WO2016127509A1 - Procédé d'application de revêtement pour revêtement éclair anti-salissure rtv d'isolateur en forme de parapluie/cloche - Google Patents
Procédé d'application de revêtement pour revêtement éclair anti-salissure rtv d'isolateur en forme de parapluie/cloche Download PDFInfo
- Publication number
- WO2016127509A1 WO2016127509A1 PCT/CN2015/078465 CN2015078465W WO2016127509A1 WO 2016127509 A1 WO2016127509 A1 WO 2016127509A1 CN 2015078465 W CN2015078465 W CN 2015078465W WO 2016127509 A1 WO2016127509 A1 WO 2016127509A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- coating
- insulator
- dip
- rotation speed
- rpm
- Prior art date
Abstract
L'invention concerne un procédé d'application de revêtement, pour un revêtement éclair, anti-salissure et RTV d'isolateur en forme de parapluie/cloche, qui est caractérisé en ce qu'il comprend les étapes suivantes : (A) le nettoyage de la surface d'un isolateur et facultativement la couverture d'une partie de l'isolateur pour laquelle un revêtement n'est pas nécessaire ; (B) l'immersion de l'isolateur dans un bain pour enduction rotative par utilisation d'une machine d'enduction ayant une fonction de rotation ; C) la solidification de l'isolateur revêtu à température ambiante et dans des conditions humides. Le procédé d'application de revêtement est simple à mettre en œuvre, peu coûteux, réduit la pollution, sa fabrication est sans danger, permet une commande automatisée pour un processus allant du revêtement par immersion à la solidification préliminaire, une qualité de produit facile à contrôler et une productivité élevée, et fournit un aspect lisse, exempt de bulles, de gouttes suspendues et d'accumulations, ainsi qu'un revêtement égal et une épaisseur uniforme.
Applications Claiming Priority (8)
Application Number | Priority Date | Filing Date | Title |
---|---|---|---|
CN201510070385.3 | 2015-02-11 | ||
CN201510070385.3A CN104599795B (zh) | 2015-02-11 | 2015-02-11 | 用于瓷或玻璃伞型、钟罩型绝缘子涂装rtv防污闪涂料的设备 |
CN201510076537.0 | 2015-02-13 | ||
CN201510076537.0A CN104637636B (zh) | 2015-02-13 | 2015-02-13 | 一种伞、钟罩状绝缘子rtv防污闪涂料的涂装方法 |
CN201520155701.2U CN204516521U (zh) | 2015-03-19 | 2015-03-19 | 绝缘子连接杆 |
CN201520155851.3 | 2015-03-19 | ||
CN201520155701.2 | 2015-03-19 | ||
CN201520155851.3U CN204516522U (zh) | 2015-03-19 | 2015-03-19 | 绝缘子浸涂机轴快接头 |
Publications (1)
Publication Number | Publication Date |
---|---|
WO2016127509A1 true WO2016127509A1 (fr) | 2016-08-18 |
Family
ID=56614150
Family Applications (2)
Application Number | Title | Priority Date | Filing Date |
---|---|---|---|
PCT/CN2015/078465 WO2016127509A1 (fr) | 2015-02-11 | 2015-05-07 | Procédé d'application de revêtement pour revêtement éclair anti-salissure rtv d'isolateur en forme de parapluie/cloche |
PCT/CN2015/078464 WO2016127508A1 (fr) | 2015-02-11 | 2015-05-07 | Dispositif de dépôt de revêtement d'embrasement éclair anti-salissure rtv sur des isolateurs de type ombrelle ou de type cloche en céramique ou en verre |
Family Applications After (1)
Application Number | Title | Priority Date | Filing Date |
---|---|---|---|
PCT/CN2015/078464 WO2016127508A1 (fr) | 2015-02-11 | 2015-05-07 | Dispositif de dépôt de revêtement d'embrasement éclair anti-salissure rtv sur des isolateurs de type ombrelle ou de type cloche en céramique ou en verre |
Country Status (1)
Country | Link |
---|---|
WO (2) | WO2016127509A1 (fr) |
Cited By (5)
Publication number | Priority date | Publication date | Assignee | Title |
---|---|---|---|---|
CN112337725A (zh) * | 2020-11-17 | 2021-02-09 | 辽宁华隆电力科技股份有限公司 | 一种绝缘子浸涂机 |
CN112967853A (zh) * | 2021-02-01 | 2021-06-15 | 徐宾 | 一种电力绝缘子表面涂层制作方法 |
CN113053599A (zh) * | 2021-03-19 | 2021-06-29 | 湖南工程学院 | 一种电气设备用绝缘元件自动加工设备 |
CN113171955A (zh) * | 2021-03-17 | 2021-07-27 | 平高集团有限公司 | 一种盆式绝缘子表面涂覆涂层固化装置 |
CN114405753A (zh) * | 2021-12-24 | 2022-04-29 | 黄启建 | 输电线路用防雷支柱绝缘子浸涂设备 |
Families Citing this family (2)
Publication number | Priority date | Publication date | Assignee | Title |
---|---|---|---|---|
CN106443393A (zh) * | 2016-11-17 | 2017-02-22 | 武汉大学 | 一种绝缘子模拟rtv涂层脱落的污闪试验方法 |
CN115171992B (zh) * | 2022-07-08 | 2024-08-13 | 山东大学 | 一种输电线路耐张绝缘子串带电喷涂机器人及工作方法 |
Citations (3)
Publication number | Priority date | Publication date | Assignee | Title |
---|---|---|---|---|
CN101340983A (zh) * | 2005-02-25 | 2009-01-07 | Csl硅树脂公司 | 使用硅氧烷组合物自动涂覆电气绝缘体的方法和装置 |
CN103545068A (zh) * | 2013-09-26 | 2014-01-29 | 国家电网公司 | 一种老化的合成绝缘子进行表面修复翻新的方法 |
CN103736645A (zh) * | 2013-12-02 | 2014-04-23 | 国网山西省电力公司晋中供电公司 | 涂有rtv防污闪涂料的绝缘子重新涂覆rtv防污闪涂料的方法 |
Family Cites Families (4)
Publication number | Priority date | Publication date | Assignee | Title |
---|---|---|---|---|
CN100998974B (zh) * | 2007-01-05 | 2012-07-04 | 福州大学 | 高压绝缘子表面涂层的喷涂工艺及喷涂装置 |
CN201586583U (zh) * | 2009-11-30 | 2010-09-22 | 浙江九天科技有限公司 | 空心复合绝缘子底涂自动喷涂机 |
CN103400668B (zh) * | 2013-07-29 | 2016-04-20 | 南方电网科学研究院有限责任公司 | 一种复合绝缘子旋转染污装置 |
CN104599795B (zh) * | 2015-02-11 | 2016-10-05 | 成都拓利科技股份有限公司 | 用于瓷或玻璃伞型、钟罩型绝缘子涂装rtv防污闪涂料的设备 |
-
2015
- 2015-05-07 WO PCT/CN2015/078465 patent/WO2016127509A1/fr active Application Filing
- 2015-05-07 WO PCT/CN2015/078464 patent/WO2016127508A1/fr active Application Filing
Patent Citations (3)
Publication number | Priority date | Publication date | Assignee | Title |
---|---|---|---|---|
CN101340983A (zh) * | 2005-02-25 | 2009-01-07 | Csl硅树脂公司 | 使用硅氧烷组合物自动涂覆电气绝缘体的方法和装置 |
CN103545068A (zh) * | 2013-09-26 | 2014-01-29 | 国家电网公司 | 一种老化的合成绝缘子进行表面修复翻新的方法 |
CN103736645A (zh) * | 2013-12-02 | 2014-04-23 | 国网山西省电力公司晋中供电公司 | 涂有rtv防污闪涂料的绝缘子重新涂覆rtv防污闪涂料的方法 |
Cited By (7)
Publication number | Priority date | Publication date | Assignee | Title |
---|---|---|---|---|
CN112337725A (zh) * | 2020-11-17 | 2021-02-09 | 辽宁华隆电力科技股份有限公司 | 一种绝缘子浸涂机 |
CN112967853A (zh) * | 2021-02-01 | 2021-06-15 | 徐宾 | 一种电力绝缘子表面涂层制作方法 |
CN112967853B (zh) * | 2021-02-01 | 2022-05-27 | 醴陵市永诚电瓷电器有限公司 | 一种电力绝缘子表面涂层制作方法 |
CN113171955A (zh) * | 2021-03-17 | 2021-07-27 | 平高集团有限公司 | 一种盆式绝缘子表面涂覆涂层固化装置 |
CN113053599A (zh) * | 2021-03-19 | 2021-06-29 | 湖南工程学院 | 一种电气设备用绝缘元件自动加工设备 |
CN113053599B (zh) * | 2021-03-19 | 2022-05-06 | 湖南工程学院 | 一种电气设备用绝缘元件自动加工设备 |
CN114405753A (zh) * | 2021-12-24 | 2022-04-29 | 黄启建 | 输电线路用防雷支柱绝缘子浸涂设备 |
Also Published As
Publication number | Publication date |
---|---|
WO2016127508A1 (fr) | 2016-08-18 |
Similar Documents
Publication | Publication Date | Title |
---|---|---|
WO2016127509A1 (fr) | Procédé d'application de revêtement pour revêtement éclair anti-salissure rtv d'isolateur en forme de parapluie/cloche | |
US10259372B2 (en) | Mobile-type power equipment maintenance device | |
CN206373015U (zh) | 一种自动化rtv浸涂环形流水线 | |
CN105529122B (zh) | 变电站支柱绝缘子rtv涂料喷涂工艺 | |
CN103736645B (zh) | 涂有rtv防污闪涂料的绝缘子重新涂覆rtv防污闪涂料的方法 | |
CN106700927A (zh) | 长效自洁防污涂料及其制备和使用方法 | |
CN106040551B (zh) | 用于支柱或套管的涂料涂覆方法及装置 | |
CN101358106A (zh) | 防覆冰纳米复合涂料及用途 | |
CN204516524U (zh) | 用于支柱绝缘子涂装rtv涂料的设备 | |
CN102875033A (zh) | 表面超快疏水处理的二氧化硅增透膜及其制备方法 | |
CN105562399A (zh) | 一种绝缘子自动清洗系统 | |
CN105080767A (zh) | 防污闪涂料变电站内现场工厂化喷涂装置 | |
CN108195516A (zh) | 车辆淋雨实验台及车辆淋雨试验台系统 | |
CN104119737A (zh) | 一种汽车用耐磨涂料及其制备方法 | |
CN115725223A (zh) | 一种防覆冰疏水涂料和应用、防覆冰疏水涂层的制备方法 | |
CN104810121A (zh) | 一种支柱绝缘子rtv涂料的涂装方法 | |
CN104637636B (zh) | 一种伞、钟罩状绝缘子rtv防污闪涂料的涂装方法 | |
CN114871033B (zh) | 一种在役风电塔筒外壁防护层现场自动再制造系统与方法 | |
CN110107137A (zh) | 一种具有天线保护功能的通讯铁塔 | |
CN105602301B (zh) | 瓷绝缘子用无机憎水防污釉料及其制备方法和应用 | |
CN209715457U (zh) | 一种复合绝缘子的喷雾系统 | |
CN106862002A (zh) | 一种单轴四联动柱式绝缘子常温rtv浸涂设备 | |
CN204735383U (zh) | 一种用于prtv和rtv涂料的喷涂设备 | |
CN106893442A (zh) | 一种透明的纳米二氧化硅-环氧树脂防腐涂料及制备方法 | |
CN107859291A (zh) | 一种自动刷漆装置及其应用 |
Legal Events
Date | Code | Title | Description |
---|---|---|---|
121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 15881670 Country of ref document: EP Kind code of ref document: A1 |
|
NENP | Non-entry into the national phase |
Ref country code: DE |
|
122 | Ep: pct application non-entry in european phase |
Ref document number: 15881670 Country of ref document: EP Kind code of ref document: A1 |