WO2001050558A1 - Group iii-nitride semiconductor structures with reduced phase separation - Google Patents
Group iii-nitride semiconductor structures with reduced phase separation Download PDFInfo
- Publication number
- WO2001050558A1 WO2001050558A1 PCT/IB2000/001836 IB0001836W WO0150558A1 WO 2001050558 A1 WO2001050558 A1 WO 2001050558A1 IB 0001836 W IB0001836 W IB 0001836W WO 0150558 A1 WO0150558 A1 WO 0150558A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- content
- layer
- conduction type
- cladding layer
- gan
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- H—ELECTRICITY
- H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
- H10H—INORGANIC LIGHT-EMITTING SEMICONDUCTOR DEVICES HAVING POTENTIAL BARRIERS
- H10H20/00—Individual inorganic light-emitting semiconductor devices having potential barriers, e.g. light-emitting diodes [LED]
- H10H20/80—Constructional details
- H10H20/81—Bodies
- H10H20/822—Materials of the light-emitting regions
- H10H20/824—Materials of the light-emitting regions comprising only Group III-V materials, e.g. GaP
- H10H20/825—Materials of the light-emitting regions comprising only Group III-V materials, e.g. GaP containing nitrogen, e.g. GaN
Definitions
- This application relates to semiconductor structures and processes, and particularly relates to group Ill-nitride quaternary and pentenary materials systems and methods such as might be used in blue or ultraviolet laser diodes and other similar semiconductors.
- Figure 1 shows a cross sectional illustration of a prior art semiconductor laser devices.
- GaN gallium nitride
- SiO 2 silicon dioxide
- an n-type GaN layer 30, an n-type indium gallium nitride (ln 0 .,Ga 09 N) layer 35, an n-type aluminum gallium nitride (Al 0 14 Ga 0 86 N)/GaN MD-SLS (Modulation Doped Strained-Layer Superlattices) cladding layer 40, and an n-type GaN cladding layer 45 are formed.
- an ln 002 Ga 098 N/ln 0 15 Ga 085 N MQW (Multiple Quantum Well) active layer 50 is formed followed by a p-type AI 02 Ga 0 ⁇ N cladding layer 55, a p-type GaN cladding layer 60, a p-type Al 0 1 4 Ga 086 N/GaN MD- SLS cladding layer 65, and a p-type GaN cladding layer 70.
- a ridge stripe structure is formed in the p-type Al 01 4 Ga 086 N/GaN MD-SLS cladding layer 55 to confine the
- Electrodes are formed on the p-type GaN cladding layer 70 and n-type GaN cladding layer 30 to provide current injection.
- the n-type GaN cladding layer 45 and the p-type GaN 60 cladding layer are light-guiding layers.
- the n-type Al 0 ., 4 Ga 086 N/GaN MD-SLS cladding layer 40 and the p-type AI 0 1 4 Ga 086 N/GaN MD-SLS cladding layer 65 act as cladding layers for confinement of the carriers and the light emitted from the active region ofthe InGaN MQW layer 50.
- the n-type ln 0 ⁇ a ⁇ N layer 35 serves as a buffer layer for the thick AIGaN film growth to prevent cracking.
- the optical field is confined in the active layer in the transverse direction by the n-type GaN cladding layer 45, the n-type AI 0 14 Ga 086 N/GaN MD-SLS cladding layers 40, the p-type GaN cladding layer 60, and the p-type AI 0.14 Ga 0 .
- the lattice constants of AIGaN, InGaN, and GaN differ sufficiently different from each other that defects are generated in the structure as a way to release the strain energy whenever the total thickness ofthe n-type ln 0 ⁇ Ga 09 N layer 35, the ln 002 Ga 0.98 N/ln 0 15 Ga ⁇ 85 N MQW active layer 50, the n-type Al 0 14 Ga 086 N/GaN MD-SLS cladding layer 40, the p-type AI 0 14 Ga 086 N/GaN MD-SLS cladding layer 65, and the p-type AI 02 Ga 08 N cladding layer 55 exceeds the critical thickness.
- the defects result from phase separation and act as absorption centers for the lasing light, causing decreased light emission efficiency and increased threshold current. The result is that the operating current becomes large, which in turn causes reliability to suffer.
- the ternary alloy system of InGaN is used as an active layer in the structure shown in Figure 1.
- the band gap energy changes from 1.9 eV for InN to 3.5 eVfor GaN. Therefore, ultraviolet light which has an energy level higher than 3.5 eV cannot be obtained by using an InGaN active layer.
- ultraviolet light is attractive as a light source for the optical pick up device in, for example, higher density optical disc memory systems and other devices.
- the mismatch of lattice constants between InN, GaN, and AIN must be understood.
- phase separation is that In atoms, Ga atoms, and Al atoms in the InGaAIN layers are not distributed uniformly according to the atomic mole fraction in each constituent layer. In turn, this means the band gap energy distribution of any layer which includes phase separation also becomes inhomogeneous. The band gap region ofthe phase separated portion acts disproportionately as an optical absorption center or causes optical scattering for the waveguided light. As noted above, a typical prior art solution to these problems has been to increase drive current, thus reducing the life of the semiconductor device.
- the present invention substantially overcomes the limitations of the prior art by providing semiconductor structures and methods which substantially reduce defect densities by materially reducing phase separation between the layers of the structures. This in turn permits substantially improved emission efficiency.
- the present invention utilizes group Ill-nitride quaternary and pentenary material systems and methods which may generally be described by the formula ln 1 . x . y Ga x Al y N 1 . z P z , where x, y and z are not all zero. It will be appreciated that, where one of x, y or z is zero, a quaternary system results. However, if none of x, y or z are zero, and the sum of x and y does not total one, a pentenary material system results.
- a GaAINP quaternary material system in accordance with the present invention, sufficient homogeneity to avoid phase separation has been found when the Al content, represented by x, and the P content, represented by y, ideally satisfy the condition that 3.18(1 -x)(1-y)+3.86(1- x)y+3.11x(1-y)+3.85xy nearly equals to a constant value.
- the constant value may be 3.18.
- a device typically includes a first layer of GaAINP material of a first conductivity, a GaAINP active layer, and a layer of GaAINP material of an opposite conductivity successively formed on one another.
- the semiconductor structure is fabricated essentially as above, using a quaternary materials system to eliminate phase separation and promote homogeneity across the layer boundaries.
- the first cladding layer is a first conduction type and composition of GaAINP
- the active layer is GaAINP of a second composition
- the second cladding layer is an opposite conduction type of GaAINP having the composition of the first layer.
- the second cladding layer has a ridge structure.
- the semiconductor structure comprises a first cladding of a first conduction type of an Ga 1 . x1 Al x1 N 1 . y1 P y1 material, an active layer of an Ga ⁇ AI ⁇ N.,. y2 P y2 material, and a second cladding layer of an opposite conduction type of an material, each successively formed on the prior layer.
- x1 , x2, and x3 define the Al content
- y1 , y2, and y3 define the P content.
- this materials system permits reduction of the optical absorption loss and the waveguide scattering loss, resulting in a high efficiency light emitting device.
- One of the benefits of the foregoing structure is to reduce the threshold current density of a laser diode. This can be achieved by use of a single or multiple quantum well structure, which reduces the density of the states of the active layer. This causes the carrier density necessary for population inversion to become smaller, leading to a reduced or low threshold current density laser diode. It is preferred that in the third light emitting device, the condition of 3.18(1- xs)(1-ys)+3.86(1-xs)ys+3.11xs(1-ys)+3.85xsys nearly equals to a constant value - on the order of or near 3.18 - is satisfied, wherein xs and ys are the Al content and the P content, respectively, in each the constituent layers. As before, this causes the lattice constants of the each constituent layers to be nearly equal to each other, which in turn substantially minimizes defects due to phase separation.
- the semiconductor structure may comprise a first cladding layer of a first conduction type of a material Ga ⁇ AI ⁇ N ⁇ P ⁇ , a Ga ⁇ AI ⁇ N ⁇ P ⁇ active layer, and a second cladding layer of an opposite conduction type of a material Ga ⁇ .
- x3 A ⁇ x3 ⁇ _ y3 P y3 each successively formed one upon the prior layer.
- the second cladding layer has a ridge structure.
- x1 , x2, and x3 define the Al content
- y1 , y2, and y3 define the As content
- InN is also attractive for the application to visible light emitting devices, visible light detectors, and high power transistor devices because of its relativlely wide band gap and direct band gap.
- the same structural design concepts for GaAINAs material are also can be applied to the semocinductor devices using the other material systems such as InGaNP, AllnNP.
- Figure 1 shows a prior art laser diode structure using a conventional ternary materials system.
- Figure 2 shows in cross-sectional view a semiconductor structure according to a first embodiment of the invention.
- Figure 3 shows a graph of the light-current characteristics of a laser diode according to the structure of Figure 1.
- Figure 4 shows an exemplary series of the fabrication steps for a semiconductor structure in accordance with a first embodiment of the invention.
- Figure 5 shows in cross-sectional view a semiconductor structure according to a second embodiment.
- Figure 6 shows a graph of the light-current characteristics of a laser diode according to the structure of Figure 4.
- Figure 7 shows an exemplary series of the fabrication steps for a semiconductor structure in accordance with the first embodiment of the invention.
- Figure 8 is a cross-sectional illustration of a semiconductor laser diode of the third embodiment.
- Figure 9 shows the light-current characteristics of the laser diode of the third embodiment.
- Figure 10 shows a series of the fabrication steps of a semiconductor laser diode in one experiment example of the third embodiment.
- Figure 11 is a cross-sectional illustration of a semiconductor laser diode of the fourth embodiment.
- Figure 12 shows the light-current characteristics of the laser diode of the fourth embodiment.
- Figure 13 shows a series of the fabrication steps of a semiconductor laser diode in one experiment example of the fourth embodiment.
- Figure 14 shows in plot form the boundary between the phase separation region and the region without phase separation at various growth temperatures.
- Figure 15 shows the content choice region of Ga content and P content in GaAINP to avoid phase separation at a growth temperature below approximately 1000 °C.
- Figure 16 shows the content choice line of Ga content and P content in
- GaAINP to avoid phase separation at a growth temperature below approximately 1000 °C which, at the same time, creates a lattice constant of GaAINP substantially equivalent to that of GaN.
- FIGS 17A and 17B show representations of bipolar and FET transistors constructed in accordance with the materials system of the present invention.
- Figure 18 shows an implementation of the present invention as a phototransistor.
- Figure 19 shows an implementation of the present invention as a photodiode.
- Figure 20 shows in cross-sectional view a semiconductor structure according to a fifth embodiment of the invention.
- Figure 21 shows an exemplary series of the fabrication steps for a semiconductor structure in accordance with a fifth embodiment of the invention.
- Figure 22 shows in cross-sectional view a semiconductor structure according to a sixth embodiment.
- Figure 23 shows an exemplary series of the fabrication steps for a semiconductor structure in accordance with the fifth embodiment of the invention.
- Figure 24 shows in plot form the boundary between the phase separation region and the region without phase separation at various growth temperatures.
- Figure 25 shows the content choice region of Ga content and P content in
- InGaNP to avoid phase separation at a growth temperature below approximately 1000 °C.
- Figure 26 shows the content choice line of Ga content and P content in InGaNP to avoid phase separation at a growth temperature below approximately 1000 °C which, at the same time, creates a lattice constant of InGaNP substantially equivalent to that of GaN.
- Figures 27A and 27B show representations of bipolar and FET transistors constructed in accordance with the materials system of the present invention.
- Figure 28 shows an implementation of the present invention as a phototransistor.
- Figure 29 shows an implementation of the present invention as a photodiode.
- Figure 30 shows in cross-sectional view a semiconductor structure according to a seventh embodiment of the invention.
- Figure 31 shows an exemplary series of the fabrication steps for a semiconductor structure in accordance with a seventh embodiment of the invention.
- Figure 32 shows in cross-sectional view a semiconductor structure according to a eighth embodiment.
- Figure 33 shows an exemplary series of the fabrication steps for a semiconductor structure in accordance with the eighth embodiment of the invention.
- Figure 34 shows in plot form the boundary between the phase separation region and the region without phase separation at various growth temperatures.
- Figure 35 shows the content choice region of In content and P content in AllnNP to avoid phase separation at a growth temperature below approximately 1000 °C.
- Figures 36A and 36B show representations of bipolar and FET transistors constructed in accordance with the materials system of the present invention.
- Figure 37 shows an implementation of the present invention as a phototransistor.
- Figure 38 shows an implementation of the present invention as a photodiode.
- FIG. 2 shown therein in cross-sectional view is a semiconductor structure according to a first embodiment of the invention.
- the semiconductor structure shown in many of the Figures will be a laser diode, although the present invention has application to a number of device types.
- an n-type GaN substrate 100 is provided and an n-type GaN first cladding layer 105 (typically 0.5 ⁇ m thick) is formed thereon.
- a second cladding layer 110 typically of an n-type Ga 075 AI 025 N 099 P 001 material which may be on the order of 1.5 ⁇ m thick, is formed thereon, followed by a multiple quantum well active layer 115 which in an exemplary arrangement may comprise three quantum well layers of Ga 085 AI 0 15 N 097 P 0. o 3 material on the order of 35 A thick together with four barrier layers of Ga 08 Al 0.2 N 0.98 Po . o 2 material on the order of 35 A thick, arranged as three pairs.
- 25 N 0.99 P 0.01 (typically on the order of 1.5 ⁇ m thick) is formed, followed by a p-type GaN fifth cladding layer 125 (on the order of 0.5 ⁇ m thick).
- a SiO 2 layer 130 having one stripe like window region 135 (3.0 ⁇ m width) is formed on the p-type GaN fourth cladding layer 125.
- a first electrode 140 is formed on the n-type GaN substrate 100, while a second electrode 145 is formed on the SiO 2 layer 130 and the window region 135.
- the Al content, x, and the P content, y, of all the layers generally satisfies the condition 3.18(1-x)(1-y)+3.86(1-x)y+3.11x(1-y)+3T85xy nearly equals to a constant value, which may be on the order of 3.18 for at least the first embodiment.
- the lattice constants of the various constituent layers are matched to each other by setting the Al content, x, and the P content, y, in each of the layers to meet the condition 3.18(1-x)(1- y)+3.86(1-x)y+3.11x(1-y)+3.85xy nearly equals to a constant value, again, for the first embodiment on the order of 3.18+0.05 so that the equivalent lattice constants of each layers become nearly equal to the lattice constant of GaN.
- the band gap energy of the n-type second cladding layer 110 and the p-type third cladding layer 120 are larger than that of the 3 pairs of multiple quantum well active layers 115. This confines the injected carriers from the n-type second cladding layer 110 and p-type third cladding layer 120 within the active layer 115, where the carriers recombine to lead to the emission of ultraviolet light.
- the refractive index of the n-type second cladding layer 110 and the p-type third cladding layer 120 are smaller than that of the multiple quantum well active layer 115, which confines the optical field in the transverse direction.
- the region in the active layer 115 under the widow region 135 is activated strongly. This causes the local modal gain in the active layer under the window region 6a to be higher than the local modal gain in the active layer under the SiO 2 layer. Therefore, a gain guided waveguide mechanism, leading to a lasing oscillation, is able to be formed in the structure of the first embodiment.
- Figure 3 shows a plot of the emitted light versus drive current for a laser diode constructed in accordance with the first embodiment.
- the laser diode is driven with a pulsed current with a duty cycle of 1 %.
- the threshold current density is found to be 6.0 kA/cm 2 .
- Figures 4A-4D show, in sequence, a summary of the fabrication steps necessary to construct an exemplary laser diode according to the first embodiment. Since the structure which results from Figures 4A-4D will resemble that shown in Figure 2, like reference numerals will be used for elements whenever possible.
- an n-type GaN substrate 100 is provided, on which is grown an n-type GaN first cladding layer 105.
- the first cladding layer 105 is typically on the order of 0.5 ⁇ m thick.
- an n- type Ga 075 AI 0.25 N 0 .ggP 0.01 second cladding layer 110 is formed, typically on the order of 1.5 ⁇ m thick.
- a multiple quantum well active layer 115 is formed by creating three quantum wells comprised of three layers of Ga 8S Al ⁇ 5 N 97 P 0-03 material each on the order of 35 A thick, together with four barrier layers of Ga 0 . 8 Al 02 N 098 P 002 material on the order of 35 A thick.
- Each of the layers is typically formed by either the Metal Organic Chemical Vapor Deposition (MOCVD) method or the Molecular Beam Epitaxy (MBE) method.
- MOCVD Metal Organic Chemical Vapor Deposition
- MBE Molecular Beam Epitaxy
- a silicon dioxide (SiO 2 ) layer 130 is formed on the p-type GaN fourth cladding layer 125, for example by the Chemical Vapor Deposition (CVD) method.
- CVD Chemical Vapor Deposition
- a window region 135 is formed as shown in Figure 4C.
- the window region 135 may be stripe-like in at least some embodiments.
- a first electrode 140 and a second electrode 145 are formed on the n-type GaN substrate 100 and on the Si0 2 layer 130, respectively, by evaporation or any other suitable process.
- an exemplary application of the second embodiment is the creation of a laser diode.
- the structure of the second embodiment permits a waveguide mechanism to be built into the structure with a real refractive index guide. This provides a low threshold current laser diode which can operate with a fundamental transverse mode.
- a first cladding layer 105 is formed of an n-type GaN on the order of 0.5 ⁇ m thick.
- an n-type second cladding layer 110 is formed of Ga 075 AI 025 N 0 ggPo . o material on the order of 1.5 ⁇ m thick.
- a multiple quantum well active layer 115 is formed comprising three well layers of Ga 085 Al 0 15 N 097 P 0. o 3 material on the order of 35 A thick together with four barrier layers of Ga 08 Al ⁇ 2 N 098 P 0. o 2 material, also on the order of 35 A thick.
- a third, p-type cladding layer 120 formed of Ga 075 Alo 25 No. 99 Po.o ⁇ material on the order of 1.5 ⁇ m thick is formed.
- a p-type GaN fourth cladding layer 125 on the order of 0.5 ⁇ m thick is formed over the ridge structure 500 of the third cladding layer 120.
- the third and fourth cladding layers are then partially removed to create a ridge structure 500.
- a silicon dioxide (SiO 2 ) layer 130 is then formed over the fourth cladding layer 125 as well as the remaining exposed portion of the third cladding layer 120.
- a first electrode 140 is formed on the n-type GaN substrate 100 and a second electrode 145 is formed on the SiO 2 layer 130 and the window region 135.
- the Al content, x, and the P content, y, of the well layer is set to be 0.15, 0.03, respectively.
- the Al content, x, and the As content, y, of all the layers satisfies the condition 3.18(1-x)(1-y)+3.86(1-x)y+3.11x(1-y)+3.85xy nearly equals to a constant Value, which may for example be 3.18+0.05.
- the band gap energy of the cladding layers is maintained larger than the band gap energy for the active layer, allowing the emission of ultraviolet light.
- the refractive index of the materials is as discussed in connection with the first embodiment, permitting the optical field to be confined in the transverse direction. Similar to the operation of the first embodiment, the region of the active layer 115 under the window region 135 is activated strongly because of the constraints on the injected current by the SiO 2 layer. The result, again, is that the local modal gain in the active layer under the window region 135 is higher than the local modal gain in the active layer under the SiO 2 layer 130.
- the design of the second embodiment provides a low threshold current laser diode which can operate with a fundamental transverse mode.
- Figure 6 shows in graph form the emitted light versus drive current characteristics of a laser diode in accordance with the second embodiment.
- the laser diode is driven with a cw current.
- the threshold current is found to be 36 mA.
- the formation of the first and second cladding layers 105 and 110 on an n-type GaN substrate 100, together with the three-pair multiple quantum well active layer 115 are the same as for the first embodiment.
- the third and fourth cladding layers 120 and 125 are formed and then partially removed - typically by etching - to create a ridge structure 500.
- the various layers are formed successively by either the MOCVD or the MBE method.
- a silicon dioxide layer 130 is formed over the fifth and third cladding layers 125 and 120, respectively, typically by the CVD method, after which a window region 135 is formed as with the first embodiment. Electrodes 140 and 145 are then evaporated or otherwise bonded to the structure.
- a third embodiment of the present invention may be better appreciated.
- the third embodiment provides slightly different mole fractions to permit the emission of ultra violet light, but is otherwise similar to the first embodiment.
- an n-type GaN substrate 100 continues to be used, together with an n-type GaN first cladding layer 105.
- the second cladding layer 810 is typically of n-type Ga 0 . Alo .6 No .99 Po.o ⁇ material on the order of 1.5 ⁇ m thick
- the three-pair quantum well active layer 815 typically includes three well layers of Ga 07 AI 03 No .99 Po.o ⁇ material together with four barrier layers of Ga 06 AI 04 N 0.99 P 0.01 material.
- the third cladding layer 820 is typically a p-type Ga 0.4 Alo 6 N 0 g 9 Po . oi material, while the fourth cladding layer 125 is, like the first embodiment, a p-type GaN material.
- the thicknesses of each layer are substantially the same as for the first embodiment.
- a SiO 2 layer 130, window region 135, and first and second electrodes 140 and 145 complete the structure.
- the Al content and the P content within the well layer 815 is set to be 0.3 and 0.01 , respectively.
- the Al content, x, and the P content, y, of each of the layers is set to satisfy the condition 3.18(1-x)(1-y)+3.86(1-x)y+3.11x(1-y)+3.85xy nearly equals to a constant value.
- the constant value may be on the order of 3.18+0.05.
- the band gap energies of cladding layers continue to be set higher than the band gap energy of the three pairs of the multiple quantum well active layer 815.
- the refractive index of the second and third cladding layers is, by design, smaller than that of the active layer, causing the optical field to be confined in the transverse direction.
- the strong current injection under the window region 135 yields comparatively higher local modal gain in the active layer relative to the portion of the active layer under the SiO 2 layer 130, again resulting in a guided waveguide mechanism which leads to a lasing oscillation.
- Figure 9 shows a plot of the emitted light versus drive current characteristics of the laser diode in accordance with the third embodiment.
- the laser diode is driven with a pulsed current with a duty cycle of 1 %.
- the threshold current density is found to be 7 kA/cm 2 .
- Figures 10A-10D show a series of the fabrication steps of a semiconductor laser diode in one example of the third embodiment. It will be appreciated that the fabrication steps are the same as those described in connection with Figures 4A- 4D, and therefore are not further described.
- a fourth embodiment of the present invention may be better appreciated.
- the fourth embodiment like the third embodiment, is designed to emit ultra violet light and therefore has the same Al and P content as the third embodiment. However, like the second embodiment, the fourth embodiment is configured to provide a ridge structure to serve as a waveguide. Because the Al and P content is similar to that of Figure 8, similar elements will be described with the reference numerals used in Figure 8.
- the structure of the fourth embodiment can be seen to have a GaN substrate 100 on which is a formed a first cladding layer 105 followed by a second cladding layer 810.
- a three-pair multiple quantum well active layer 815 is formed thereabove, followed by a third cladding layer 820.
- a fourth cladding layer 125, silicon dioxide layer 130, windows 135 and electrodes 140 and 145 are all formed as before.
- the Al content , , and the P content, y, of the layers is set to satisfy the condition 3.18(1 -x)(1-y)+3.86(1- x)y+3.11x(1-y)+3.85xy nearly equals to a constant value on the order of 3.18+0.05, as with the third embodiment.
- the band gap energy, refractive index and modal gain for current injection are all substantially as discussed in connection with the third embodiment and are not further discussed.
- Figure 12 plots drive current versus emitted light of a laser diode constructed in accordance with the fourth embodiment.
- the laser diode is driven with a cw current.
- the threshold current is found to be 40 mA.
- Figure 13 shows a summary of the fabrication steps of a semiconductor laser diode in accordance with the fourth embodiment. The steps are essentially identical to those discussed in connection with Figures 7A-7E and are not further discussed.
- the selection of the Al content, x, and the P content, y, and the relationship therebetween for the constituent GaAINP layers may be better understood.
- the lattice constant of GaN, AIN, GaP and AIP are different from each other.
- the lattice mismatch between GaN and GaP, between AIN and AIP, and between GaN and AIN, are 21.2%, 23.9%, and 2.3%o, respectively. Therefore, an internal strain energy is accumulated in GaAINP layer, even if the equivalent lattice constant is the same as that of the substrate due to the fact that equivalent bond length are different from each other between GaN, AIN, GaP and AIP.
- Figure 14 shows the boundary of phase separation region plotted against various growth temperatures. The lines in Figure 14 show the boundary between the compositionally unstable (phase separation) region and stable region with respect to various temperatures.
- phase separation occurs, Ga atoms, Al atoms, N atoms, and P atoms in the GaAINP layers are not distributed uniformly according to the atomic content in each constituent layer. Stated differently, the band gap energy distribution of the phase separated layer also becomes inhomogeneous in the layer. The region of the relatively small band gap region in the phase separated layer acts as an optical absorption center, or causes an optical scattering for the waveguided light. This means that the phase separation phenomena should be avoided to obtain a high efficiency light emitting device. Referring still to Figure 14, it can be seen that the phase separation region varies with temperature. The lines in Fig. 14 show the boundary between the compositionally unstable region - that is, resulting in phase separation - and the stable region with respect to various temperatures.
- the region surrounded with the GaP-GaN line, AIP-AIN line and the boundary line shows the phase separation content region. It has been discovered that the ternary alloys AINP and GaNP have a large phase separation region due to the large lattice mismatch between AIN and AIP, and between GaN and GaP. On the other hand, it has been found that the ternary alloys GaAIN and GaAIP have no phase separation region at crystal growth temperatures around 1000 °C, due to the small lattice mismatch between AIN and GaN, and between AIP and GaP.
- an GaAINP material system can be provided in which the usual crystal growth temperature is in the approximate range of around 600 °C to around 1000°C.
- phase separation of the Al content and P content of GaAINP does not occur in significant amounts at processing temperatures between on the order of 600 °C and on the order of 1000 °C.
- the result is the substantially uniform distribution of Ga atoms, Al atoms, N atoms and P atoms in each constituent layer according to the atomic mole fraction.
- Figure 16 shows the content choice line of Al content, x, and P content, y, in an GaAINP system to avoid the phase separation phenomenon at growth temperatures below around 1000 °C and still ensure a reasonable lattice match to GaN.
- Group-Ill nitride materials are promising for use in electronic devices which can operate under high-power and high-temperature conditions - for example, microwave power transistors. This results, in part, from their wide band gap (3.5 eV for GaN and 6.2 eV for AIN), high breakdown electronic field, and high saturation velocity.
- the band gaps of AIAs, GaAs, and Si are 2.16 eV, 1.42 eV, and 1.12 eV, respectively. This has led to significant research in the use of AIGaN/GaN materials for such field effect transistors (FETs).
- the different lattice constants of AlGaN and GaN cause the generate of significant defects, limiting the mobility of electrons in the resultant structure and the utility of such materials systems for FET use.
- the present invention substantially overcomes these limitations, in that the
- GaAINP/GaN material of the present invention has a lattice constant equal to GaN.
- FIG. 17A there is shown therein an exemplary embodiment of a heterojunction field effect transistor(HFET) using GaAINP/GaN material in accordance with the present invention.
- HFET heterojunction field effect transistor
- a GaN substrate 520 On a GaN substrate 520, a 0.5 ⁇ m i-GaN layer 525 is formed, followed by a thin, approximately 10 nm GaN conducting channel layer 530 and a 10 nm GaAINP layer 535.
- Source and drain electrodes 540A-B, and gate electrode 545 are formed in a conventional manner.
- the Al content, x, and P content, y, of the GaAINP layer are set to be 0.25 and 0.01 , respectively.
- this permits high electron velocities to be achieved because the two dimensional electron gas formed in the heterointerface of GaAINP and GaN layer is not scattered by any fluctuation in atomic content of the GaAINP layer (such as would be caused in the presence of defects).
- the band gap of the GaAINP is larger than 4 eV so that reliable high-temperature operation can be achieved by using the structure shown in Figure 17A.
- Figure 17B shows an embodiment of a heterojunction bipolar transistor(HBT) in accordance with the present invention.
- HBT heterojunction bipolar transistor
- a 400 nm thick n-type GaAINP collector layer 555 is formed, followed by a 50 nm thick p-type GaN base layer 560, and a 300 nm thick n-type GaAINP emitter layer 565.
- Base electrode 570, collector electrode 575 and emitter electrode 580 are formed conventionally.
- the Al and P contents x and y of the GaAINP layer are set to be 0.25, 0.01 , respectively, and x and y are required to satisfy the same relationships as discussed above.
- an GaAINP layer without significant phase separation and with a lattice constant equal to GaN is realized, resulting in a very high quality heterojunction of GaAINP/GaN.
- the band gap of the GaAINP emitter layer (4 eV) is larger than that of GaN base layer (3.5eV) so that holes generated in the p-type base layer are well confined in that base layer. This results because of the larger valence band discontinuity between GaN and
- GaAINP than would occur in a GaN homojunction bipolar transistor. This has the benefit of obtaining a large current amplification of collector current relative to base current. Moreover, as mentioned above, the bandgap of the GaAINP and the GaN layer is large so that the transistor can be used reliably in high- temperature applications.
- GaN and AlGaN are attractive materials for photo detectors in ultraviolet(UV) range, since both GaN and AIN have a wide band gap (3.5 eV for GaN which corresponds to the light wavelength of 200 nm, 6.2 eV for AIN which corresponds to the light wavelength of 350 nm). Due to the direct band gap and the availability of AlGaN in the entire AIN alloy composition range, AIGaN/GaN based UV photo detectors have the advantage of high quantum efficiency, as well as tunability of high cut-off wavelength.
- the Ga ⁇ x A N ⁇ P y quaternary material whose Al content, x and P content, y satisfy the relationship of 3.18(1-x)(1-y)+3.86(1-x)y+3.11x(1-y)+3.85xy 3.18 has a lattice constant equal to GaN and a bandgap larger than 3.5eV. Therefore, by using GaAINP/GaN material whose Al content, x and P content, y satisfy the above relationship, UV photo detectors with low defect density can be realized. In the event that detection of other frequencies is desired, for example blue light, only slight modification is required.
- the semiconductor device of the present invention can be implemented as a heterojunction phototransistor(HPT) using GaAINP/GaN material.
- a GaAINP collector layer 705 is formed on the order of 500 nm thick n-type, followed by the formation of a 200 nm thick p- type GaN base layer 710.
- a GaAINP emitter layer 715 is formed on the order of 500 nm thick.
- a ring shaped electrode 720 is formed to permit light to impinge on the base layer.
- the Al content, x and P content, y of the GaAINP layer are set to be 0.25 and 0.01 , respectively.
- the band gap of the GaAINP emitter layer (4 eV which corresponds to the light wavelength of 307 nm) is larger than that of GaN base layer (3.5eV which corresponds to the light wavelength of 350 nm).
- the light impinges on the emitter side.
- impinging light in the wavelength range between 307 nm and 350 nm is transparent to the emitter layer, so that the light in that range is absorbed in the GaN base layer and generates electron and hole pairs.
- the holes generated by the optical absorption in the p- type base layer are well confined in the base layer because the valence band discontinuity between GaN and GaAINP is larger than that for a conventional GaN homojunction photo transistor.
- the GaN base layer may be replaced with, for example for blue light, InGaN.
- an n-type substrate 900 is provided, on which is formed an n-type layer 910 of quaternary material or equivalent, which conforms to the relationships discussed above in connection with Figure 18.
- An active layer 915 is thereafter formed, and above that is formed a layer 920 of p-type Ga ⁇ ⁇ Al ⁇ N ⁇ - y P y quaternary material.
- a p-type second cladding layer 925 is formed above the layer 920, and a window 930 is formed therein to expose a portion of the layer 920.
- the window 930 provides a port by which light can impinge on the layer 920, causing the creation of holes.
- a pair of electrodes 935 and 940 may be fabricated in a conventional manner, with the electrode 935 typically being a ring electrode around the window 930.
- the band gap of the second cladding layer 925 is preferably larger than the band gap of the layer 920, which is in turn preferably larger than the band gap of the active Iayer915; such an approach provides sensitivity to the widest range of wavelength of light.
- a material with a lower band gap than the layer 920 may be used for the layer 925.
- FIG. 20 shown therein in cross-sectional view is a semiconductor structure according to a fifth embodiment of the invention.
- the semiconductor structure shown in many of the Figures will be a laser diode, although the present invention has application to a number of device types.
- an n-type GaN substrate 200 is provided and an n-type GaN first cladding layer 205 (typically 0.5 ⁇ m thick) is formed thereon.
- a second cladding layer 210 typically of an n-type ln 0 oo ⁇ Ga 099 gN 0999 P 0 oo ⁇ material which may be on the order of 1.5 ⁇ m thick, is formed thereon, followed by a multiple quantum well active layer 215 which in an exemplary arrangement may comprise three quantum well layers of ln 0 o ⁇ Ga 099 N 0 g 7 Po . o 3 material on the order of 35 A thick together with four barrier layers of lno .001 Gao .999 No .97 5Po .025 material on the order of 35 A thick, arranged as three pairs.
- a third cladding layer 220 of a p-type ln 0001 Ga 0999 N 0999 P 0001 (typically on the order of 1.5 ⁇ m thick) is formed, followed by a p-type GaN fifth cladding layer 225 (on the order of 0.5 ⁇ m thick).
- a first electrode 240 is formed on the n-type GaN substrate 200, while a second electrode 245 is formed on the SiO 2 layer 230 and the window region 235.
- the Ga content, x, and the As content, y, of all the layers generally satisfies the condition 3.54(1-x)(1-y)+4.15(1-x)y+3.18x(1-y)+3.86xy nearly equals to a constant value, which may be on the order of 3.18 for at least the fifth embodiment.
- the lattice constants of the various constituent layers are matched to each other by setting the Ga content, x, and the P content, y, in each of the layers to meet the condition 3.54(1-x)(1-y)+4.15(1-x)y+3.18x(1-y)+3.86xy nearly equals to a constant value, again, for the fifth embodiment on the order of 3.18+0.05 so that the equivalent lattice constants of each layers become nearly equal to the lattice constant of GaN.
- the band gap energy of the n-type second cladding layer 210 and the p-type third cladding layer 220 are larger than that of the 3 pairs of multiple quantum well active layers 215. This confines the injected carriers from the n-type second cladding layer 210 and p-type third cladding layer 220 within the active layer 215, where the carriers recombine to lead to the emission of blue light.
- the refractive index of the n-type second cladding layer 210 and the p-type third cladding layer 220 are smaller than that of the multiple quantum well active layer 215, which confines the optical field in the transverse direction.
- the region in the active layer 215 under the widow region 235 is activated strongly. This causes the local modal gain in the active layer, under the window region to be higher than the local modal gain in the active layer under the SiO 2 layer. Therefore, a gain guided waveguide mechanism, leading to a lasing oscillation, is able to be formed in the structure of the first embodiment.
- Figures 21A-21 D show, in sequence, a summary of the fabrication steps necessary to construct an exemplary laser diode according to the fifth embodiment. Since the structure which results from Figures 21A-21D will resemble that shown in Figure 20, like reference numerals will be used for elements whenever possible.
- an n-type GaN substrate 200 is provided, on which is grown an n-type GaN first cladding layer 205.
- the first cladding layer 205 is typically on the order of 0.5 ⁇ m thick.
- an n-type lno. 001 Gao .999 No. 999 Po .001 second cladding layer 210 is formed, typically on the order of 1.5 ⁇ m thick.
- a multiple quantum well active layer 215 is formed by creating three quantum wells comprised of three layers of ln 0 .o ⁇ Ga 0 g 9 097 Poo 3 material each on the order of 35 A thick, together with four barrier layers of ln 0001 Ga 09 g 9 N 0.975 P 0025 material on the order of 35 A thick.
- Each of the layers is typically formed by either the Metal Organic Chemical Vapor Deposition (MOCVD) method or the Molecular Beam Epitaxy (MBE) method.
- MOCVD Metal Organic Chemical Vapor Deposition
- MBE Molecular Beam Epitaxy
- a silicon dioxide (SiO 2 ) layer 230 is formed on the p-type GaN fourth cladding layer 225, for example by the Chemical Vapor Deposition (CVD) method.
- CVD Chemical Vapor Deposition
- a window region 235 is formed as shown in Figure 21 C.
- the window region 235 may be stripe-like in at least some embodiments.
- a first electrode 240 and a second electrode 245 are formed on the n-type GaN substrate 200 and on the SiO 2 layer 230, respectively, by evaporation or any other suitable process.
- a sixth embodiment of a semiconductor structure in accordance with the present invention may be better appreciated.
- an exemplary application of the sixth embodiment is the creation of a laser diode.
- the structure of the sixth embodiment permits a waveguide mechanism to be built into the structure with a real refractive index guide. This provides a low threshold current laser diode which can operate with a fundamental transverse mode.
- a first cladding layer 205 is formed of an n-type GaN on the order of 0.5 ⁇ m thick.
- an n-type second cladding layer 210 is formed of ln oo1 Ga ⁇ 999 N 0-999 P ⁇ oo ⁇ material on the order of 1.5 ⁇ m thick.
- a multiple quantum well active layer 215 is formed comprising three well layers of ln 00 ⁇ Ga 099 N 097 P 003 material on the order of 35 A thick together with four barrier layers of ln 001 Ga 0 . 999 N 0 .
- a third, p-type cladding layer 220 formed of ln 0.0 o ⁇ Ga 0.999 N 999 P 0.001 material on the order of 1.5 ⁇ m thick is formed.
- a p-type GaN fourth cladding layer 225 on the order of 0.5 ⁇ m thick is formed over the ridge structure 1500 of the third cladding layer 220.
- the third and fourth cladding layers are then partially removed to create a ridge structure 1500.
- a silicon dioxide (SiO 2 ) layer 230 is then formed over the fourth cladding layer 225 as well as the remaining exposed portion of the third cladding layer 220.
- a window region 235 which may be stripelike on the order of 2.0+m width, is formed through the SiO 2 layer above the fourth and third cladding layers 225 and 220, respectively.
- a first electrode 240 is formed on the n-type GaN substrate 200 and a second electrode 245 is formed on the SiO 2 layer 230 and the window region 235.
- the Ga content, x, and the P content, y, of the well layer is set to be 0.99, 0.03, respectively.
- the Ga content, x, and the P content, y, of all the layers satisfies the condition 3.54(1-x)(1-y)+4.15(1-x)y+3.18x(1-y)+3.86xy nearly equals to a constant value, which may for example be 3.18+0.05.
- the band gap energy of the cladding layers is maintained larger than the band gap energy for the active layer, allowing the emission of blue light.
- the refractive index of the materials is as discussed in connection with the fifth embodiment, permitting the optical field to be confined in the transverse direction.
- the region of the active layer 215 under the window region 235 is activated strongly because of the constraints on the injected current by the SiO 2 layer.
- the result, again, is that the local modal gain in the active layer under the window region 235 is higher than the local modal gain in the active layer under the SiO 2 layer 230.
- the formation of the first and second cladding layers 205 and 210 on an n-type GaN substrate 200, together with the three-pair multiple quantum well active layer 215 are the same as for the fifth embodiment.
- the third and fourth cladding layers 220 and 225 are formed and then partially removed - typically by etching - to create a ridge structure 1500.
- the various layers are formed successively by either the MOCVD or the MBE method.
- a silicon dioxide layer 230 is formed over the fifth and third cladding layers 225 and 220, respectively, typically by the CVD method, after which a window region 235 is formed as with the fifth embodiment. Electrodes 240 and 245 are then evaporated or otherwise bonded to the structure.
- the selection of the Ga content, x, and the P content, y, and the relationship therebetween for the constituent InGaNP layers may be better understood.
- the lattice constant of GaN, InN, GaP and InP are different from each other.
- the lattice mismatch between GaN and GaP, between InN and InP, and between GaN and InN are 21.2%, 17.2%, and 10.2%o, respectively. Therefore, an internal strain energy is accumulated in InGaNP layer, even if the equivalent lattice constant is the same as that of the substrate due to the fact that equivalent bond length are different from each other between GaN, InN, GaP and InP.
- Figure 24 shows the boundary of phase separation region plotted against various growth temperatures. The lines in Figure 24 show the boundary between the compositionally unstable (phase separation) region and stable region with respect to various temperatures.
- Ga atoms, In atoms, N atoms, and P atoms in the InGaNP layers are not distributed uniformly according to the atomic content in each constituent layer. Stated differently, the band gap energy distribution of the phase separated layer also becomes inhomogeneous in the layer. The region of the relatively small band gap region in the phase separated layer acts as an optical absorption center, or causes an optical scattering for the waveguided light. This means that the phase separation phenomena should be avoided to obtain a high efficiency light emitting device.
- the phase separation region varies with temperature.
- the lines in Fig. 24 show the boundary between the compositionally unstable region - that is, resulting in phase separation - and the stable region with respect to various temperatures.
- the region surrounded with the InP-lnN line, GaP-GaN line, and the boundary line shows the phase separation content region.
- the ternary alloys InNP, InGaN, and GaNP have a large phase separation region due to the large lattice mismatch between InN and InP, between InN and GaN, and between GaN and GaP.
- the ternary alloys InGaP have no phase separation region at crystal growth temperatures around 1000 °C, due to the relatively small lattice mismatch between InP and GaP.
- an InGaNP material system can be provided in which the usual crystal growth temperature is in the approximate range of around 600 °C to around 1000°C.
- phase separation of the Ga content and P content of InGaNP does not occur in significant amounts at processing temperatures between on the order of 600 °C and on the order of 1000 °C.
- the result is the substantially uniform distribution of Ga atoms, In atoms, N atoms and P atoms in each constituent layer according to the atomic mole fraction.
- Figure 26 shows the content choice line of Ga content, x, and P content, y, in an InGaNP system to avoid the phase separation phenomenon at growth temperatures below around 1000 °C and still ensure a reasonable lattice match to GaN.
- Group-Ill nitride materials are promising for use in electronic devices which can operate under high-power and high-temperature conditions - for example, microwave power transistors. This results, in part, from their wide band gap (3.5 eV for GaN and 6.2 eV for AIN), high breakdown electronic field, and high saturation velocity.
- the band gaps of AIAs, GaAs, and Si are 2.16 eV, 1.42 eV, and 1.12 eV, respectively.
- FETs field effect transistors
- the different lattice constants of AlGaN and GaN cause the generate of significant defects, limiting the mobility of electrons in the resultant structure and the utility of such materials systems for FET use.
- the present invention substantially overcomes these limitations, in that the InGaNP/GaN material of the present invention has a lattice constant equal to GaN.
- FIG. 27A there is shown therein an exemplary embodiment of a heterojunction field effect transistor(HFET) using InGaNP/GaN material in accordance with the present invention.
- HFET heterojunction field effect transistor
- a GaN substrate 1520 On a GaN substrate 1520, a 0.5 ⁇ m i- InGaNP layer 1525 is formed, followed by a thin, approximately 10 nm InGaNP conducting channel layer 1530 and a 10 nm GaN layer 1535.
- Source and drain electrodes 1540A-B, and gate electrode 1545 are formed in a conventional manner.ln the structure, the Ga content, x, and P content, y, of the InGaNP layer are set to be 0.999 and 0.025, respectively.
- the band gap of the InGaNP is larger than 3 eV so that reliable high-temperature operation can be achieved by using the structure shown in Figure 27A.
- Figure 27B shows an embodiment of a heterojunction bipolar transistor(HBT) in accordance with the present invention.
- HBT heterojunction bipolar transistor
- a 400 nm thick n-type GaN collector layer 1555 is formed, followed by a 50 nm thick p-type InGaNP base layer 1560, and a 300 nm thick n-type GaN emitter layer 1565.
- Base electrode 1570, collector electrode 1575 and emitter electrode 1580 are formed conventionally.
- the Ga and P contents x and y of the InGaNP layer are set to be 0.999, 0.025, respectively, and x and y are required to satisfy the same relationships as discussed above.
- an InGaNP layer without significant phase separation and with a lattice constant equal to GaN is realized, resulting in a very high quality heterojunction of InGaNP/GaN.
- the band gap of the GaN emitter layer (3.5 eV) is larger than that of InGaNP base layer (3 eV) so that holes generated in the p-type base layer are well confined in that base layer. This results because of the larger valence band discontinuity between GaN and InGaNP than would occur in a GaN homojunction bipolar transistor. This has the benefit of obtaining a large current amplification of collector current relative to base current.
- the bandgap of the InGaNP and the GaN layer is large so that the transistor can be used reliably in high-temperature applications.
- GaN and InGaN are attractive materials for photo detectors in visible light range, since both GaN and InN have a wide band gap (3.5 eV for GaN which corresponds to the light wavelength of 350 nm, 1.9 eV for InN which corresponds to the light wavelength of 650 nm). Due to the direct band gap and the availability of InGaN in the entire InN alloy composition range, InGaN/GaN based visible light photo detectors have the advantage of high quantum efficiency, as well as tunability of high cut-off wavelength.
- the lattice constant of InGaN is sufficiently different from GaN that defects tend to be formed, which leads increased leakage current.
- the ln ⁇ _ x Ga x N ⁇ offers not only a band gap larger than 2.7 eV, but also can be fabricated in layers with equal atomic content distribution, so that InGaNP material also can be used for visible light photo detector applications.
- the ln ⁇ _ x Ga x N ⁇ offers not only a band gap larger than 2.7 eV, but also can be fabricated in layers with equal atomic content
- the semiconductor device of the present invention can be implemented as a heterojunction phototransistor(HPT) using InGaNP/GaN material.
- a GaN collector layer 1705 is formed on the order of 500 nm thick n-type, followed by the formation of a 200 nm thick p- type InGaNP base layer 1710.
- a InGaNP emitter layer 1715 is formed on the order of 500 nm thick.
- a ring shaped electrode 1720 is formed to permit light to impinge on the base layer.
- the Ga content, x and P content, y of the InGaNP layer are set to be 0.999 and 0.025, respectively.
- the band gap of the GaN emitter layer (3.5 eV which corresponds to the light wavelength of 350 nm) is larger than that of InGaNP base layer (3 eV which corresponds to the light wavelength of 410 nm).
- the light impinges on the emitter side.
- impinging light in the wavelength range between 350 nm and 410 nm is transparent to the emitter layer, so that the light in that range is absorbed in the InGaNP base layer and generates electron and hole pairs.
- the holes generated by the optical absorptipn in the p-type base layer are well confined in the base layer because the valence band discontinuity between GaN and InGaNP is larger than that for a conventional GaN homojunction photo transistor.
- an n- type substrate 1900 is provided, on which is formed an n-type layer 1910 of In ⁇ x Ga x Ni. y P y quaternary material or equivalent, which conforms to the relationships discussed above in connection with Figure 28.
- An active layer 1915 is thereafter formed, and above that is formed a layer 1920 of p-type ln ⁇ .
- a p-type second cladding layer 1925 is formed above the layer 1920, and a window 1930 is formed therein to expose a portion of the layer 1920.
- the window 1930 provides a port by which light can impinge on the layer 1920, causing the creation of holes.
- a pair of electrodes 1935 and 1940 may be fabricated in a conventional manner, with the electrode 1935 typically being a ring electrode around the window 1930.
- the band gap of the second cladding layer 1925 is preferably larger than the band gap of the layer 1920, which is in turn preferably larger than the band gap of the active layer 1915; such an approach provides sensitivity to the widest range of wavelength of light.
- a material with a lower band gap than the layer 1920 may be used for the layer 1925.
- FIG. 30 shown therein in cross-sectional view is a semiconductor structure according to a seventh embodiment of the invention.
- the semiconductor structure shown in many of the Figures will be a laser diode, although the present invention has application to a number of device types.
- an n-type GaN substrate 300 is provided and an n-type GaN first cladding layer 305 (typically 0.5 ⁇ m thick) is formed thereon.
- a second cladding layer 310 typically of an n-type Al 099 ln 001 N 099 P 001 material which may be on the order of 1.5 ⁇ m thick, is formed thereon, followed by a multiple quantum well active layer 315 which in an exemplary arrangement may comprise three quantum well layers of Alo. 99 l n o.o ⁇ 0.973 Po . o 27 material on the order of 35 A thick together with four barrier layers of Al 0-99 ln 0.01 N 0.975 Po . o 2 5 material on the order of 35 A thick, arranged as three pairs.
- a third cladding layer 320 of a p-type Al ⁇ 99 ln ⁇ 01 N 99 P ⁇ 01 (typically on the order of 1.5 ⁇ m thick) is formed, followed by a p-type GaN fifth cladding layer 325 (on the order of 0.5 ⁇ m thick).
- a first electrode 340 is formed on the n-type GaN substrate 300, while a second electrode 345 is formed on the Si0 2 layer 330 and the window region 335.
- the In content, x, and the P content, y, of all the layers generally satisfies the -condition 3.11(1-x)(1-y)+3.85(1-x)y+3.54x(1-y)+4.15xy nearly equals to a constant value, which may be on the order of 3.11+0.05 for at least the seventh embodiment.
- the lattice constants of the various constituent layers are matched to each other by setting the In content, x, and the P content, y, in each of the layers to meet the condition 3.11(1-x)(1-y)+3.85(1-x)y+3.54x(1-y)+4.15xy nearly equals to a constant value, again, for the seventh embodiment on the order of 3.18+0.05 so that the equivalent lattice constants of each layers become nearly equal to the lattice constant of GaN.
- the band gap energy of the n-type second cladding layer 310 and the p-type third cladding layer 320 are larger than that of the 3 pairs of multiple quantum well active layers 315.
- the refractive index of the n-type second cladding layer 310 and the p-type third cladding layer 320 are smaller than that of the multiple quantum well active layer 315, which confines the optical field in the transverse direction.
- the region in the active layer 315 under the widow region 335 is activated strongly. This causes the local modal gain in the active layer under the window region to be higher than the local modal gain in the active layer under the Si0 2 layer. Therefore, a gain guided waveguide mechanism, leading to a lasing oscillation, is able to be formed in the structure of the first embodiment.
- Figures 31A-31 D show, in sequence, a summary of the fabrication steps necessary to construct an exemplary laser diode according to the seventh embodiment. Since the structure which results from Figures 31 A-31 D will resemble that shown in Figure 30, like reference numerals will be used for elements whenever possible.
- an n-type GaN substrate 300 is provided, on which is grown an n-type GaN first cladding layer 305.
- the first cladding layer 305 is typically on the order of 0.5 ⁇ m thick.
- an n-type Al 99 ln 01 N 0 _ 99 P 01 second cladding layer 310 is formed, typically on the order of 1.5 ⁇ m thick.
- a multiple quantum well active layer 315 is formed by creating three quantum wells comprised of three layers of Alo. 9 glrio. 01 No.g 3 Po . 027 material each on the order of 35 A thick, together with four barrier layers of Al 0.99 ln 0. o ⁇ N 0.975 P 0. o 25 material on the order of 35 A thick.
- Each of the layers is typically formed by either the Metal Organic Chemical Vapor Deposition (MOCVD) method or the Molecular Beam Epitaxy (MBE) method.
- MOCVD Metal Organic Chemical Vapor Deposition
- MBE Molecular Beam Epitaxy
- a silicon dioxide (Si0 2 ) layer 330 is formed on the p-type GaN fourth cladding layer 325, for example by the Chemical Vapor Deposition (CVD) method.
- CVD Chemical Vapor Deposition
- a window region 335 is formed as shown in Figure 31 C.
- the window region 335 may be stripe-like in at least some embodiments.
- a first electrode 340 and a second electrode 345 are formed on the n-type GaN substrate 300 and on the Si0 2 layer 330, respectively, by evaporation or any other suitable process.
- a eighth embodiment of a semiconductor structure in accordance with the present invention may be better appreciated.
- an exemplary application of the eighth embodiment is the creation of a laser diode.
- the structure of the eighth embodiment permits a waveguide mechanism to be built into the structure with a real refractive index guide. This provides a low threshold current laser diode which can operate with a fundamental transverse mode.
- a first cladding layer 305 is formed of an n-type GaN on the order of 0.5 ⁇ m thick.
- an n-type second cladding layer 310 is formed of Al g9 ln o1 N 99 P 0-01 material on the order of 1.5 ⁇ m thick.
- a multiple quantum well active layer 315 is formed comprising three well layers of AI 0.99 ln 0.01 N 0.973 P 0.027 material on the order of 35 A thick together with four barrier layers of Al 0.99 ln ⁇ o1 N 97S P 0.025 material, also on the order of 35 A thick.
- a third, p-type cladding layer 320 formed of AI 099 ln 0 o ⁇ No . g 9 Po . o ⁇ material on the order of 1.5 ⁇ m thick is formed.
- a p-type GaN fourth cladding layer 325 on the order of 0.5 ⁇ m thick is formed over the ridge structure 2500 of the third cladding layer 320.
- the third and fourth cladding layers are then partially removed to create a ridge structure 2500.
- a silicon dioxide (Si0 2 ) layer 330 is then formed over the fourth cladding layer 5 325 as well as the remaining exposed portion of the third cladding layer 320.
- a window region 335 which may be stripe-like on the order of 2.0 ⁇ m width, is formed through the Si0 2 layer above the fourth and third cladding layers 325 and 320, respectively.
- a first electrode 340 is formed on the n-type GaN substrate 300 and a second electrode 345 is formed on 0 the Si0 2 layer 330 and the window region 335.
- the In content, x, and the P content, y, of the well layer is set to be 0.01 , 0.027, respectively.
- the In content, x, and the P content, y, of all the layers satisfies the condition 3.11(1-x)(1-y)+3.85(1 -x)y+3.54x(1- y)+4.15xy nearly equals to a constant value, which may for example be 3.13+0.05.
- the band gap energy of the cladding layers is maintained larger than the band gap energy for the active layer, allowing the emission of blue 0 light.
- the refractive index of the materials is as discussed in connection with the seventh embodiment, permitting the optical field to be confined in the transverse direction.
- the region of the active layer 315 under the window region 335 is activated strongly because of the 5 constraints on the injected current by the Si0 2 layer.
- This, combined with the relatively higher effective refractive index in the transverse direction inside the ridge stripe region compared to that outside the ridge stripe region, 0 provides an effective refractive index step.
- FIG. 33A-33E a summary of the key fabrication steps is shown for an exemplary device of a semiconductor laser diode in accordance with the sixth embodiment.
- the formation of the first and second cladding layers 305 and 310 on an n-type GaN substrate 300, together with the three-pair multiple quantum well active layer 315 are the same as for the seventh embodiment.
- the third and fourth cladding layers 320 and 325 are formed and then partially removed - typically by etching — to create a ridge 0 structure 2500.
- the various layers are formed successively by either the MOCVD or the MBE method.
- a silicon dioxide layer 330 is formed over the fifth and third cladding layers 325 and 320, respectively, typically by the CVD method, after which a window region 335 is formed as with the seventh 5 embodiment. Electrodes 340 and 345 are then evaporated or otherwise bonded to the structure.
- the selection of the In content, x, and the P content, y, and the relationship therebetween for the constituent InAINP layers may be better understood.
- the lattice constant of AIN, InN, AIP and InP are different from each other.
- the lattice mismatch between AIN and AIP, between InN and InP, and between AIN and InN are 23.9%, 17.2%, and
- Figure 34 shows the boundary of phase separation region plotted against various growth temperatures. The lines in Figure
- phase separation region 30 34 show the boundary between the compositionally unstable (phase separation) region and stable region with respect to various temperatures.
- phase separation occurs, Al atoms, In atoms, N atoms, and P atoms in the InAINP layers are not distributed uniformly according to the atomic content in each constituent layer.
- the band gap energy distribution of the phase separated layer also becomes inhomogeneous in the layer.
- the region of the relatively small band gap region in the phase separated layer acts as an optical absorption center, or causes an optical scattering for the waveguided light. This means that the phase separation phenomena should be avoided to obtain a high efficiency light emitting device.
- the phase separation region varies with temperature. The lines in Fig.
- an AllnNP material system can be provided in which the usual crystal growth temperature is in the approximate range of around 600 °C to around 1000°C.
- phase separation of the Al content and P content of AllnNP does not occur in significant amounts at processing temperatures between on the order of 600 °C and on the order of 1000 °C.
- the result is the substantially uniform distribution of Al atoms, In atoms, N atoms and P atoms in each constituent layer according to the atomic mole fraction.
- Group-Ill nitride materials are promising for use in electronic devices which can operate under high-power and high-temperature conditions - for example, microwave power transistors. This results, in part, from their wide band gap (3.5 eV for GaN and 6.2 eV for AIN), high breakdown electronic field, and high saturation velocity.
- the band gaps of AIAs, GaAs, and Si are 2.16 eV, 1.42 eV, and 1.12 eV, respectively.
- FETs field effect transistors
- the different lattice constants of AlGaN and GaN cause the generate of significant defects, limiting the mobility of electrons in the resultant structure and the utility of such materials systems for FET use.
- the present invention substantially overcomes these limitations, in that the AllnNP/AIN material of the present invention has a lattice constant nearly equal to AIN.
- the band gap of the AllnNP is larger than 5.2 eV so that reliable high-temperature operation can be achieved by using the structure shown in Figure 36A.
- Figure 36B shows an embodiment of a heterojunction bipolar transistor(HBT) in accordance with the present invention.
- HBT heterojunction bipolar transistor
- n-type AIN collector layer 2555 is formed, followed by a 50 nm thick p-type AllnNP base layer 2560, and a 300 nm thick n-type AIN emitter layer 2565.
- Base electrode 2570, collector electrode 2575 and emitter electrode 2580 are formed conventionally.
- the In and P contents x and y of the AllnNP layer are
- GaN and AIN are attractive materials for photo detectors in ultra violet light range, since both GaN and AIN have a wide band gap (3.5 eV for GaN which corresponds to the light wavelength of 350 nm, 6.2 eV for AIN which corresponds to the light wavelength of 200 nm). Due to the direct band gap and the availability of AlGaN in the entire AIN alloy composition range, AIGaN/GaN based visible light photo detectors have the advantage of high quantum efficiency, as well as tunability of high cut-off wavelength.
- the AI.,_ x ln x N.,_ y P y quaternary material whose In content, x and P content, y satisfy the relationship of 3.11(1-x)(1-y)+3.85(1-x)y+3.54x(1-y)+4.15xy nearly equals to 3.11 has a lattice constant nearly equal to AIN and a bandgap larger than 5 eV. Therefore, by using AllnNP/AIN material whose In content, x and P content, y satisfy the above relationship, UV light photo detectors with low defect density can be realized. In the event that detection of other frequencies is desired, only slight modification is required.
- the semiconductor device of the present invention can be implemented as a heterojunction phototransistor(HPT) using AllnNP/AIN material.
- a AIN collector layer 2705 is formed on the order of 500 nm thick n-type, followed by the formation of a 200 nm thick p-type AllnNP base layer 2710.
- a AIN emitter layer 2715 is formed on the order of 500 nm thick.
- a ring shaped electrode 2720 is formed to permit light to impinge on the base layer.
- the In content, x and P content, y of the AllnNP layer are set to be 0.01 and 0.027, respectively.
- the band gap of the AIN emitter layer (6.2 eV which corresponds to the light wavelength of 200 nm) is larger than that of AllnNP base layer (5.2 eV which corresponds to the light wavelength of 230 nm).
- the light impinges on the emitter side.
- impinging light in the wavelength range between 200 nm and 230 nm is transparent to the emitter layer, so that the light in that range is absorbed in the AllnNP base layer and generates electron and hole pairs.
- the holes generated by the optical absorption in the p- type base layer are well confined in the base layer because the valence band discontinuity between AIN and AllnNP is larger than that for a conventional AIN homojunction photo transistor.
- an n-type substrate 2900 is provided, on which is formed an n-type layer 2910 of quaternary material or equivalent, which conforms to the relationships discussed above in connection with Figure 37.
- An active layer 2915 is thereafter formed, and above that is formed a layer 2920 of p-type Al ⁇ n x N ⁇ y P y quaternary material. Then, a p-type second cladding layer 2925 is formed above the layer 2920, and a window 2930 is formed therein to expose a portion of the layer 2920.
- the window 2930 provides a port by which light can impinge on the layer 2920, causing the creation of holes.
- a pair of electrodes 2935 and 2940 may be fabricated in a conventional manner, with the electrode 2935 typically being a ring electrode around the window 2930.
- the band gap of the second cladding layer 2925 is preferably larger than the band gap of the layer 2920, which is in turn preferably larger than the band gap of the active layer 2915; such an approach provides sensitivity to the widest range of wavelength of light. If the event a narrower range is desired, a material with a lower band gap than the layer 2920 may be used for the layer 2925. In addition, it is also not necessary to include the layer 2925 in all embodiments, as the layers 2910, 2915 and 2920 provide, in at least some instances, an adequate photosensitive pn-junction.
Landscapes
- Semiconductor Lasers (AREA)
- Solid State Image Pick-Up Elements (AREA)
- Bipolar Transistors (AREA)
- Junction Field-Effect Transistors (AREA)
- Led Devices (AREA)
Priority Applications (1)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2001550837A JP4836382B2 (ja) | 1999-12-31 | 2000-12-08 | 発光素子 |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| US09/476,017 | 1999-12-31 | ||
| US09/476,017 US6472679B1 (en) | 1999-12-31 | 1999-12-31 | Semiconductor structures using a group III-nitride quaternary material system with reduced phase separation and method of fabrication |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2001050558A1 true WO2001050558A1 (en) | 2001-07-12 |
Family
ID=23890156
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/IB2000/001836 Ceased WO2001050558A1 (en) | 1999-12-31 | 2000-12-08 | Group iii-nitride semiconductor structures with reduced phase separation |
Country Status (3)
| Country | Link |
|---|---|
| US (1) | US6472679B1 (enExample) |
| JP (1) | JP4836382B2 (enExample) |
| WO (1) | WO2001050558A1 (enExample) |
Cited By (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| GB2522597B (en) * | 2012-12-21 | 2018-03-07 | Intel Corp | Lattice mismatched hetero-epitaxial film |
Families Citing this family (9)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP4387472B2 (ja) * | 1998-02-18 | 2009-12-16 | 三菱電機株式会社 | 半導体レーザ |
| JP2002314205A (ja) * | 2001-04-19 | 2002-10-25 | Sharp Corp | 窒化物半導体発光素子ならびにそれを用いた光学装置および発光装置 |
| EP1353384A3 (en) * | 2002-04-10 | 2005-01-12 | Hitachi, Ltd. | Heterojunction bipolar transistor, manufacturing thereof and power amplifier module |
| DE10355962A1 (de) * | 2003-09-30 | 2005-04-28 | Osram Opto Semiconductors Gmbh | Strahlungsemittierender Halbleiterkörper mit Confinement-Schichten |
| EP1521311A3 (de) * | 2003-09-30 | 2010-09-15 | OSRAM Opto Semiconductors GmbH | Strahlungsemittierender Halbleiterkörper mit Confinement-Schichten |
| US20080258131A1 (en) * | 2005-09-30 | 2008-10-23 | Seoul Opto-Device Co., Ltd. | Light Emitting Diode |
| RU2650606C2 (ru) * | 2016-08-17 | 2018-04-16 | Российская Федерация, от имени которой выступает Федеральное государственное казенное учреждение "Войсковая часть 35533" | ГЕТЕРОСТРУКТУРА GaPAsN СВЕТОДИОДА И ФОТОПРИЕМНИКА НА ПОДЛОЖКЕ Si И СПОСОБ ЕЕ ИЗГОТОВЛЕНИЯ |
| JP7461630B2 (ja) * | 2020-01-23 | 2024-04-04 | 国立大学法人東海国立大学機構 | 高電子移動度トランジスタ装置、半導体多層膜ミラーおよび縦型ダイオード |
| KR102682627B1 (ko) * | 2021-10-12 | 2024-07-05 | (재)한국나노기술원 | 다파장 광 검출기 및 이의 제조 방법 |
Citations (8)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US5005057A (en) * | 1989-04-28 | 1991-04-02 | Kabushiki Kaisha Toshiba | Semiconductor light-emitting diode and method of manufacturing the same |
| EP0487822A1 (en) * | 1990-11-27 | 1992-06-03 | Pioneer Electronic Corporation | Semiconductor light emitting element |
| EP0617491A2 (de) * | 1993-03-26 | 1994-09-28 | Daimler-Benz Aktiengesellschaft | Lichtemittierendes Halbleiterbauelement |
| JPH1084163A (ja) * | 1996-09-05 | 1998-03-31 | Ricoh Co Ltd | 半導体発光素子 |
| US5825052A (en) * | 1994-08-26 | 1998-10-20 | Rohm Co., Ltd. | Semiconductor light emmitting device |
| JPH11284282A (ja) * | 1998-03-31 | 1999-10-15 | Fuji Photo Film Co Ltd | 短波長発光素子 |
| EP0952645A2 (en) * | 1998-04-22 | 1999-10-27 | Matsushita Electric Industrial Co., Ltd. | Semiconductor laser device |
| WO2001009996A1 (en) * | 1999-07-30 | 2001-02-08 | Matsushita Electric Industrial Co., Ltd. (Mei) | Semiconductor structures using a group iii-nitride quaternary material system |
Family Cites Families (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| DE4310569A1 (de) * | 1993-03-26 | 1994-09-29 | Daimler Benz Ag | Laserdiode |
| JPH11284225A (ja) * | 1998-03-27 | 1999-10-15 | Showa Denko Kk | Iii族窒化物半導体発光素子 |
| JP4054480B2 (ja) * | 1999-05-18 | 2008-02-27 | キヤノン株式会社 | Si基板上の光電融合デバイス構造、その製造方法、及び成膜方法 |
| JP2001024282A (ja) * | 1999-07-09 | 2001-01-26 | Hitachi Ltd | Iii−v族混晶半導体を用いた半導体装置の製造方法及び光通信システム |
-
1999
- 1999-12-31 US US09/476,017 patent/US6472679B1/en not_active Expired - Lifetime
-
2000
- 2000-12-08 JP JP2001550837A patent/JP4836382B2/ja not_active Expired - Fee Related
- 2000-12-08 WO PCT/IB2000/001836 patent/WO2001050558A1/en not_active Ceased
Patent Citations (8)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US5005057A (en) * | 1989-04-28 | 1991-04-02 | Kabushiki Kaisha Toshiba | Semiconductor light-emitting diode and method of manufacturing the same |
| EP0487822A1 (en) * | 1990-11-27 | 1992-06-03 | Pioneer Electronic Corporation | Semiconductor light emitting element |
| EP0617491A2 (de) * | 1993-03-26 | 1994-09-28 | Daimler-Benz Aktiengesellschaft | Lichtemittierendes Halbleiterbauelement |
| US5825052A (en) * | 1994-08-26 | 1998-10-20 | Rohm Co., Ltd. | Semiconductor light emmitting device |
| JPH1084163A (ja) * | 1996-09-05 | 1998-03-31 | Ricoh Co Ltd | 半導体発光素子 |
| JPH11284282A (ja) * | 1998-03-31 | 1999-10-15 | Fuji Photo Film Co Ltd | 短波長発光素子 |
| EP0952645A2 (en) * | 1998-04-22 | 1999-10-27 | Matsushita Electric Industrial Co., Ltd. | Semiconductor laser device |
| WO2001009996A1 (en) * | 1999-07-30 | 2001-02-08 | Matsushita Electric Industrial Co., Ltd. (Mei) | Semiconductor structures using a group iii-nitride quaternary material system |
Non-Patent Citations (4)
| Title |
|---|
| HO I ET AL: "Solubility of nitrogen in binary III-V systems", JOURNAL OF CRYSTAL GROWTH, 1997, vol. 178, pages 1 - 7, XP004084971, ISSN: 0022-0248 * |
| PATENT ABSTRACTS OF JAPAN vol. 1998, no. 08 30 June 1998 (1998-06-30) * |
| PATENT ABSTRACTS OF JAPAN vol. 2000, no. 01 31 January 2000 (2000-01-31) * |
| TU C ET AL: "Growth and characterization of (InGa)(NP) on GaP", COMPOUND SEMICONDUCTORS, ST. PETERSBURG, 1996, pages 213 - 218, XP000990124, ISBN: 0-7503-0452-9 * |
Cited By (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| GB2522597B (en) * | 2012-12-21 | 2018-03-07 | Intel Corp | Lattice mismatched hetero-epitaxial film |
Also Published As
| Publication number | Publication date |
|---|---|
| US6472679B1 (en) | 2002-10-29 |
| JP2003519931A (ja) | 2003-06-24 |
| JP4836382B2 (ja) | 2011-12-14 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| US6521917B1 (en) | Semiconductor structures using a group III-nitride quaternary material system with reduced phase separation | |
| US7402843B2 (en) | Group III-V compound semiconductor and group III-V compound semiconductor device using the same | |
| US6525335B1 (en) | Light emitting semiconductor devices including wafer bonded heterostructures | |
| JP2002540618A (ja) | 歪補償層を有する半導体構造及び製造方法 | |
| CN100499190C (zh) | 半导体器件 | |
| US20030116767A1 (en) | Edge-emitting nitride-based laser diode with P-N tunnel junction current injection | |
| US5321712A (en) | Semiconductor light-emitting device having a cladding layer composed of an InGaAlp-based compound | |
| KR20050085757A (ko) | 반도체 메사 구조와 도전형 접합을 포함하는 전자 소자 및그 제조방법 | |
| US7391062B2 (en) | Semiconductor structures using a group III-nitride material system with reduced phase separation and method of fabrication | |
| US6229150B1 (en) | Semiconductor structures using a group III-nitride quaternary material system with reduced phase separation and method of fabrication | |
| JP4837012B2 (ja) | 発光素子 | |
| US6472679B1 (en) | Semiconductor structures using a group III-nitride quaternary material system with reduced phase separation and method of fabrication | |
| JPH05175594A (ja) | 半導体レーザ装置 | |
| US6472680B1 (en) | Semiconductor structures using a group III-nitride quaternary material system with reduced phase separation | |
| JP2885198B2 (ja) | p型電極構造およびそれを有する半導体発光素子 | |
| JPH11284280A (ja) | 半導体レーザ装置及びその製造方法ならびにiii−v族化合物半導体素子の製造方法 | |
| JPH05160504A (ja) | 半導体レーザ装置 | |
| JPH11307880A (ja) | 半導体発光装置 | |
| US20060243992A1 (en) | Semiconductor light-emitting device | |
| JPH1187835A (ja) | 半導体レーザ及びその製造方法 | |
| JPH0936415A (ja) | 発光ダイオード |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| AK | Designated states |
Kind code of ref document: A1 Designated state(s): CN JP |
|
| AL | Designated countries for regional patents |
Kind code of ref document: A1 Designated state(s): AT BE CH CY DE DK ES FI FR GB GR IE IT LU MC NL PT SE TR |
|
| DFPE | Request for preliminary examination filed prior to expiration of 19th month from priority date (pct application filed before 20040101) | ||
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application | ||
| DFPE | Request for preliminary examination filed prior to expiration of 19th month from priority date (pct application filed before 20040101) | ||
| ENP | Entry into the national phase |
Ref country code: JP Ref document number: 2001 550837 Kind code of ref document: A Format of ref document f/p: F |
|
| 122 | Ep: pct application non-entry in european phase |