WO1994016803A1 - Thermally induced phase separated azlactone membrane - Google Patents
Thermally induced phase separated azlactone membrane Download PDFInfo
- Publication number
- WO1994016803A1 WO1994016803A1 PCT/US1994/001062 US9401062W WO9416803A1 WO 1994016803 A1 WO1994016803 A1 WO 1994016803A1 US 9401062 W US9401062 W US 9401062W WO 9416803 A1 WO9416803 A1 WO 9416803A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- azlactone
- membrane
- carbon atoms
- polymer
- blended
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J9/00—Working-up of macromolecular substances to porous or cellular articles or materials; After-treatment thereof
- C08J9/28—Working-up of macromolecular substances to porous or cellular articles or materials; After-treatment thereof by elimination of a liquid phase from a macromolecular composition or article, e.g. drying of coagulum
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D67/00—Processes specially adapted for manufacturing semi-permeable membranes for separation processes or apparatus
- B01D67/0002—Organic membrane manufacture
- B01D67/0023—Organic membrane manufacture by inducing porosity into non porous precursor membranes
- B01D67/0025—Organic membrane manufacture by inducing porosity into non porous precursor membranes by mechanical treatment, e.g. pore-stretching
- B01D67/0027—Organic membrane manufacture by inducing porosity into non porous precursor membranes by mechanical treatment, e.g. pore-stretching by stretching
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D67/00—Processes specially adapted for manufacturing semi-permeable membranes for separation processes or apparatus
- B01D67/0002—Organic membrane manufacture
- B01D67/0023—Organic membrane manufacture by inducing porosity into non porous precursor membranes
- B01D67/003—Organic membrane manufacture by inducing porosity into non porous precursor membranes by selective elimination of components, e.g. by leaching
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D71/00—Semi-permeable membranes for separation processes or apparatus characterised by the material; Manufacturing processes specially adapted therefor
- B01D71/06—Organic material
- B01D71/26—Polyalkenes
- B01D71/261—Polyethylene
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D71/00—Semi-permeable membranes for separation processes or apparatus characterised by the material; Manufacturing processes specially adapted therefor
- B01D71/06—Organic material
- B01D71/26—Polyalkenes
- B01D71/262—Polypropylene
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D71/00—Semi-permeable membranes for separation processes or apparatus characterised by the material; Manufacturing processes specially adapted therefor
- B01D71/06—Organic material
- B01D71/44—Polymers obtained by reactions only involving carbon-to-carbon unsaturated bonds, not provided for in a single one of groups B01D71/26-B01D71/42
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D71/00—Semi-permeable membranes for separation processes or apparatus characterised by the material; Manufacturing processes specially adapted therefor
- B01D71/06—Organic material
- B01D71/76—Macromolecular material not specifically provided for in a single one of groups B01D71/08 - B01D71/74
- B01D71/78—Graft polymers
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D2323/00—Details relating to membrane preparation
- B01D2323/08—Specific temperatures applied
- B01D2323/081—Heating
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D2323/00—Details relating to membrane preparation
- B01D2323/24—Use of template or surface directing agents [SDA]
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
- B01D—SEPARATION
- B01D71/00—Semi-permeable membranes for separation processes or apparatus characterised by the material; Manufacturing processes specially adapted therefor
- B01D71/06—Organic material
- B01D71/58—Other polymers having nitrogen in the main chain, with or without oxygen or carbon only
- B01D71/62—Polycondensates having nitrogen-containing heterocyclic rings in the main chain
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J2201/00—Foams characterised by the foaming process
- C08J2201/04—Foams characterised by the foaming process characterised by the elimination of a liquid or solid component, e.g. precipitation, leaching out, evaporation
- C08J2201/054—Precipitating the polymer by adding a non-solvent or a different solvent
- C08J2201/0542—Precipitating the polymer by adding a non-solvent or a different solvent from an organic solvent-based polymer composition
- C08J2201/0543—Precipitating the polymer by adding a non-solvent or a different solvent from an organic solvent-based polymer composition the non-solvent being organic
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J2201/00—Foams characterised by the foaming process
- C08J2201/04—Foams characterised by the foaming process characterised by the elimination of a liquid or solid component, e.g. precipitation, leaching out, evaporation
- C08J2201/054—Precipitating the polymer by adding a non-solvent or a different solvent
- C08J2201/0545—Precipitating the polymer by adding a non-solvent or a different solvent from an aqueous solvent-based polymer composition
- C08J2201/0546—Precipitating the polymer by adding a non-solvent or a different solvent from an aqueous solvent-based polymer composition the non-solvent being organic
-
- Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
- Y10—TECHNICAL SUBJECTS COVERED BY FORMER USPC
- Y10T—TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION
- Y10T428/00—Stock material or miscellaneous articles
- Y10T428/249921—Web or sheet containing structurally defined element or component
- Y10T428/249953—Composite having voids in a component [e.g., porous, cellular, etc.]
- Y10T428/249978—Voids specified as micro
-
- Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
- Y10—TECHNICAL SUBJECTS COVERED BY FORMER USPC
- Y10T—TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION
- Y10T428/00—Stock material or miscellaneous articles
- Y10T428/249921—Web or sheet containing structurally defined element or component
- Y10T428/249953—Composite having voids in a component [e.g., porous, cellular, etc.]
- Y10T428/249978—Voids specified as micro
- Y10T428/249979—Specified thickness of void-containing component [absolute or relative] or numerical cell dimension
Definitions
- the present invention is generally related to azlactone modified polymeric membranes and is more particularly related to a thermally induced, phase separated polymeric membrane containing an azlactone moiety which was added to the polymer by extrusion grafting or blending.
- the thermally induced, phase separated azlactone polymeric membranes are suitable for use in a variety of separation and chromatographic applications.
- Polymeric supports which have been modified to include an azlactone moiety may be useful for a number of applications.
- the capability of the azlactone moiety to covalently bind a variety of biologically significant or useful materials to a polymer have allowed the use of azlactone-modified polymers as complexing agents, enzymes, catalysts, polymeric reagents, and chromatographic supports as well as other types of activated supports.
- Another reported method of attaching an azlactone moiety to a polymeric support involves coating the surface of a polymerized substrate with an azlactone reagent.
- Reported processes provide a polymer having an azlactone moiety being covalently attached or bound to outer surfaces of the polymeric support.
- the covalent attachment of the azlactone moiety to the polymer avoids problems typically associated with surface coatings which are not bound to the polymer surface such as leaching of the coating from the polymer surface during the use of the coated polymer.
- the reported azlactone graft copolymer may be extruded, formed or molded into a variety of configurations such as beads, pellets, strips, films, or wells and may be used in diverse applications such as thermoplastic adhesives and tie layers for barrier films.
- the azlactone moiety may be reacted with nucleophilic reagents such as proteins and other biologically active reagents.
- nucleophilic reagents such as proteins and other biologically active reagents.
- the covalent attachment of biological reagents to the polymeric support through the grafted azlactone moiety allows use of the graft copolymers in separation and chromatographic applications.
- Microporous films or membranes are one specialized type of material which has potential application in a number of separation or chromatographic uses such as analysis of air, microbiological products, intravenous fluids or vaccines.
- a specific type of microporous film or membrane is reported in U.S. Patent 4,539,256 to Shipman.
- This patent reports a microporous film or sheet material that has a microporous structure characterized by having a multiplicity of spaced, randomly dispersed, equiaxed, non-uniformly shaped particles of polymeric material that are connected to each other by a plurality of three-dimensionally dispersed polymeric fibrils.
- a method of making this type of microporous film is also reported in U.S. Patent 4,539,256.
- the method of making such a microporous film involves melt blending a crystallizable thermoplastic polymer with a compound which is miscible with the polymer at the melting temperature of the polymer but that phase separates at a temperature at or below the crystallization temperature of the polymer.
- the melt-blend After the formation of the melt-blend, it is shaped into an article and the article is then cooled to a temperature at which the polymer crystallizes and causes phase separation to occur between the polymer and the compound to give a two phase article.
- the compound used to form the melt-blend is extracted or removed from the shaped article.
- the article is then oriented or stretched in a least one direction to give a network of particles interconnected with fibrils throughout the article.
- the present invention provides a unique microporous membrane material formed from an azlactone-modified thermoplastic composition.
- a microporous material or membrane is produced from an alkenyl azlactone moiety which is grafted onto a
- crystallizable thermoplastic polyolefin to provide a porous material having an internal structure characterized by a multiplicity of spaced, randomly disposed, non-uniformly shaped, equiaxed particles of the azlactone graft copolymer.
- Each of the adjacent particles throughout the material are separated from one another to provide the material with a network of interconnected micropores.
- each of the particles are connected to each other by a plurality of fibrils.
- a microporous material or membrane having substantially the same properties as those listed above is produced from a polyazlactone homopolymer or copolymer which is extrusion blended with a crystallizable thermoplastic polyolefin.
- Preferred alkenyl azlactone monomers suitable for use in extrusion grafting or for use in preparing polyazlactone homopolymers or copolymers suitable for use in extrusion blending include a compound or monomer of the formula
- R 1 is hydrogen or methyl and where R 2 and R 3 are, independently, alkyl having 1-14 carbon atoms, cycloalkyl having 3-14 carbon atoms, aryl having 5-12 carbons atoms, arenyl having 6-26 carbons atoms and 0-3 sulfur, nitrogen, and nonperoxidic oxygen atoms, or R 2 and R 3 taken together with the carbon atom to which they are attached form a carbocyclic ring having 4-12 carbon atoms.
- a highly preferred alkenyl azlactone monomer is vinyl dimethyl azlactone.
- Preferred base polymers for use in this invention include polyolefins such as polyethylene, polypropylene and polymethylpentene.
- a highly preferred polymer is high density polyethylene.
- membranes which have been modified by subsequent reaction of the azlactone moiety with a suitable nucleophile are also included within the scope of the present invention.
- nucleophiles capable of reacting with an azlactone membrane of this invention include biologically significant nucleophiles such as amines, thiols and alcohols as well as amino acids, nucleic acids and proteins.
- Particular preferred nucleophiles are biological active proteins such as antigens and antibodies.
- Grafted or blended azlactone thermoplastic compositions are believed to produce a microporous material or a membrane containing grafted azlactone monomer or blended polyazlactone polymer distributed throughout the bulk of membrane rather than being distributed only on accessible, exposed or outer surfaces of the membrane.
- the distribution of the azlactone moiety throughout the bulk of the membrane is also believed to increase the available active sites on the membrane which provides a substantial increase in the binding capacity of the membrane for a variety of useful reagents.
- Figure 1 is a schematic diagram of the process steps used to prepare a membrane of this invention.
- Figure 2 is a schematic diagram of an extrusion blending process using a twin screw extruder.
- the present invention provides an azlactone membrane having a network of spaced, randomly disposed, non-uniformly shaped, equiaxed particles interconnected with a plurality of fibrils to provide a network of interconnected particles containing dialkylazlactone moieties extrusion grafted to or blended with a crystallizable thermoplastic polymer.
- Suitable extrusion grafted azlactone thermoplastic compositions for use in this invention may be made according to the process reported in EP 0 392 783 which is incorporated by reference herein for the purpose of describing methods of preparing azlactone graft copolymers. Briefly, a suitable polyolefin resin such as high density polyethylene, polypropylene or
- polymethylpentene is mixed with a free radical initiator, such as a peroxide or azo initiator, and the mixture is heated in an extruder at a temperature sufficient to break down the initiator and produce free radicals.
- a free radical initiator such as a peroxide or azo initiator
- the free radical initiator is selected from a variety of known compounds based on the properties of the polyolefin resin and the amount of added free radical initiator is selected to provide for sufficient grafting without causing undesired side reactions such as cross-linking of the polyolefin resin. Typical amounts of free radical initiator used to graft a vinyl dialkylazlactone to a polyolefin resin are about 0.01-0.25 weight percent.
- the free radicals produced then extract hydrogen atoms off of the polyolefin resin.
- the polyolefin resin loses hydrogen radicals, the polyolefin resin is activated and may undergo several subsequent reactions such as crosslinking with other base polymers, degradation, oxidation or, significantly, reaction with a suitable alkenyl monomer.
- a vinyl dialkylazlactone monomer such as vinyl dimethyl azlactone is injected into the extruder.
- the injected vinyl azlactone monomer then covalently binds to the activated polyolefin resin and may be used to form a membrane.
- the vinyl azlactone copolymer is susceptible to hydrolysis. Therefore, the grafting process and reaction are preferably done in the absence of water in an inert atmosphere or an unreactive environment. Use of these conditions prevents the azlactone from degrading and prevents side reactions from interfering with the grafting or addition of the vinyl azlactone monomer to the polyolefin resin.
- Suitable extrusion blended azlactone thermoplastic compositions for use in the this invention may be prepared according to the processes reported in pending U.S. patent application Serial Number 08/119,036 filed September 9, 1993, which is incorporated by reference in the present application for the purposes of describing the preparation of blended azlactone thermoplastic compositions.
- Melt blending of polyazlactone homopolymers or copolymers with thermoplastic polymers is an alternative to the extrusion graft process described above.
- polyazlactone polymers are melt blended with thermoplastic polymers, a two phase, incompatible blended product usually results. This incompatibility generally does not have deleterious properties of incompatible compositions due to the ability of azlactone-functionality to react with desired biological ligands.
- polyazlactone blends may be prepared from any thermoplastic polymer that is non-reactive with an azlactone monomer.
- thermoplastic polymers suitable for melt blending with polyazlactone homopolymers or copolymers include polyamides (e.g., nylon 6), polyurethanes, polyacrylates, polymethacrylates, polystyrene, polyolefins, ethylene-vinyl acetate copolymers, poly(N-vinyl lactams)
- polyvinylpyrrolidone e.g., polyvinylpyrrolidone
- polyvinyl acetates e.g., polyvinyl acetates
- polyoxyalkylenes e.g., polyvinyl ethylene glycol dimethacrylate
- thermoplastic polymers may be homopolymers or copolymers.
- Thermoplastic copolymers may include azlactone copolymers, such as graft copolymers reported in U.S. Patent
- Polyazlactone polymers may be any compound containing or comprising at least one azlactone moiety.
- Preferred polyazlactone polymers are homopolymers of 2-alkenyl azlactone monomers.
- Suitable 2-alkenyl azlactone monomers are known compounds, their synthesis being described for example in U.S. Patents 4,304,705; 5,081,197 and 5,091,489 all to Heilmann et al.
- Suitable 2-alkenyl azlactones include:
- 2-ethenyl-4,4-dimethyl-1,3-oxazolin-6-one Most preferred 2-alkenyl azlactones include 2-ethenyl-4,4-dimethyl-1,3-oxazolin-5-one (VDM) and 2-isopropenyl-
- azlactone monomers include the 2-(4- alkenylphenyl)-5-oxazolones reported in U.S. Patent 5,039,813.
- a comonomer having similar or different chemical or physical properties may be included, depending on the desired characteristics for the copolymer to be blended.
- Nonlimiting examples of comonomers useful to be copolymerized with azlactone moieties to form copolymers include methyl methacrylate, vinyl acetate, vinyl aromatic monomers, alpha,beta-unsaturated carboxylic acids or their derivatives or vinyl esters, vinyl alkyl ethers, olefins, N-vinyl compounds, vinyl ketones, styrene, or vinyl aldehydes.
- Nonlimiting examples of such comonomers are reported in EP 0 392 735 and EP 0 392 783.
- Polyazlactone copolymers may be prepared by bulk polymerization as reported in U.S. Patent 4,695,608 to Engler et al.
- polyazlactone polymers and oligomers may be typically prepared by free radical polymerization of azlactone monomers, optionally with
- thermoplastic polymers are readily commercially available from a number of sources. While thermoplastic polymers may be melt blended at temperatures ranging from about 50°C to about 350°C, it is preferred that thermoplastic polymers are melt blended at temperatures from about 75°C to about 300°C, and more preferably from about 100°C to about 300°C.
- melt blending of thermoplastic polymer with a polyazlactone homopolymer or copolymer may occur at temperatures which are required for the melting of the thermoplastic polymer. Because polyazlactone
- melt blending should occur below about 210°C.
- the temperature of melt blending must be at least at or above the glass transition temperature (Tg) of both the polyazlactone homopolymer and the thermoplastic polymer and preferably is at least about 25°C above the Tg of amorphous or glassy polymers such as polystyrene or polymethylmethacrylate and at least about 10°C above the melting point of semicrystalline polymers such as polyethylene and polypropylene.
- Tg glass transition temperature
- Melt blending of polyazlactone homopolymers with a thermoplastic polymer may be done using a twin-screw extruder. As illustrated in Fig. 2, after homopolymerization of alkenyl azlactone, polyazlactone homopolymer (or other polyazlactone copolymer) in a pelletized form is introduced to extruder 30 from vessel 32. Thermoplastic polymer is introduced in pelletized form into extruder 30 from vessel 34. Vacuum ports 35 vent off volatiles. If thermoplastic polymer were introduced into the extruder 30 in solution, then vacuum ports 35 would vent off the solvent also. Gear pump 36 eliminates surging and produces a continuous strand of the blended
- the blended composition is quenched in bath 37 which contains a cold (dry ice temperature) inert cooling fluid such as FLUORINERT heat transfer liquid (3M, St. Paul, MN). Finally, the cooled, blended composition is directed through pelletizer 38.
- a cold (dry ice temperature) inert cooling fluid such as FLUORINERT heat transfer liquid (3M, St. Paul, MN).
- the weight ratio of thermoplastic polymer to polyazlactone polymer may range from about 99.99:0.01 to about 50:50.
- the weight ratio of thermoplastic polymer to azlactone polymer is about 95:5, when the azlactone polymer is azlactone homopolymer prepared according to the method reported in EP 0 392 735.
- any of the polyazlactone copolymers and oligomers described in pending U.S. patent application Serial Number 08/119,036 may be used in melt blending with thermoplastic polymer. These blends need not be compatible. However, the reactivity of incompatible blends with biologically active substances is not compromised by polymer blend incompatibility. Generally, the mixing conditions and temperature conditions for melt blending azlactone copolymers are similar to melt blending azlactone homopolymers.
- the melt blending of the azlactone-modified thermoplastic composition should not adversely alter bulk properties of the thermoplastic polymer.
- Melt flow index is a key bulk property.
- the azlactone-modified composition may have a melt flow index (g/10 min.) ranging from within about 50% of the melt flow index of the thermoplastic polymer alone to within about 99% of the melt flow index of the thermoplastic polymer alone.
- the melt flow index of the azlactone-modified composition is within about 75 % of the melt flow index of the thermoplastic polymer alone.
- azlactone graft or blend compositions may be formed into a microporous membrane.
- an azlactone thermoplastic composition is starve-fed from hopper 10 into extruder 14.
- the composition is formed into a melt-blend with a blending compound injected through port 12 in extruder 14.
- Preferred blending compounds are typically solvents or mixtures of solvents which will form a homogeneous solution with the polymer at high temperatures and will form two phases when the homogeneous mixture is cooled below the crystalline temperature of the composition.
- mineral oil is a preferred solvent because it is capable of forming a
- the amount of blending compound which is mixed with the azlactone thermoplastic composition depends on the base polymeric resin.
- the amount of mineral oil used to form a melt- blend of high density polyethylene is about 55-80 weight percent, for polypropylene and polymethylpentene the amount of mineral oil used to form a melt-blend is about 30-75 weight percent.
- a small amount of nucleating agent such as pigments and polysorbitol derivatives may be added to the melt-blend.
- Extruder 14 is maintained at a temperature which is sufficient to form a homogenous melt of the composition and blending compound.
- extruder 14 may contain a static mixer, not shown, to ensure that a uniform, homogeneous melt-blend is obtained.
- the extruder 14 is preferably configured so that when the melt-blend reaches a temperature greater than the melting point of the composition, the hot melt-blend is then extruded through die 16 onto cold roller or casting wheel 18.
- the temperature of casting wheel 18 is maintained at a temperature below the melting point of the polymer so that the melt-blend forms two phases on contact with the casting wheel.
- the casting wheel is typically maintained at a temperature of between 30-180°C.
- Extractor 20 preferably uses a solvent which is miscible with the blending compound and is also preferably a nonaqueous solvent. Suitable solvents include trichloroethane and fluorinated hydrocarbons as well as mixtures of fluorinated hydrocarbons. Preferably, the nonaqueous extraction solvent is removed and recycled after being used to extract the blending compound from the cooled melt-blend.
- the resulting matrix is dried in dryer 22 at an elevated temperature to insure complete removal of all of the extraction solvent.
- the dried matrix is then oriented in at least the machine direction in orienter 24 and then is preferably oriented in the transverse direction in tenter 26.
- the dried matrix is stretched in both the machine and transverse directions up to about three-fold.
- the formation of the particles and connecting fibrils are generally formed during the orienting process. Although orientation in both machine and traverse directions to provide a biaxially oriented material is preferred, those of ordinary skill will understand that the dried matrix may be oriented in a single direction if desired.
- the azlactone-containing membrane is preferably stored in the absence of water or water vapor in order to prevent hydrolysis or degradation of the azlactone.
- the azlactone thermally induced, phase separated membranes of the present invention may be further modified with a variety of biologically useful ligands.
- ligands for use in the present membranes may include biologically active materials having azlactone-reactive, nucleophilic functional groups.
- biologically active materials are substances which are biologically, immunochemically, physiologically, or pharmaceutically active.
- biologically active substances include proteins, peptides, polypeptides, antibodies, antigenic substances, enzymes, cofactors, inhibitors, lectins, hormones, receptors, coagulation factors, amino acids, histones, vitamins, drugs, cell surface markers, and substances which interact with them.
- proteins, enzymes and antigenic substances are desired for coupling to the present azlactone-modified membranes.
- proteins, enzymes, and antigenic substances include natural and recombinant Protein A, immunoglobulins such as rat, human, bovine, rabbit, and mouse, concanavalin A, bovine serum albumin, thyroglobulin, apoferritin, lysozyme, carbonic anhydrase, lipase, pig liver esterase, penicillin acylase, and bacterial antigen.
- step 3 If the sample is water wettable (hydrophilic), go to step 3. If the sample did not wet-out (hydrophobic), immerse it in ethanol and then rinse it with water directly before going to step 3.
- the average pore size of the membrane sample was determined using
- LUPERSOL 101 (2,5-dimethyl-2,5-di-(t-butylperoxy)hexane):LUPERSOL 130 (2,5-dimethyl-2,5-di-(t-butylperoxy)hex-3-yne); AtoChem, Farmindale, N.Y.) in tetrahydrofuran (50:50) was dripped under a nitrogen atmosphere into the extruder feed throat at a rate to provide 0.1 wt. % of initiator based on polymer weight.
- Monomeric 2-ethenyl-4,4-dimethyl-2-oxazoline-5-one (VDM, available from SNPE, Inc, Princeton, NJ) was fed in a port between barrel zones 3 and 4.
- the extruder speed was set at 75 rpm and the feed rates were adjusted to provide a total flow rate of 80 g/minute.
- the feed throat was water cooled. Zones 1-7 were heated; Zone 1 at 150°C, Zone 2 at 160°C, Zone 3 at 170°C, Zones 4 and 5 at 180°C, Zones 6 and 7 at 190°C, and the end adaptor at 190°C.
- the extrudate was quenched in a bath of fluorinated coolant
- the grafted copolymer was introduced into the hopper of a 25mm twin screw extruder (Model ZE 25, Berstorff, Hannover, Germany) fitted with a flat film die.
- the grafted copolymer was fed into the extruder at a rate of 3.2 lb (1.5 Kg) per hour and the extruder operated at a 8 lb (3.6 Kg) per hour throughput rate.
- Mineral oil (SUPERLA Mineral Oil 31-USP, Amoco, Chicago, IL) was introduced into the extruder through an injection port at a rate to provide a blend of 40% by weight of grafted copolymer and 60% by weight of mineral oil.
- the mixture was cast as a transparent film onto a smooth casting wheel at a temperature of 32°C and a casting speed of 1.8 m/min.
- the extruder zone temperatures were as follows: Zone 1 at 196°C, Zones 2 and 3 at 265 °C, Zone 4 at 216°C, Zones 5-9 at 165°C.
- the film was washed in a metal frame with 1,1,1-trichloroethane for 15 minutes then air-dried at ambient temperature in a vented hood. It was biaxially stretched at 1.5 times its original length/width with a film stretcher (TM LongStretcher, Somerville, N.J.) at 74°C.
- the resulting film was stored in a desiccator.
- the physical characteristics of this membrane are listed in Table 1.
- Example 1 Using the method of Example 1, a copolymer containing 5% by weight of VDM grafted onto high density polyethylene (Dow 8345N, Midland, MI) was prepared. The resulting graft copolymer was then made into a film using the procedures described in Example 1 and stored in a desiccator. The physical characteristics of this membrane are listed in Table 1.
- Example 2 Using the general method of Example 1 except that a twin screw extruder (Model ZE-40x40D, Bertstorff, Hannover, Germany) was used and the processing zones were maintained at 180°C, a copolymer containing 3% by weight of VDM grafted onto polypropylene (PP, PRO-FAX 6723, HIMONT, Willmington, DE) was prepared.
- a twin screw extruder Model ZE-40x40D, Bertstorff, Hannover, Germany
- a copolymer containing 3% by weight of VDM grafted onto polypropylene PP, PRO-FAX 6723, HIMONT, Willmington, DE
- Example 2 Using the general method of Example 1 with only 50% by weight mineral oil, 49.5% by weight VDM grafted polypropylene and 0.5% by weight of a polyol acetal nucleating agent (MILLAD 3905, Milliken Chemical Spartanburg, SC) based on polymer, this copolymer was made into a film, washed with HCFC-123 (VERTREL 423, DuPont,
- Example 2 Using the general method of Example 1, except that a twin screw extruder (Model ZE-40x40D, Bertstorff, Hannover, Germany) was used with the processing zones maintained at 260°C and the initiator system was 50% by weight of 25:25:50 LUPERSOL 101:LUPERSOL 130:cumene hydroperoxide (AtoChem, Farmington, N.Y.) in tetrahydrofuran, a copolymer containing 3% by weight of VDM grafted onto polymethylpentene (TPX, Mitsui Petrochemical Industries, Ltd., Tokyo, Japan) was prepared.
- TPX Mitsui Petrochemical Industries, Ltd., Tokyo, Japan
- this copolymer was made into a film at 232 °C, washed with HCFC-123 (Vertrel 423, DuPont, Willington, DE), biaxially stretched at 138°C, and stored in a desiccator.
- HCFC-123 Verytrel 423, DuPont, Willington, DE
- Table 1 The physical characteristics of this membrane are listed in Table 1.
- a 35 % solids solution of azlactone homopolymer (solid powder having an average number molecular weight of about 11 ,000 prepared by solution polymerization of VDM (SNPE) with 0.5 wt. % azobisisobutyronitrile (VAZO 64) in tetrahydrofuran) in tetrahydrofuran was blended with polyolefin in a corotating twin screw extruder (Model ZE-40X40D, Bertstorff, Hannover, Germany; rpm 109, amps 31, volts 108, zone temperatures: Zone 1 - 25°C, Zones 2-4 - 180°C, Zone 5 - 170°C, Zone 6 - 180°C, Zone 7 - 177°C, Zone 8 - 125°C, Zone 9 - 195°C, Zone 10 - 200°C, Zone 11 - 205°C).
- a vacuum port was used at zone 9 of the extruder to pull off any volatiles in the material.
- the blend was extruded as a strand into a cold (dry ice) FLUORINET liquid solution (3M, St. Paul, MN) where the strand was quenched and pelletized using a Conair pelletizer (Con Air Group of Bay City, MI).
- Example 2 Using the general method of Example 1 (except that a twin screw extruder was used, Model ZE-40X40D, Bertstorff, Hannover, Germany having processing temperature zones as follows: Zone 1 - 248°C, Zone 2 - 271 °C, Zone 3 - 271 ° C, Zone 4 - 248°C, and Zone 5 - 177°C) the blended azlactone compositions were made into films.
- the weight percent of blended polymer was 35 wt. % and the weight percent of mineral oil was 65 wt. % .
- Table 2 The physical characteristics of the blended azlactone films are listed in Table 2.
- Example 3 Three control samples were prepared in a similar fashion to the second stage of Example 1.
- the three base resins high density polyethylene 8354N: Dow; polypropylene: Profax 6723: HiMont; polymethylpentene: Mitsui Petrochemical Industries, Ltd., Tokyo, Japan
- polypropylene a Millad nucleating agent (0.5 weight % based on polymer) and 50 weight % of mineral oil in place of the VDM grafted resins, were used.
- the physical properties of the three membranes which did not contain azlactone are listed in Table 3.
- the PBS buffer contained 25 mM sodium phosphate and 150 mM sodium chloride with a pH of 7.5.
- the sulfate buffer contained 25 mM sodium phosphate and 1.5 M sodium sulfate with a pH of 7.5.
- Discs (8 mm diameter) were punched from each film using a standard office paper punch.
- Each disc was placed in a 2.0 ml polypropylene microfuge tube then incubated with 200 ⁇ L of Protein A solution for 2 hours at ambient temperature with rocking. Each blend and control were run in triplicate. After 2 hours the protein solution was removed and unreacted azlactone was inactivated by incubating the disc with 1.0 M ethanolamine (500 ⁇ L solution in 25 mM sodium phosphate, pH 9.0) for 1 hour with rocking. All discs were rinsed for a minimum of 15 minutes with 500 ⁇ L of the PBS buffer. Bound radioactivity was determined with a Packard Gamma Scintillation Spectrometer (Model 5230; Packard Instruments, Downers Grove, IL).
- SDS sodium dodecyl sulfate
Landscapes
- Chemical & Material Sciences (AREA)
- Chemical Kinetics & Catalysis (AREA)
- Engineering & Computer Science (AREA)
- Manufacturing & Machinery (AREA)
- Materials Engineering (AREA)
- Health & Medical Sciences (AREA)
- Medicinal Chemistry (AREA)
- Polymers & Plastics (AREA)
- Organic Chemistry (AREA)
- Compositions Of Macromolecular Compounds (AREA)
- Manufacture Of Porous Articles, And Recovery And Treatment Of Waste Products (AREA)
- Separation Using Semi-Permeable Membranes (AREA)
- Treatment Of Liquids With Adsorbents In General (AREA)
Priority Applications (6)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| DE69403445T DE69403445T2 (de) | 1993-01-29 | 1994-01-28 | Azlacton-membran mit thermisch induzierter phasentrennung |
| EP94907369A EP0681507B1 (en) | 1993-01-29 | 1994-01-28 | Thermally induced phase separated azlactone membrane |
| US08/464,795 US5750245A (en) | 1993-01-29 | 1994-01-28 | Thermally induced phase separated azlactone membrane |
| CA002153319A CA2153319C (en) | 1993-01-29 | 1994-01-28 | Thermally induced phase separated azlactone membrane |
| JP6517373A JPH08506601A (ja) | 1993-01-29 | 1994-01-28 | 熱誘発式に相分離されたアズラクトン膜 |
| US08/996,681 US6063484A (en) | 1993-01-29 | 1997-12-23 | Thermally induced phase separated azlactone membrane |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| US1136693A | 1993-01-29 | 1993-01-29 | |
| US08/011,366 | 1993-01-29 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO1994016803A1 true WO1994016803A1 (en) | 1994-08-04 |
Family
ID=21750079
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/US1994/001062 Ceased WO1994016803A1 (en) | 1993-01-29 | 1994-01-28 | Thermally induced phase separated azlactone membrane |
Country Status (6)
| Country | Link |
|---|---|
| US (2) | US5750245A (enExample) |
| EP (1) | EP0681507B1 (enExample) |
| JP (1) | JPH08506601A (enExample) |
| CA (1) | CA2153319C (enExample) |
| DE (1) | DE69403445T2 (enExample) |
| WO (1) | WO1994016803A1 (enExample) |
Cited By (6)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO1995007317A3 (en) * | 1993-09-09 | 1995-06-01 | Minnesota Mining & Mfg | Azlactone-functional polymer blends, articles produced therefrom and methods for preparing both |
| WO1995032792A1 (en) * | 1994-05-26 | 1995-12-07 | Minnesota Mining And Manufacturing Company | Azlactone-functional membranes and methods of preparing and using same |
| WO1999053319A3 (en) * | 1998-04-13 | 1999-12-23 | 3M Innovative Properties Co | High-density, miniaturized arrays and methods of manufacturing same |
| WO2001016370A1 (en) * | 1999-09-02 | 2001-03-08 | 3M Innovative Properties Company | Arrays with mask layers and methods of manufacturing same |
| WO2001036958A1 (en) * | 1999-11-18 | 2001-05-25 | 3M Innovative Properties Company | Film based addressable programmable electronic matrix articles and methods of manufacturing and using the same |
| US6881538B1 (en) * | 2000-03-05 | 2005-04-19 | 3M Innovative Properties Company | Array comprising diamond-like glass film |
Families Citing this family (21)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US6482638B1 (en) * | 1999-12-09 | 2002-11-19 | 3M Innovative Properties Company | Heat-relaxable substrates and arrays |
| US6787635B2 (en) * | 2001-04-05 | 2004-09-07 | 3M Innovative Properties Company | Solid phase synthesis supports and methods |
| US20030040125A1 (en) * | 2001-08-21 | 2003-02-27 | 3M Innovative Properties Company | Methods for performing immunological assays |
| US7556858B2 (en) * | 2004-09-30 | 2009-07-07 | 3M Innovative Properties Company | Substrate with attached dendrimers |
| JP2009522405A (ja) * | 2005-12-30 | 2009-06-11 | スリーエム イノベイティブ プロパティズ カンパニー | 官能化基材を作製する方法 |
| US8586338B2 (en) | 2008-05-30 | 2013-11-19 | 3M Innovative Properties Company | Ligand functionalized substrates |
| US8652582B2 (en) * | 2008-05-30 | 2014-02-18 | 3M Innovative Properties Company | Method of making ligand functionalized substrates |
| WO2009158071A2 (en) * | 2008-06-26 | 2009-12-30 | 3M Innovative Properties Company | Solid support with a grafted chain |
| JP2012531531A (ja) | 2009-06-23 | 2012-12-10 | スリーエム イノベイティブ プロパティズ カンパニー | 官能化不織布物品 |
| EP2496987B1 (en) * | 2009-11-04 | 2020-04-29 | Alcon Inc. | A silicone hydrogel lens with a grafted hydrophilic coating |
| TWI483996B (zh) * | 2009-12-08 | 2015-05-11 | Novartis Ag | 具有共價貼合塗層之聚矽氧水凝膠鏡片 |
| US8377672B2 (en) * | 2010-02-18 | 2013-02-19 | 3M Innovative Properties Company | Ligand functionalized polymers |
| CN102844662B (zh) | 2010-03-03 | 2015-04-29 | 3M创新有限公司 | 配体胍基官能化聚合物 |
| EP4657144A3 (en) | 2010-07-30 | 2026-03-04 | Alcon Inc. | Silicone hydrogel lenses with water-rich surfaces |
| CA2851668C (en) | 2011-10-12 | 2016-08-16 | Novartis Ag | Method for making uv-absorbing ophthalmic lenses by coating |
| WO2014095690A1 (en) | 2012-12-17 | 2014-06-26 | Novartis Ag | Method for making improved uv-absorbing ophthalmic lenses |
| CN105829081B (zh) | 2013-12-17 | 2017-12-19 | 诺华股份有限公司 | 具有交联的亲水性涂层的硅水凝胶镜片 |
| SG10201901379TA (en) | 2014-08-26 | 2019-03-28 | Novartis Ag | Method for applying stable coating on silicone hydrogel contact lenses |
| SG11201803726VA (en) | 2015-12-15 | 2018-06-28 | Novartis Ag | Method for applying stable coating on silicone hydrogel contact lenses |
| EP3724699B1 (en) | 2017-12-13 | 2023-07-26 | Alcon Inc. | Method for producing mps-compatible water gradient contact lenses |
| CA3189382A1 (en) * | 2020-09-11 | 2022-03-17 | Jared M. CLINGER | Affinity chromatography devices containing a heat treated fibrillated polymer membrane and manifolds containing the same |
Citations (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| EP0105666A1 (en) * | 1982-09-30 | 1984-04-18 | Minnesota Mining And Manufacturing Company | Method of hydrophilizing or hydrophobizing polymers |
| US4868222A (en) * | 1985-06-10 | 1989-09-19 | The Dow Chemical Company | Preparation of asymmetric membranes by the solvent extraction of polymer components from polymer blends |
| EP0392783A2 (en) * | 1989-04-10 | 1990-10-17 | Minnesota Mining And Manufacturing Company | Azlactone graft copolymers |
| WO1994000464A1 (en) * | 1992-06-23 | 1994-01-06 | Minnesota Mining And Manufacturing Company | Deproteinization with azlactone-functional supports |
Family Cites Families (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US4539256A (en) * | 1982-09-09 | 1985-09-03 | Minnesota Mining And Manufacturing Co. | Microporous sheet material, method of making and articles made therewith |
| US4737560A (en) * | 1987-03-13 | 1988-04-12 | Minnesota Mining And Manufacturing Company | Polymer beads |
| US5292840A (en) * | 1987-03-13 | 1994-03-08 | Minnesota Mining And Manufacturing Company | Polymeric supports |
| US4871824A (en) * | 1987-03-13 | 1989-10-03 | Minnesota Mining And Manufacturing Company | Variably crosslinked polymeric supports |
| US5200100A (en) * | 1991-04-24 | 1993-04-06 | Texaco Inc. | Multifunctional viscosity index improver containing phenothiazine |
-
1994
- 1994-01-28 CA CA002153319A patent/CA2153319C/en not_active Expired - Fee Related
- 1994-01-28 WO PCT/US1994/001062 patent/WO1994016803A1/en not_active Ceased
- 1994-01-28 EP EP94907369A patent/EP0681507B1/en not_active Expired - Lifetime
- 1994-01-28 DE DE69403445T patent/DE69403445T2/de not_active Expired - Fee Related
- 1994-01-28 JP JP6517373A patent/JPH08506601A/ja active Pending
- 1994-01-28 US US08/464,795 patent/US5750245A/en not_active Expired - Lifetime
-
1997
- 1997-12-23 US US08/996,681 patent/US6063484A/en not_active Expired - Fee Related
Patent Citations (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| EP0105666A1 (en) * | 1982-09-30 | 1984-04-18 | Minnesota Mining And Manufacturing Company | Method of hydrophilizing or hydrophobizing polymers |
| US4868222A (en) * | 1985-06-10 | 1989-09-19 | The Dow Chemical Company | Preparation of asymmetric membranes by the solvent extraction of polymer components from polymer blends |
| EP0392783A2 (en) * | 1989-04-10 | 1990-10-17 | Minnesota Mining And Manufacturing Company | Azlactone graft copolymers |
| WO1994000464A1 (en) * | 1992-06-23 | 1994-01-06 | Minnesota Mining And Manufacturing Company | Deproteinization with azlactone-functional supports |
Cited By (17)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| EP0784063A3 (en) * | 1993-09-09 | 1998-01-07 | Minnesota Mining And Manufacturing Company | Azlactone-functional polymer blends, articles produced therefrom and methods for preparing both |
| WO1995007317A3 (en) * | 1993-09-09 | 1995-06-01 | Minnesota Mining & Mfg | Azlactone-functional polymer blends, articles produced therefrom and methods for preparing both |
| WO1995032792A1 (en) * | 1994-05-26 | 1995-12-07 | Minnesota Mining And Manufacturing Company | Azlactone-functional membranes and methods of preparing and using same |
| US6548607B2 (en) | 1998-04-13 | 2003-04-15 | 3M Innovative Properties Company | High density, miniaturized arrays and methods of manufacturing same |
| WO1999053319A3 (en) * | 1998-04-13 | 1999-12-23 | 3M Innovative Properties Co | High-density, miniaturized arrays and methods of manufacturing same |
| US7189842B2 (en) | 1998-04-13 | 2007-03-13 | 3M Innovative Properties Company | High density, miniaturized arrays and methods of manufacturing same |
| US6841258B2 (en) | 1998-04-13 | 2005-01-11 | 3M Innovative Properties Company | High density, miniaturized arrays and methods of manufacturing same |
| US6376619B1 (en) | 1998-04-13 | 2002-04-23 | 3M Innovative Properties Company | High density, miniaturized arrays and methods of manufacturing same |
| US6573338B2 (en) | 1998-04-13 | 2003-06-03 | 3M Innovative Properties Company | High density, miniaturized arrays and methods of manufacturing same |
| US6664060B2 (en) | 1999-09-02 | 2003-12-16 | 3M Innovative Properties Company | Arrays with mask layers and methods of manufacturing same |
| US6593089B2 (en) | 1999-09-02 | 2003-07-15 | 3M Innovative Properties Company | Arrays with mask layers and methods of manufacturing same |
| US6395483B1 (en) | 1999-09-02 | 2002-05-28 | 3M Innovative Properties Company | Arrays with mask layers |
| WO2001016370A1 (en) * | 1999-09-02 | 2001-03-08 | 3M Innovative Properties Company | Arrays with mask layers and methods of manufacturing same |
| US6451191B1 (en) | 1999-11-18 | 2002-09-17 | 3M Innovative Properties Company | Film based addressable programmable electronic matrix articles and methods of manufacturing and using the same |
| WO2001036958A1 (en) * | 1999-11-18 | 2001-05-25 | 3M Innovative Properties Company | Film based addressable programmable electronic matrix articles and methods of manufacturing and using the same |
| US7220344B2 (en) | 1999-11-18 | 2007-05-22 | 3M Innovative Properties Company | Film based addressable programmable electronic matrix articles and methods of manufacturing and using the same |
| US6881538B1 (en) * | 2000-03-05 | 2005-04-19 | 3M Innovative Properties Company | Array comprising diamond-like glass film |
Also Published As
| Publication number | Publication date |
|---|---|
| US6063484A (en) | 2000-05-16 |
| EP0681507B1 (en) | 1997-05-28 |
| JPH08506601A (ja) | 1996-07-16 |
| CA2153319C (en) | 2003-11-11 |
| DE69403445D1 (de) | 1997-07-03 |
| EP0681507A1 (en) | 1995-11-15 |
| US5750245A (en) | 1998-05-12 |
| DE69403445T2 (de) | 1997-12-18 |
| CA2153319A1 (en) | 1994-08-04 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| EP0681507B1 (en) | Thermally induced phase separated azlactone membrane | |
| EP0214859B1 (en) | Microporous polymeric films and process for their manufacture | |
| US5486358A (en) | Azlactone-functional polymer blends, articles produced therefrom and methods for preparing both | |
| US5466747A (en) | Graft copolymers and graft copolymer/protein compositions | |
| JP3401726B2 (ja) | 分離工程用高分子ボディおよびその製造方法 | |
| EP0370260B1 (en) | Porous polymer beads and process | |
| HK10794A (en) | Thermoplastically processed solvent-resistant polymer blends | |
| WO1990004609A1 (en) | Process for the covalent surface modification of hydrophobic polymers and articles made therefrom | |
| US20030022994A1 (en) | Polymers having co-continuous architecture | |
| US5510421A (en) | Azlactone-functional membranes and methods of preparing and using same | |
| AU679257B2 (en) | Composite membranes and their preparation from polymer particles on a porous substrate | |
| US6245270B1 (en) | Process for the production of porous polyolefin | |
| JP2835342B2 (ja) | 分離膜及び分離方法 | |
| KR100513945B1 (ko) | 열가소성 조성물에서 에폭시드 관능기를 갖는 잔류단량체의 트랩핑 방법 | |
| CN1655864A (zh) | 用于微型过滤器的过滤材料 | |
| HK1006845B (en) | Graft copolymers and graft copolymer/protein compositions | |
| AU2002226185A1 (en) | Polymers having co-continuous architecture |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| AK | Designated states |
Kind code of ref document: A1 Designated state(s): CA CZ JP KR NO US |
|
| AL | Designated countries for regional patents |
Kind code of ref document: A1 Designated state(s): AT BE CH DE DK ES FR GB GR IE IT LU MC NL PT SE |
|
| DFPE | Request for preliminary examination filed prior to expiration of 19th month from priority date (pct application filed before 20040101) | ||
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application | ||
| WWE | Wipo information: entry into national phase |
Ref document number: 2153319 Country of ref document: CA |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 1994907369 Country of ref document: EP |
|
| WWP | Wipo information: published in national office |
Ref document number: 1994907369 Country of ref document: EP |
|
| WWG | Wipo information: grant in national office |
Ref document number: 1994907369 Country of ref document: EP |