  • Pentyl acid hydroxymethyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, hydroxypentyl acrylate, hydroxymethyl methacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, hydroxybutyl methacrylate, methacrylic acid Hydroxypentyl and the like can be used.
  • ⁇ , ⁇ unsaturated carboxylic acid monomer for example, acrylic acid, methacrylic acid, maleic acid and the like can be used.
  • monomer copolymerizable with the monomer for example, vinyl acetate, styrene, vinyl chloride, vinyl sulfonic acid and the like can be used.
  • the solvent is not particularly limited as long as dicalcium phosphate can be suitably dispersed, but water is usually used.
  • An organic solvent may be added to water.
  • the content of the organic solvent relative to the total amount of the solvent is usually 10% by weight or less, may be 5% by weight or less, and may be 3% by weight or less.
  • the type of the organic solvent is not particularly limited, and examples thereof include alcohol-based organic solvents, hydrocarbon-based organic solvents, ketone-based organic solvents, and amide-based organic solvents.
  • the content of dicalcium phosphate particles in the surface conditioner is usually 0.05 g / L or more as a solid content concentration, and may be 0.1 g / L or more. Moreover, an upper limit is 20 g / L or less normally, 10 g / L or less may be sufficient and 5 g / L or less may be sufficient. If it is in the said range, the dispersibility of the dicalcium phosphate particle in a surface conditioning agent is favorable.
  • the surface conditioner may contain a thickener, a dispersion stability improver, a pH adjuster, and the like as necessary.
  • the thickener ensures dispersibility of the dicalcium phosphate particles in the surface conditioner and can prevent caking due to the precipitation of the dicalcium phosphate particles.
  • the type of thickener is not particularly limited.
  • natural polymers such as proteins, natural rubbers, saccharides (including sugar derivatives), alginic acids, and celluloses; amine resins, carboxylic acid resins , Synthetic polymers such as olefin-based resins, ester-based resins, urethane-based resins, PVA, acrylic (methacrylic) -based resins, or copolymers obtained by combining two or more of these resins;
  • examples include various surfactants such as surfactants, cationic surfactants, anionic surfactants, and amphoteric surfactants; various coupling agents such as silane coupling agents and titanium coupling agents.
  • the content of the thickener in the surface conditioner is usually 0.1% by weight or more and 0.5% by weight or more from the viewpoint of maintaining good dispersibility. Moreover, an upper limit is 20 weight% or less normally, and may be 10 weight% or less.
  • the dispersion stability improver is an agent that improves the dispersion stability of the dicalcium phosphate particles in the surface conditioner.
  • examples of the dispersion stability improver include condensed phosphate alkali salts such as sodium polyphosphate, potassium polyphosphate, sodium metaphosphate, potassium metaphosphate, sodium pyrophosphate, and potassium pyrophosphate.
  • the pH adjuster is a drug for adjusting the pH of the surface adjuster within a predetermined range.
  • the type of pH adjuster is not particularly limited, and examples thereof include phosphate-based phosphates such as disodium hydrogen phosphate hydrate, dipotassium hydrogen phosphate, magnesium hydrogen phosphate hydrate, and diammonium hydrogen phosphate. Examples include alkali additives; carbonate-based alkali additives such as sodium carbonate, potassium carbonate, basic magnesium carbonate hydrate, ammonium hydrogen carbonate, and calcium carbonate;
  • the pH of the surface conditioner is usually adjusted to 6 or more and 11 or less. The lower limit may be 7 or more, and the upper limit may be 10 or less, or 9 or less.
  • pH in this specification shows the value which measured the 25 degreeC surface adjustment agent with the commercially available pH meter.
  • the surface conditioner according to the present embodiment is, for example, adjusting the pH of a mixture obtained by mixing dicalcium phosphate particles in a solvent and, if necessary, a dispersant to a predetermined pH with a pH adjuster, and subsequently adjusting the pH.
  • the obtained mixture can be wet pulverized and then stirred to disperse the dicalcium phosphate particles.
  • the pH of a mixture obtained by mixing dicalcium phosphate particles preliminarily adjusted to a predetermined particle size in a solvent and, if necessary, a dispersant can be produced by adjusting the pH to a predetermined pH with a pH adjusting agent. it can.
  • the dispersant and the pH adjuster are preliminarily mixed with the dicalcium phosphate particles before wet pulverization. However, either of them is mixed with dicalcium phosphate particles before wet pulverization and wet pulverization. Later, the other may be mixed with dicalcium phosphate particles. Moreover, you may mix a dispersing agent and a pH adjuster with a dicalcium phosphate particle after wet-grinding.
  • the order of addition of the raw material to the solvent is not particularly limited, dicalcium phosphate, a dispersant and a pH adjuster may be added at once, dibasic calcium phosphate is added to the solvent with only the dispersant added, You may add a pH adjuster as needed.
  • the wet pulverization for adjusting the particle diameter can be performed using, for example, a bead mill, but is not limited thereto.
  • the pulverization time is not particularly limited, and may be performed until a desired particle diameter is obtained.
  • the present invention is a magnesium-containing metal material with a coating, and the coating is a chemical conversion coating.
  • This chemical conversion film has crystalline particles of dicalcium phosphate.
  • the method for producing a magnesium-containing metal material having a chemical conversion film includes a first contact step of bringing the surface conditioner into contact with the surface of the magnesium-containing metal material, and a magnesium ion-containing metal material in contact with the surface treatment agent. And a second contact step in which a surface treatment agent containing calcium ions is contacted.
  • the first contact process is referred to as a surface adjustment process.
  • the second contact process is hereinafter referred to as a chemical conversion treatment process.
  • a chemical conversion film having excellent adhesion and corrosion resistance can be formed on the surface of the magnesium-containing metal material.
  • pre-processing processes such as degreasing, pickling, etching, smut removal, and paper grinding
  • the oxide film of the magnesium-containing metal material, the oil or dirt adhering to the magnesium-containing metal material can be removed, and the surface can be cleaned.
  • treatments such as solvent washing, steam treatment (also referred to as “hydrothermal treatment”, “magnesium hydroxide film formation treatment”, etc.) may be performed.
  • the adhesion between the magnesium-containing metal material and the chemical conversion film can be improved, and a coated magnesium-containing metal material having excellent corrosion resistance can be obtained.
  • a known method can be used as the steam treatment method.
  • post treatment steps such as washing with water, drying, and painting may be appropriately performed. These pretreatment steps and posttreatment steps can be performed by known methods.
  • the surface conditioning treatment step is a method of treating the surface by bringing the surface conditioning agent into contact with a magnesium-containing metal material.
  • Examples of the contact method of the surface adjusting agent include a spray coating method, a dip coating method, a roll coating method, a curtain coating method, a spin coating method, and a method in which these are appropriately combined.
  • the temperature of the surface treatment agent or the magnesium-containing metal material in the surface conditioning treatment step is usually 0 ° C. or higher, may be 10 ° C. or higher, is usually 40 ° C. or lower, and may be 30 ° C. or lower.
  • the contact time between the surface conditioner and the magnesium-containing metal material is usually 1 second or longer, 5 seconds or longer, and 10 seconds or longer. Also, it is usually 10 minutes or less, 5 minutes or less, 3 minutes or less, or 1 minute or less.
  • the chemical conversion treatment step is a method in which a surface treatment agent (chemical conversion treatment agent) is brought into contact with the magnesium-containing metal material that has been brought into contact with the surface conditioning agent, and the surface thereof is subjected to chemical conversion treatment.
  • the chemical conversion treatment agent is not particularly limited as long as it contains phosphate ions and calcium ions.
  • the phosphate ion supply source include phosphoric acid and water-soluble phosphate.
  • the calcium ion supply source include calcium hydroxide, calcium carbonate, and calcium nitrate.
  • the calcium ion concentration and the phosphate ion concentration of the chemical conversion treatment agent are not particularly limited as long as a chemical conversion film having crystalline particles of dicalcium phosphate can be formed on the magnesium-containing metal material.
  • the phosphate ion concentration is usually 500 ppm or more, may be 1000 ppm or more, is usually 20000 ppm or less, and may be 10000 ppm or less.
  • the calcium ion concentration is usually 100 ppm or more, may be 500 ppm or more, is usually 10000 ppm or less, and may be 5000 ppm or less.
  • the pH of the chemical conversion treatment agent is usually 2.0 or more, 3.0 or more, 4.0 or more, usually 5.0 or less, and 4.5 or less. .
  • the pH adjuster for adjusting the pH of the chemical conversion treatment agent is not particularly limited, and an acid component such as nitric acid, phosphoric acid or sulfuric acid, or an alkali component such as sodium hydroxide, sodium carbonate, aqueous ammonia or ammonium hydrogen carbonate is used. be able to.
  • the method of chemical conversion treatment is not particularly limited, and examples thereof include a spray treatment method, an immersion treatment method, an electrolytic treatment method, and a pouring treatment method.
  • the temperature of the chemical conversion treatment is usually 10 ° C or higher, 40 ° C or higher, 70 ° C or higher, and usually 100 ° C or lower and 90 ° C or lower.
  • the contact time between the magnesium-containing metal material and the surface treatment agent is usually 1 minute or longer, 3 minutes or longer, 5 minutes or longer, and usually 60 minutes or shorter, 30 It may be less than or equal to 15 minutes or less.
  • the magnesium-containing metal material that is the target of the surface conditioning treatment and chemical conversion treatment is a metal material mainly composed of magnesium, such as a magnesium material or a magnesium alloy material.
  • the magnesium alloy material is composed of two metal components, the magnesium alloy material only needs to contain 50% by weight or more, and preferably contains 80% by weight or more.
  • a magnesium alloy material consists of three or more metal components, what is necessary is just to contain magnesium most.
  • the magnesium alloy material include AZ91, AM60, ZK51, ZK61, AZ31, AZ61, ZK60, and the like.
  • ⁇ Magnesium-containing alloy material with film> Another embodiment of the present invention is a coated magnesium-containing metal material having a film containing dicalcium phosphate particles on the surface of the magnesium-containing metal material.
  • the magnesium-containing metal material with a film may be a film containing dicalcium phosphate particles and a rust preventive oil or sealing agent attached thereto, or a coating film may be further formed on the film containing dicalcium phosphate particles. You may have.
  • the dicalcium phosphate particles contained in the film are crystalline particles.
  • the dicalcium phosphate particles may be monetite or brushite, or may contain both. Moreover, when both are included, those content ratios are not specifically limited.
  • the film containing crystalline dicalcium phosphate particles has a uniform and dense structure. Therefore, the film has excellent adhesion and corrosion resistance.
  • XRD X-ray diffraction
  • the crystalline particles of dicalcium phosphate in the film have an average primary particle size of 0.7 ⁇ m or more, 1 ⁇ m or more, 2 ⁇ m or more, 3 ⁇ m or more, and 25 ⁇ m or less. , 20 ⁇ m or less, 15 ⁇ m or less, or 10 ⁇ m or less.
  • a film containing crystalline dicalcium phosphate particles having an average primary particle diameter within the above range has excellent adhesion and corrosion resistance.
  • the dicalcium phosphate particles in the film have a standard deviation of the particle size distribution of 5 or less, 3 or less, 1.5 or less, or 1 or less.
  • a film containing crystalline dicalcium phosphate particles having a standard deviation within this range has a more uniform and dense structure.
  • the average primary particle diameter can be determined by observation with a scanning electron microscope. Specifically, the maximum diameter and the minimum diameter of 100 randomly selected crystalline dicalcium phosphate particles are measured, and the average value of all the diameters is calculated to obtain the average primary particle diameter. Further, the standard deviation of the particle size distribution can be obtained by measuring the diameter of 100 randomly selected crystalline dicalcium phosphate particles and preparing the particle size distribution. As means for adjusting the dicalcium phosphate particles in the film to the above-mentioned diameter and standard deviation, performing the above-mentioned surface adjustment treatment step and chemical conversion treatment step can be mentioned.
  • the coverage of the film formed on the magnesium-containing metal material is preferably high from the viewpoint of corrosion resistance, and is usually 90% or more and may be 95% or more.
  • the coverage can be calculated by observation with a scanning electron microscope, and can be calculated by measuring the area ratio between the base of the magnesium-containing metal material and the portion covered with the film by visual observation or image analysis.
  • the amount of film formed on the magnesium-containing metal material is usually 0.5 g / m 2 or more, may be at 1.0 g / m 2 or more, generally not more than 10g / m 2, 5g / m 2 It may be the following.
  • a magnesium-containing metal material having a film containing crystalline dicalcium phosphate having a film amount within the above range has good adhesion and corrosion resistance.
  • the amount of the film containing the crystalline dicalcium phosphate particles can be calculated by quantifying the amount of calcium and the amount of phosphorus by fluorescent X-ray spectroscopic analysis and converting them to CaHPO 4 . Examples of the method for increasing the coverage and the method for increasing the coating amount include a method for adjusting the treatment time in the chemical conversion treatment step, as well as a method for performing the surface adjustment treatment step with the surface conditioning agent before the chemical conversion treatment step.
  • the film thickness of the film is not particularly limited, but is usually 1 ⁇ m or more, 2 ⁇ m or more, or 15 ⁇ m or less, or 10 ⁇ m or less from the viewpoint of corrosion resistance.
  • the film thickness of the film can be determined by observing the cross-sectional shape of the film using a laser microscope.
  • the surface of the film formed on the magnesium-containing metal material is preferably uniform, but may have a predetermined roughness.
  • the arithmetic average surface roughness (Ra) of the film surface may be 7 ⁇ m or less, and may be 4 ⁇ m or less.
  • the coating containing the dicalcium phosphate particles is a porous coating, as described above, the pores of the coating are filled by attaching rust preventive oil or a sealing agent to the coating containing the second calcium phosphate particles. More excellent corrosion resistance.
  • the said coating film can be formed by coating on the film
  • the coating method is not particularly limited, and examples thereof include known methods such as electrodeposition coating (for example, cationic electrodeposition coating), solvent coating, and powder coating.
  • electrodeposition coating for example, cationic electrodeposition coating
  • solvent coating for example, solvent coating
  • powder coating for example, solvent coating
  • powder coating a coating film on the film
  • the thickness of the coating film is not particularly limited, but is on average 5 to 30 ⁇ m, and may be 8 to 25 ⁇ m.
  • Magneium alloy material As the magnesium alloy material, an ASTM (American Society for Testing and Materiarls) -AZ31 plate was used. In addition, before performing the below-mentioned surface adjustment process with respect to a board
  • an alkaline degreasing agent Naippon Parkerizing Co., Ltd .; Fine Cleaner MG110E
  • phosphoric acid and calcium nitrate tetrahydrate were dissolved in deionized water so that the final concentrations would be 7 g / L and 12 g / L, respectively, and then the pH was adjusted to 3.5 with sodium hydroxide. Then, a surface treatment agent (chemical conversion treatment agent) was prepared.
  • ⁇ Surface conditioning treatment and chemical conversion treatment> The polished plate material was immersed in a surface conditioner at 25 ° C. for 30 seconds to perform surface adjustment treatment. Thereafter, the plate material was immersed in a chemical conversion treatment agent for 15 minutes to perform chemical conversion treatment. Subsequently, the plate material was washed with deionized water and dried with hot air to prepare a coated magnesium alloy material.
  • Table 2 shows the temperature of each chemical conversion treatment agent used in the chemical conversion treatment.
  • ⁇ Adhesion evaluation> A magnesium alloy material with a film was electrodeposited and the adhesion of the coating film to the magnesium alloy material was evaluated. Using a cationic electrodeposition paint “GT-10LF” manufactured by Kansai Paint Co., Ltd., a coating film was formed under the conditions of a paint temperature of 28 ° C. and a voltage of 200V. Then, it washed with water and baked for 20 minutes at 150 degreeC, and obtained the magnesium alloy material which has a coating film with a dry film thickness of 20 micrometers.
  • GT-10LF cationic electrodeposition paint
  • a magnesium alloy material having a coating film was immersed in deionized water at 40 ° C., and after 240 hours, the paper was cross-cut with a paper cutter, a cellophane tape was attached to the cross-cut portion, and a tape peeling test was performed. .
  • the grid-like cross cut was made into 100 squares by crossing 11 parallel lines with 1 mm intervals at right angles. The number of squares peeled after tape peeling was measured, and adhesiveness was evaluated according to the following criteria. The results are shown in Table 2.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Organic Chemistry (AREA)
  • General Chemical & Material Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Engineering & Computer Science (AREA)
  • Materials Engineering (AREA)
  • Mechanical Engineering (AREA)
  • Metallurgy (AREA)
  • Chemical Treatment Of Metals (AREA)
  • Inorganic Chemistry (AREA)
PCT/JP2016/088312 2015-12-25 2016-12-22 表面調整剤、並びに、皮膜付きマグネシウム材又はマグネシウム合金材、及びそれらの製造方法 Ceased WO2017110986A1 (ja)

Priority Applications (7)

Application Number Priority Date Filing Date Title
KR1020187018842A KR20180083433A (ko) 2015-12-25 2016-12-22 표면 조정제, 그리고, 피막 부착 마그네슘재 또는 마그네슘 합금재, 및 그것들의 제조 방법
EP16878873.5A EP3396020B1 (en) 2015-12-25 2016-12-22 Surface-conditioning agent, as well as magnesium member or magnesium alloy material with film, and manufacturing method therefor
CN201680074828.9A CN108368613A (zh) 2015-12-25 2016-12-22 表面调整剂、带被膜的镁材料或镁合金材料及其制造方法
JP2017558250A JP6407453B2 (ja) 2015-12-25 2016-12-22 表面調整剤、並びに、皮膜付きマグネシウム材又はマグネシウム合金材、及びそれらの製造方法
US16/064,511 US20190003058A1 (en) 2015-12-25 2016-12-22 Surface-conditioning agent, as well as magnesium member or magnesium alloy material with film, and manufacturing method therefor
KR1020197036954A KR102178613B1 (ko) 2015-12-25 2016-12-22 표면 조정제, 그리고, 피막 부착 마그네슘재 또는 마그네슘 합금재, 및 그것들의 제조 방법
US16/922,072 US11725287B2 (en) 2015-12-25 2020-07-07 Method for manufacturing a magnesium material or magnesium alloy material with a coating

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2015254045 2015-12-25
JP2015-254045 2015-12-25

Related Child Applications (2)

Application Number Title Priority Date Filing Date
US16/064,511 A-371-Of-International US20190003058A1 (en) 2015-12-25 2016-12-22 Surface-conditioning agent, as well as magnesium member or magnesium alloy material with film, and manufacturing method therefor
US16/922,072 Division US11725287B2 (en) 2015-12-25 2020-07-07 Method for manufacturing a magnesium material or magnesium alloy material with a coating

Publications (1)

Publication Number Publication Date
WO2017110986A1 true WO2017110986A1 (ja) 2017-06-29

Family

ID=59089539

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2016/088312 Ceased WO2017110986A1 (ja) 2015-12-25 2016-12-22 表面調整剤、並びに、皮膜付きマグネシウム材又はマグネシウム合金材、及びそれらの製造方法

Country Status (6)

Country Link
US (2) US20190003058A1 (enExample)
EP (1) EP3396020B1 (enExample)
JP (2) JP6407453B2 (enExample)
KR (2) KR20180083433A (enExample)
CN (2) CN111926316B (enExample)
WO (1) WO2017110986A1 (enExample)

Families Citing this family (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN113862686A (zh) * 2021-09-17 2021-12-31 马鞍山佰斯予菲环保新材料科技有限公司 一种金属表面处理剂及其制备方法和应用

Citations (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH116076A (ja) * 1997-06-13 1999-01-12 Nippon Parkerizing Co Ltd 鉄鋼材料のりん酸塩処理方法
JP2002121681A (ja) * 2000-10-12 2002-04-26 Kiwa Kagaku Yakuhin Kk マグネシウム合金の皮膜化成用組成物及び方法

Family Cites Families (23)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
USRE16340E (en) 1926-05-04 Christian bergh backer
FR1591353A (enExample) * 1968-01-15 1970-04-27
JPH06900B2 (ja) * 1985-09-28 1994-01-05 関西ペイント株式会社 鋼板用塗料組成物
JP3451334B2 (ja) * 1997-03-07 2003-09-29 日本パーカライジング株式会社 金属のりん酸塩皮膜化成処理前の表面調整用前処理液及び表面調整方法
US6361623B1 (en) 1997-06-13 2002-03-26 Henkel Corporation Method for phosphatizing iron and steel
JP3783995B2 (ja) 1999-05-12 2006-06-07 日本パーカライジング株式会社 マグネシウム合金の表面処理方法
DE10161827A1 (de) * 2001-12-15 2003-06-26 Dot Gmbh Verfahren zur Beschichtung eines Substrats mit Calciumphosphat
JP3845328B2 (ja) 2002-03-29 2006-11-15 株式会社栗本鐵工所 マグネシウム合金の化成処理皮膜の形成方法
ATE353987T1 (de) 2002-06-13 2007-03-15 Nippon Paint Co Ltd Zinkphosphatkonditioniermittel für phosphatkonversionsbeschichtung von stahlplatte und entsprechendes produkt
US20060013921A1 (en) * 2002-12-04 2006-01-19 Hidemitsu Kasahara Calcium phosphate base particulate compound, process for producing the same and composition comprising the compound
JP2007077498A (ja) * 2005-08-19 2007-03-29 Nippon Paint Co Ltd 表面調整用組成物及び表面調整方法
CN101243207B (zh) * 2005-08-19 2010-11-24 日本油漆株式会社 用于表面调整的组合物以及表面调整方法
US8119239B2 (en) * 2005-08-19 2012-02-21 Nippon Paint Co., Ltd. Surface-conditioning composition comprising metal phosphate particles, metal alkoxide and stabilizer, and method of production thereof
EP1930473B1 (en) 2005-08-19 2016-04-06 Nippon Paint Co., Ltd. Surface-conditioning composition, method for production thereof, and surface conditioning method
CN101191207A (zh) * 2006-11-23 2008-06-04 汉达精密电子(昆山)有限公司 镁合金表面钙系磷化溶液及其化成处理工艺
CN101274494B (zh) * 2007-03-26 2013-07-17 株式会社神户制钢所 表面稳定性优异的铝合金材
JP2009029693A (ja) * 2007-06-29 2009-02-12 Mitsubishi Chemicals Corp 薄片状リン酸水素カルシウム無水物およびその製造方法
CN101565825B (zh) * 2009-06-03 2011-02-02 哈尔滨工业大学 镁或镁合金表面的处理方法
US20110046239A1 (en) * 2009-08-24 2011-02-24 Keiser Bruce A Calcium based carrier particles
JP6302696B2 (ja) * 2014-02-13 2018-03-28 権田金属工業株式会社 マグネシウム合金の表面処理方法
US20150374751A1 (en) 2014-06-25 2015-12-31 Skeletal Kinetics, Llc Implantable, Malleable Calcium Phosphate Compositions and Methods for Making and Using the Same
GB201417020D0 (en) 2014-09-26 2014-11-12 Univ Leeds And Univ St Andrews The Formulation
CN104947097B (zh) * 2015-06-30 2017-08-25 山东大学 一种纯钛表面磷酸氢钙微纳米纤维转化膜的制备方法

Patent Citations (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH116076A (ja) * 1997-06-13 1999-01-12 Nippon Parkerizing Co Ltd 鉄鋼材料のりん酸塩処理方法
JP2002121681A (ja) * 2000-10-12 2002-04-26 Kiwa Kagaku Yakuhin Kk マグネシウム合金の皮膜化成用組成物及び方法

Also Published As

Publication number Publication date
US11725287B2 (en) 2023-08-15
JP2018193620A (ja) 2018-12-06
CN111926316A (zh) 2020-11-13
KR102178613B1 (ko) 2020-11-13
JP6407453B2 (ja) 2018-10-17
EP3396020A1 (en) 2018-10-31
US20190003058A1 (en) 2019-01-03
CN111926316B (zh) 2022-03-01
CN108368613A (zh) 2018-08-03
KR20180083433A (ko) 2018-07-20
EP3396020B1 (en) 2021-04-07
EP3396020A4 (en) 2019-09-11
KR20190141029A (ko) 2019-12-20
JPWO2017110986A1 (ja) 2018-09-20
JP6803881B2 (ja) 2020-12-23
US20200340123A1 (en) 2020-10-29

Similar Documents

Publication Publication Date Title
ES2286889T3 (es) Acondicionamiento de superficies metalicas antes de la fosfatacion de las mismas.
RU2748349C2 (ru) Улучшенный способ не содержащего никель фосфатирования металлических поверхностей
CN1735713A (zh) 涂料组合物
JP2001049451A (ja) 金属材料のりん酸塩化成処理方法
US11725287B2 (en) Method for manufacturing a magnesium material or magnesium alloy material with a coating
US20210172067A1 (en) Production method for magnesium-containing metal material provided with coating
RU2363769C2 (ru) Состав для нанесения покрытий
BR112016017018B1 (pt) Método para revestimento de superfícies metálicas, seus substratos revestidos e seu uso
CN101451239B (zh) 一种化学转化处理液和镁合金表面的处理方法
AU7619094A (en) Pre-rinse for phosphating metal surfaces
EP1930474A1 (en) Surface-conditioning composition, method for production thereof, and surface conditioning method
JP5428105B2 (ja) マグネシウム合金用黒色化成処理液、化成処理方法及び化成処理部材
CA2434306A1 (en) Aqueous surface conditioner and surface conditioning method for phosphating treatment
WO2002031223A1 (en) Surface-treating agent for metallic material with excellent suitability for press forming and chemical treatment and method of treatment
RU2096522C1 (ru) Композиция для получения защитного фосфатного покрытия и корректирующий состав для нее
WO2022002792A1 (en) Improved activation agent for manganese phosphating processes
WO2019131766A1 (ja) 金属表面処理剤、並びに表面処理皮膜を有する金属材料及びその製造方法
WO2026125200A1 (en) Surface conditioner for metallic surfaces prior to conversion coating
MXPA01000609A (en) Conditioning metal surfaces before phosphating them
JP2006299379A (ja) 表面調整剤及び表面調整方法

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 16878873

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2017558250

Country of ref document: JP

Kind code of ref document: A

NENP Non-entry into the national phase

Ref country code: DE

ENP Entry into the national phase

Ref document number: 20187018842

Country of ref document: KR

Kind code of ref document: A

WWE Wipo information: entry into national phase

Ref document number: 1020187018842

Country of ref document: KR

WWE Wipo information: entry into national phase

Ref document number: 2016878873

Country of ref document: EP

ENP Entry into the national phase

Ref document number: 2016878873

Country of ref document: EP

Effective date: 20180725