RU2577348C1 - Reinforced plaster-polysterene concrete mixture - Google Patents

Reinforced plaster-polysterene concrete mixture Download PDF

Info

Publication number
RU2577348C1
RU2577348C1 RU2014148875/03A RU2014148875A RU2577348C1 RU 2577348 C1 RU2577348 C1 RU 2577348C1 RU 2014148875/03 A RU2014148875/03 A RU 2014148875/03A RU 2014148875 A RU2014148875 A RU 2014148875A RU 2577348 C1 RU2577348 C1 RU 2577348C1
Authority
RU
Russia
Prior art keywords
mixture
polystyrene
gypsum
water
proportion
Prior art date
Application number
RU2014148875/03A
Other languages
Russian (ru)
Inventor
Александр Петрович Свинцов
Гази Халед Сариб Масри
Лариса Георгиевна Калашникова
Нина Александровна Егорова
Original Assignee
федеральное государственное автономное образовательное учреждение высшего образования "Российский университет дружбы народов" (РУДН)
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by федеральное государственное автономное образовательное учреждение высшего образования "Российский университет дружбы народов" (РУДН) filed Critical федеральное государственное автономное образовательное учреждение высшего образования "Российский университет дружбы народов" (РУДН)
Priority to RU2014148875/03A priority Critical patent/RU2577348C1/en
Application granted granted Critical
Publication of RU2577348C1 publication Critical patent/RU2577348C1/en

Abstract

FIELD: construction.
SUBSTANCE: invention relates to construction materials and can be used for making plaster-polysterene concrete articles used in bearing and enclosing structures of buildings. Reinforced plaster-polysterene concrete mixture containing the following components per 1 m3 of the mixture: Portland cement 10.0-50.0 kg, gypsum or anhydrite, or their mixture in any ratio 60.0-250.0 kg, tripoli or gaize, or diatomite, or their mixture in any ratio of 7-75 kg, crushed polystyrene or mixture in any ratio with foamed granulated polystyrene 0.70-0.98 m3, chrysotile asbestos fibre 10.0-25.0 kg, plasticising additive S-3 0.03-1.40 kg, 10 % solution of polyacrylamide 0.40-0.60 kg, water-soluble methyl cellulose ether or construction cellulose or carboxymethylated starch 0.01-0.05 kg, tartaric or citric, or hydroxyethylidene diphosphonic acid 0.01-0.20 kg, water 20.0-140.0 litres.
EFFECT: technical result consists in faster setting of the mixture, hardening and strength of products, characterised by low density, heat conductivity, high water resistance and frost resistance, recycling wastes of styrofoam.
1 cl, 5 ex

Description

Изобретение относится к области строительных материалов и может быть использовано для изготовления гипсополистиролбетонных изделий, применяемых в несущих и ограждающих конструкциях зданий.The invention relates to the field of building materials and can be used for the manufacture of gypsum-polystyrene concrete products used in the supporting and enclosing structures of buildings.

Одной из важнейших проблем современного строительства является возведение объектов с высокими энергосберегающими характеристиками. Для этого широко применяют полистиролбетонные смеси на основе гидравлического вяжущего. Для сокращения сроков строительства полистиролбетонную смесь целесообразно делать на основе быстротвердеющего вяжущего. Кроме того, в качестве компонентов целесообразно использовать отходы различной производственной и хозяйственной деятельности, что позволит с меньшей интенсивностью увеличивать антропогенную нагрузку на окружающую среду. Одним из направлений утилизации отходов является повторное использование полистирола из упаковочного материала в качестве заполнителя. Указанные отходы существенно загрязняют окружающую среду и занимают большие территории, исключая их из полезного использования. Для обеспечения равномерного распределения гранул полистирола в изделии и для предотвращения расслоения смеси при транспортировании и укладке ее армируют щелочестойким волокном, например базальтовым. Однако в настоящее время имеется более эффективное, в рассматриваемом аспекте, щелочеустойчивое вещество, например, из хризотил-асбеста.One of the most important problems of modern construction is the construction of facilities with high energy-saving characteristics. For this, polystyrene concrete mixtures based on a hydraulic binder are widely used. To reduce the construction time, it is advisable to make a polystyrene concrete mixture on the basis of a quick-hardening binder. In addition, it is advisable to use waste from various industrial and economic activities as components, which will allow increasing the anthropogenic pressure on the environment with less intensity. One of the directions of waste disposal is the reuse of polystyrene from packaging material as a filler. These wastes significantly pollute the environment and occupy large areas, excluding them from useful use. To ensure uniform distribution of polystyrene granules in the product and to prevent delamination of the mixture during transportation and laying, it is reinforced with an alkali-resistant fiber, such as basalt. However, at present there is a more effective, in the considered aspect, alkali-resistant substance, for example, from chrysotile asbestos.

Известна полистиролбетонная смесь (патент РФ №2338725 С04В 38/08 от 20.11.2009 г.), содержащая массовую часть: портландцемент 10,0-15,0; водоудерживающую добавку - водорастворимый полимер на основе эфира целлюлозы 0,02-0,06; гранулированный пенополистирол - фракций 0,8-1,3 мм - 0,1-0,2, 1,6-2,0 мм - 0,3-0,8; 2,4-3,0 мм - 0,1-0,3.Known polystyrene concrete mixture (RF patent No. 2338725 С04В 38/08 from 11/20/2009), containing the mass part: Portland cement 10.0-15.0; water-holding additive - a water-soluble cellulose ether polymer 0.02-0.06; granular polystyrene foam - fractions 0.8-1.3 mm - 0.1-0.2, 1.6-2.0 mm - 0.3-0.8; 2.4-3.0 mm - 0.1-0.3.

Известна смесь к способу изготовления полистиролбетонных изделий (патент РФ №2223931 С04В 38/08 от 20.02.2004 г.), включающая компоненты, масса %: портландцемент - 68-70; вспененный полистирол - 3-6; смола древесная омыленная (на сухое вещество) - 0,02-0,1; пластифицирующая добавка (на сухое вещество) - 0,1-0,2; вода - остальное; армирующий материал в виде нитей и прутков (сверх 100%) - 5-12, при этом армирующий материал установлен в опалубке, куда подают полистиролбетонную смесь, а нити и прутки армирующего материала имеют диаметр, равный (0,5-3) среднего диаметра гранул полистирола, и связаны поперечными прутками диаметром (1-4) среднего диаметра гранул полистирола.A known mixture to a method for the manufacture of polystyrene concrete products (RF patent No. 2223931 С04В 38/08 of 02/20/2004), including components, mass%: Portland cement - 68-70; expanded polystyrene - 3-6; saponified wood resin (on dry matter) - 0.02-0.1; plasticizing additive (dry matter) - 0.1-0.2; water - the rest; the reinforcing material in the form of threads and rods (in excess of 100%) is 5-12, while the reinforcing material is installed in the formwork where the polystyrene concrete mixture is fed, and the threads and rods of the reinforcing material have a diameter equal to (0.5-3) the average diameter of the granules polystyrene, and are connected by transverse rods with a diameter (1-4) of the average diameter of polystyrene granules.

Недостатком указанного решения является интенсивное образование усадочных трещин из-за того, что гранулы полистирола не связаны между собой армированием. Кроме того, применение в качестве вяжущего портландцемента обусловливает длительные сроки твердения и набора прочности.The disadvantage of this solution is the intensive formation of shrinkage cracks due to the fact that polystyrene granules are not interconnected by reinforcement. In addition, the use of Portland cement as a binder determines the long hardening and curing times.

Известен состав полистиролбетонной смеси (патент РФ №2150446 С04В 38/08 от 10.06.2000 г.), включающий массу %: минеральное вяжущее - 68-90; полистирольный заполнитель - 0,7-2,3; волокнистый материал - 1,4-5,2; воздухововлекающую добавку - 0,3-0,7; пластифицирующую добавку - 0,25-0,55 и воду - остальное, причем в качестве полистирольного заполнителя он содержит смесь частиц из вспененных полистирольных гранул фракции 0,04-1,25 мм и/или частиц рваного пенополистирола фракции 0,04-1,63 мм при их массовом отношении 1:(8-12). В качестве армирующего волокнистого материала предусмотрено щелочестойкое волокно (стекловолокно или минеральная вата).The known composition of the polystyrene concrete mixture (RF patent No. 2150446 С04В 38/08 from 10.06.2000,), including the mass%: mineral binder - 68-90; polystyrene aggregate - 0.7-2.3; fibrous material - 1.4-5.2; air-entraining additive - 0.3-0.7; a plasticizing additive - 0.25-0.55 and water - the rest, moreover, as a polystyrene aggregate it contains a mixture of particles of expanded polystyrene granules of a fraction of 0.04-1.25 mm and / or particles of torn polystyrene foam of a fraction of 0.04-1, 63 mm with a mass ratio of 1: (8-12). Alkali-resistant fiber (fiberglass or mineral wool) is provided as a reinforcing fibrous material.

Недостатком указанной смеси является высокая трудоемкость формования гомогенной массы, что обусловливает низкое качество изделий из-за образования усадочных трещин. Кроме того, для изготовления изделий из смеси по указанному составу необходима термическая обработка, что приводит к потребности в энергоресурсах.The disadvantage of this mixture is the high complexity of molding a homogeneous mass, which leads to low quality products due to the formation of shrinkage cracks. In addition, for the manufacture of products from a mixture of the specified composition requires heat treatment, which leads to the need for energy.

Прототипом заявляемого состава является армированная полистиролбетонная смесь (патент РФ №2309134 С04В 38/08 от 27.10.2007 г.), включающая кг/м3: портландцемент - 160-170; полистирольный заполнитель - 15-17; щелочестойкое минеральное волокно в виде базальтового волокна - 0,5-0,7; структурообразующую добавку в виде полиакриламида (10%-й раствор) - 0,4-0,6; пластифицирующую добавку С-3 - 1,5-2,5; регулятор твердения лигнопан Б-2 - 0,35-0,50; воду - 50-55.The prototype of the claimed composition is a reinforced polystyrene concrete mixture (RF patent No. 2309134 С04В 38/08 from 10/27/2007), including kg / m 3 : Portland cement - 160-170; polystyrene aggregate - 15-17; alkali-resistant mineral fiber in the form of basalt fiber - 0.5-0.7; structure-forming additive in the form of polyacrylamide (10% solution) - 0.4-0.6; plasticizing additive C-3 - 1.5-2.5; hardening regulator lignopane B-2 - 0.35-0.50; water - 50-55.

Недостатком прототипа является большой срок схватывания, твердения смеси и набора прочности изделиями из нее. Начало срока схватывания не ранее 45 мин, окончание - не позднее, чем через 10 часов. Нормативная прочность определяется через 28 суток. Для сокращения срока схватывания в прототипе предусмотрен ускоритель-пластификатор лигнопан Б-2. Однако, даже при использовании ускорителя-пластификатора распалубить изделие возможно не ранее, чем через 24 часа после укладки смеси. Это не позволяет сокращать технологическую продолжительность изготовления изделий, например, штучных блоков, панелей, а также монолитных конструкций, например, стен, перегородок, утеплителей и пр. Большая продолжительность изготовления изделий также является недостатком прототипа.The disadvantage of the prototype is the long hardening, hardening of the mixture and the set of strength products from it. The beginning of the setting period is not earlier than 45 minutes, the end - no later than 10 hours. Standard strength is determined after 28 days. To reduce the setting time in the prototype provides an accelerator-plasticizer lignopane B-2. However, even when using an accelerator-plasticizer, it is possible to dismantle the product no earlier than 24 hours after laying the mixture. This does not allow to reduce the technological duration of the manufacture of products, for example, piece blocks, panels, as well as monolithic structures, for example, walls, partitions, insulation, etc. The long production time of products is also a disadvantage of the prototype.

Недостатком прототипа является также интенсивное образование усадочных трещин из-за невозможности создать гомогенную смесь. Невозможность создания гомогенной смеси обусловлена тем, что при перемешивании компонентов хрупкие базальтовые волокна ломаются, измельчаются и после этого не являются армирующими элементами, связывающими между собой гранулы полистирольного заполнителя. Неравномерное распределение гранул заполнителя по объему формуемых изделий приводит к снижению их прочности и ухудшению теплотехнических характеристик.The disadvantage of the prototype is also the intense formation of shrinkage cracks due to the inability to create a homogeneous mixture. The impossibility of creating a homogeneous mixture is due to the fact that when the components are mixed, the fragile basalt fibers break, are crushed and after that they are not reinforcing elements that bind together polystyrene aggregate granules. The uneven distribution of aggregate granules in the volume of the molded products leads to a decrease in their strength and deterioration of thermal characteristics.

Недостатком прототипа является также невозможность утилизации отходов дробленого полистирола от упаковочного и теплоизоляционного материала, накапливающегося на полигонах захоронения (на свалках).The disadvantage of the prototype is the inability to dispose of waste polished polystyrene from packaging and heat-insulating material that accumulates in landfills (landfills).

Техническим результатом изобретения является сокращение сроков схватывания гипсополистирольной смеси, ее твердения и набора прочности в изделиях, свойства которых характеризуются низкой плотностью и теплопроводностью, а также высокой водостойкостью и морозостойкостью в сочетании с прочностными показателями для изделий с плотностью 100-500 кг/м3. Техническим результатом изобретения является также возможность утилизации отходов пенополистирола из упаковочных и теплоизоляционных элементов.The technical result of the invention is to reduce the setting time of the gypsum-polystyrene mixture, its hardening and strength gain in products whose properties are characterized by low density and thermal conductivity, as well as high water resistance and frost resistance in combination with strength indicators for products with a density of 100-500 kg / m 3 . The technical result of the invention is also the possibility of recycling polystyrene waste from packaging and insulating elements.

Технический результат достигается тем, что состав для получения армированной гипсополистиролбетонной смеси включает портландцемент, полистирольный заполнитель, щелочестойкое минеральное волокно, 10%-ный раствор полиакриламида, пластифицирующую добавку С-3, регулятор твердения, воду, гипс или ангидрит, или их смесь в любой пропорции, водорастворимый эфир метилцеллюлозы или целлюлозу строительную, или карбоксиметилированный крахмал, а в качестве полистирольного заполнителя - дробленый полистирол или смесь в любой пропорции со вспененным полистиролом, в качестве щелочестойкого минерального волокна - хризотил-асбестовое волокно, в качестве регулятора твердения - винную, или лимонную, или оксиэтилидендифосфоновую кислоту, а компоненты имеют следующее соотношение на 1 м3 смеси: портландцемент, кг - 10,0-50,0; гипс или ангидрит или их смесь в любой пропорции, кг - 60,0-250,0; дробленый полистирол или смесь в любой пропорции со вспененным гранулированным полистиролом, м3 - 0,70-0,98; хризотил-асбестовое волокно, кг - 10,0-25,0; пластифицирующая добавка С-3, кг - 0,03-1,40; 10%-ный раствор полиакриламида, кг - 0,40-0,60; водорастворимый эфир метилцеллюлозы или целлюлоза строительная, или карбоксиметилированный крахмал, кг - 0,01-0,05; винная, или лимонная, или оксиэтилидендифосфоновая кислота, кг - 0,01-0,20; трепел или опока, или диатомит, или их смесь в любой пропорции, кг - 7-75; вода, л - 20,0-140,0.The technical result is achieved in that the composition for producing reinforced gypsum-polystyrene concrete mixture includes Portland cement, polystyrene aggregate, alkali-resistant mineral fiber, 10% polyacrylamide solution, plasticizing additive C-3, hardening regulator, water, gypsum or anhydrite, or a mixture of any proportion , water-soluble methyl cellulose ether or construction cellulose, or carboxymethyl starch, and crushed polystyrene or a mixture in any proportion with foamed foam as a filler m polystyrene, as an alkali-resistant mineral fiber - chrysotile asbestos fiber, as a hardening regulator - tartaric, or citric, or hydroxyethylidene diphosphonic acid, and the components have the following ratio per 1 m 3 of the mixture: Portland cement, kg - 10.0-50.0 ; gypsum or anhydrite or a mixture thereof in any proportion, kg - 60.0-250.0; crushed polystyrene or a mixture in any proportion with foamed granular polystyrene, m 3 - 0.70-0.98; chrysotile asbestos fiber, kg - 10.0-25.0; plasticizing additive C-3, kg - 0.03-1.40; 10% solution of polyacrylamide, kg - 0.40-0.60; water-soluble methyl cellulose ether or construction cellulose, or carboxymethylated starch, kg - 0.01-0.05; tartaric or citric or hydroxyethylidene diphosphonic acid, kg - 0.01-0.20; tripoli or flask, or diatomite, or their mixture in any proportion, kg - 7-75; water, l - 20.0-140.0.

Указанный качественный и количественный состав обеспечивает возможность получения простым способом гипсополистиролбетонной смеси с равномерным распределением гранул по объему и с минимальными усадочными деформациями, не расслаивающуюся и не схватывающуюся в течение прогнозируемого времени, достаточного для транспортировки от места приготовления и затворения смеси до места ее укладки и изготовления изделия.The specified qualitative and quantitative composition makes it possible to obtain in a simple way a gypsum-polystyrene concrete mixture with uniform distribution of granules in volume and with minimal shrinkage deformations, not delaminating and not setting during the predicted time, sufficient for transportation from the place of preparation and mixing of the mixture to the place of its laying and manufacturing of the product .

Содержание компонентов в составе смеси ниже или выше указанных пределов негативно отражается на устойчивости к расслоению, легкости перемешивания компонентов, удобоукладываемости затворенной смеси, прочности, теплопроводности, водо- и морозостойкости изделий из гипсополистиролбетонной смеси по заявляемому техническому решению.The content of the components in the mixture below or above the specified limits negatively affects the resistance to delamination, ease of mixing of the components, workability of the closed mixture, strength, thermal conductivity, water and frost resistance of products made of gypsum-polystyrene concrete mixture according to the claimed technical solution.

Минеральное вяжущее в гипсополистиролбетонной смеси состоит из смеси портландцемента, гипса или ангидрита или их смеси в любой пропорции, минеральной добавки (трепела или опоки, или диатомита, или их смеси в любой пропорции) и предназначено для скрепления между собой элементов дробленого или гранулированного полистирола, или их смеси, армированных щелочестойким минеральным волокном. При затворении водой минеральное вяжущее образует удобообрабатываемое тесто, способное к адгезии как к полистиролу, так и к щелочестойкому минеральному волокну, и затвердевающее в воде и на воздухе. Состав минерального вяжущего включает смесь в соотношении, кг/м3: (10-50):(60-250):(7-75) портландцемента с гипсом полуводным или с ангидритом, или с их смесью в любой пропорции и трепела или опоки, или диатомита, или их смеси в любой пропорции.The mineral binder in the gypsum-polystyrene concrete mixture consists of a mixture of Portland cement, gypsum or anhydrite or any mixture thereof in any proportion, a mineral additive (tripoli or flask, or diatomite, or their mixture in any proportion) and is intended for bonding together elements of crushed or granular polystyrene, or mixtures thereof, reinforced with alkali-resistant mineral fiber. When mixed with water, the mineral binder forms a conveniently processed dough, capable of adhesion to both polystyrene and alkali-resistant mineral fiber, and hardens in water and in air. The composition of the mineral binder includes a mixture in the ratio, kg / m 3 : (10-50) :( 60-250) :( 7-75) Portland cement with gypsum, semi-aquatic or with anhydrite, or any mixture thereof in any proportion and tripoli or flask, or diatomite, or mixtures thereof in any proportion.

Портландцемент включен в состав смеси для придания минеральному вяжущему свойств гидравлического вяжущего, а также для обеспечения требуемых прочностных характеристик изделия, регулируемых количеством вводимого материала. Количество портландцемента, включаемого в минеральное вяжущее по заявляемому решению составляет от 10 до 50 кг/м3.Portland cement is included in the composition of the mixture to give the mineral binder the properties of a hydraulic binder, as well as to provide the required strength characteristics of the product, controlled by the amount of input material. The amount of Portland cement included in the mineral binder according to the claimed solution is from 10 to 50 kg / m 3 .

Обоснование количественных пределов портландцемента в составе минерального вяжущего по заявляемому решению.Justification of the quantitative limits of Portland cement in the composition of the mineral binder according to the claimed solution.

Нижний предел количества портландцемента (10 кг на 1 м3 смеси) обусловлен тем, что при меньшем количестве гипс не приобретает свойства гидравлического вяжущего и не может быть использован при изготовлении изделий, к которым предъявляются требования по водостойкости.The lower limit of the amount of Portland cement (10 kg per 1 m 3 of the mixture) is due to the fact that with a smaller amount of gypsum it does not acquire the properties of a hydraulic binder and cannot be used in the manufacture of products requiring water resistance.

Превышение верхнего значения количества добавляемого портландцемента (50 кг на 1 м3 смеси) не приводит к улучшению свойств водостойкости. Добавление гидравлического вяжущего в указанных количествах позволяет получать изделия из гипсополистиролбетона со свойствами, соответствующими задаче изобретения.Exceeding the upper value of the amount of added Portland cement (50 kg per 1 m 3 of the mixture) does not lead to an improvement in the water resistance properties. The addition of a hydraulic binder in the indicated amounts makes it possible to obtain products from gypsum-polystyrene concrete with properties corresponding to the objective of the invention.

Гипс как основное минеральное вяжущее предназначен для скрепления зерен полистирола в единую массу с определенной прочностью после твердения. Количество гипса составляет 60-250 кг/м3. Для практического применения наиболее целесообразно применение строительного полуводного гипса. По сравнению с гидравлическим вяжущим, применяемым в аналогах, гипс позволяет существенно сократить сроки набора распалубочной прочности смеси и повысить интенсивность технологического процесса изготовления изделий. Вместо полуводного гипса смесь может включать ангидрит в том же количестве или их смесь в любой пропорции.Gypsum as the main mineral binder is intended for bonding polystyrene grains into a single mass with a certain strength after hardening. The amount of gypsum is 60-250 kg / m 3 . For practical use, the most appropriate is the use of semi-aquatic gypsum construction. Compared with the hydraulic binder used in analogues, gypsum can significantly reduce the time required to set the stripping strength of the mixture and increase the intensity of the manufacturing process. Instead of semi-aquatic gypsum, the mixture may include anhydrite in the same amount or any mixture in any proportion.

Обоснование пределов количества гипса в смеси.Justification of the limits of the amount of gypsum in the mixture.

Введение в состав смеси количества гипса меньше нижнего значения (60 кг на 1 м3 смеси) приводит к тому, что часть пустот между зернами полистирола остается незаполненной вяжущим. В результате наблюдается расслоение смеси и снижение ее прочностных показателей. При использовании количества гипса больше верхнего значения (250 кг на 1 м3 смеси) увеличивается объемная масса изделия с существенным ухудшением теплотехнических характеристик.The introduction of the amount of gypsum into the mixture is less than the lower value (60 kg per 1 m 3 of the mixture) leads to the fact that part of the voids between the grains of polystyrene remains unfilled with a binder. As a result, delamination of the mixture and a decrease in its strength indicators are observed. When using the amount of gypsum more than the upper value (250 kg per 1 m 3 of the mixture), the bulk mass of the product increases with a significant deterioration in the thermal characteristics.

Минеральная добавка в виде трепела или опоки, или диатомита, или их смеси в любой пропорции необходима для придания минеральному вяжущему свойств гидравлического вяжущего. Количество минеральной добавки составляет от 7 до 75 кг на 1 м3 смеси.A mineral additive in the form of tripoli or flask, or diatomite, or a mixture thereof in any proportion is necessary to give the mineral binder the properties of a hydraulic binder. The amount of mineral additives is from 7 to 75 kg per 1 m 3 of the mixture.

При введении указанной минеральной добавки в количестве менее 7 кг на 1 м3 смеси свойства гидравлического вяжущего у минерального вяжущего не проявляются. Это не позволяет получить искомый технический результат.When this mineral additive is introduced in an amount of less than 7 kg per 1 m 3 of the mixture, the properties of the hydraulic binder in the mineral binder do not appear. This does not allow to obtain the desired technical result.

При введении указанной минеральной добавки в количестве более 75 кг на 1 м3 смеси снижаются прочностные и теплоизоляционные свойства изделий из заявляемой смеси. Это не позволяет получить искомый технический результат.With the introduction of the specified mineral additives in an amount of more than 75 kg per 1 m 3 of the mixture, the strength and thermal insulation properties of the products from the inventive mixture are reduced. This does not allow to obtain the desired technical result.

Полистирольный заполнитель, получаемый посредством измельчения полистирольного упаковочного материала или в виде вспененного полистирола, необходим для придания изделиям высоких теплотехнических свойств. Диапазон количества полистирола обусловлен необходимостью изготовления изделий с заранее запроектированными теплотехническими и физико-механическими характеристиками.Polystyrene aggregate, obtained by grinding polystyrene packaging material or in the form of expanded polystyrene, is necessary to give products high thermal properties. The range of polystyrene quantities is due to the need to manufacture products with pre-designed thermotechnical and physico-mechanical characteristics.

Обоснование количественных пределов полистирольного заполнителя.Justification of the quantitative limits of polystyrene aggregate.

Нижнее значение (0,7 м3 на 1 м3 смеси) обусловлено необходимостью равномерного заполнения всего объема полистирольным заполнителем и объединением его гранул в единый структурный массив. Если количество полистирола будет меньше нижнего предела, то изделие не будет обладать требуемыми теплотехническими свойствами.The lower value (0.7 m 3 per 1 m 3 of the mixture) is due to the need to uniformly fill the entire volume with a polystyrene aggregate and the union of its granules into a single structural array. If the amount of polystyrene is less than the lower limit, the product will not have the required thermal properties.

Верхнее значение количества полистирольного заполнителя (0,98 м3 на 1 м3 смеси) обусловлено тем, что его превышение в массиве приводит к образованию областей, недостаточно покрытых вяжущим, вследствие чего образуется расслоение смеси и существенное снижение прочностных показателей и невозможности формирования и изготовления изделий.The upper value of the amount of polystyrene aggregate (0.98 m 3 per 1 m 3 of the mixture) is due to the fact that its excess in the array leads to the formation of areas insufficiently covered with binders, as a result of which stratification of the mixture and a significant decrease in strength indicators and the impossibility of forming and manufacturing products .

Применение полистирольного заполнителя в указанном количественном диапазоне позволяет получать гипсополистиролбетонную смесь и изделия из нее в соответствии с задачами изобретения.The use of polystyrene aggregate in the specified quantitative range allows to obtain a gypsum-polystyrene concrete mixture and products from it in accordance with the objectives of the invention.

Щелочестойкое минеральное волокно необходимо для объединения гранул полистирольного заполнителя в единый структурный массив, а также для уменьшения усадочных деформаций и образования усадочных трещин. В качестве щелочестойкого минерального волокна гипсополистиролбетонная смесь содержит хризотил-асбестовое волокно. Хризотил-асбестовое волокно обладает высокой адгезионной способностью к тесту минерального вяжущего. Будучи гибким, хризотил-асбестовое волокно обладает способностью обволакивать элементы полистирольного заполнителя, армируя его. При твердении минерального вяжущего указанные свойства хризотил-асбестового волокна позволяют получать гомогенную гипсополистиролбетонную смесь и изделия из нее без усадочных трещин и деформаций. Хризотил-асбестовое волокно эластично и характеризуется высокой прочностью на растяжение. Это позволяет использовать его в качестве материала, армирующего гипсопенополистиролбетонные изделия, как связующего элемента между гранулами пенополистирола при высокой адгезии к минеральному вяжущему.Alkali-resistant mineral fiber is necessary for combining polystyrene aggregate granules into a single structural array, as well as to reduce shrinkage deformation and the formation of shrinkage cracks. As an alkali-resistant mineral fiber, the gypsum-polystyrene concrete mixture contains chrysotile asbestos fiber. Chrysotile asbestos fiber has a high adhesive ability to test mineral binder. Being flexible, chrysotile asbestos fiber has the ability to envelop the elements of polystyrene aggregate, reinforcing it. When hardening a mineral binder, the indicated properties of chrysotile asbestos fiber make it possible to obtain a homogeneous gypsum-polystyrene concrete mixture and products from it without shrinkage cracks and deformations. Chrysotile asbestos fiber is elastic and has high tensile strength. This allows you to use it as a material reinforcing gypsum polystyrene concrete products, as a bonding element between polystyrene foam granules with high adhesion to a mineral binder.

Обоснование количества хризотил-асбестового волокна в составе гипсополистирольной смеси.Justification of the amount of chrysotile asbestos fiber in the composition of the gypsum-polystyrene mixture.

Нижний предел количества щелочестойкого минерального волокна (хризотил-асбестового волокна) (10 кг на 1 м3 смеси) объясняется тем, что при использовании меньшего количества армирование частиц дробленого или гранулированного полистирола не обеспечивается по всему массиву. Это приводит к образованию не связанных волокном областей гипсополистирольной смеси и снижению прочности получаемых изделий из-за расслоения смеси и усадочных деформаций. Указанный недостаток не позволяет получать гипсопенополистиролбетонные изделия высокого качества с минимальными трудозатратами.The lower limit of the amount of alkali-resistant mineral fiber (chrysotile asbestos fiber) (10 kg per 1 m 3 of the mixture) is explained by the fact that when using a smaller amount, the reinforcement of crushed or granular polystyrene particles is not provided throughout the array. This leads to the formation of non-fiber-bonded areas of the gypsum-polystyrene mixture and a decrease in the strength of the resulting products due to delamination of the mixture and shrinkage deformations. The specified disadvantage does not allow to obtain high-quality gypsum-polystyrene concrete products with minimal labor costs.

Верхний предел количества хризотил-асбестового волокна (25 кг на 1 м3 смеси) объясняется тем, что его превышение не приводит к улучшению физико-механических и теплотехнических характеристик изделий из армированного гипсопенополистиролбетона по заявляемому решению.The upper limit of the amount of chrysotile asbestos fiber (25 kg per 1 m 3 of the mixture) is explained by the fact that exceeding it does not lead to an improvement in the physicomechanical and thermotechnical characteristics of products made of reinforced gypsum-foam polystyrene according to the claimed solution.

Пластифицирующая добавка С-3 предназначена для обеспечения лучшего перемешивания смеси и ее удобоукладываемости (ГОСТ 24211-91. Добавки для бетонов. Общие технические требования). Суперпластификатор С-3 представляет собой смесь нейтрализованных едким натром полимерных соединений, получаемых при конденсации сульфокислот нафталина с формальдегидом. Выпускается в сухом (порошок коричневого цвета) и жидком виде.Plasticizing additive C-3 is designed to provide better mixing of the mixture and its workability (GOST 24211-91. Additives for concrete. General technical requirements). Superplasticizer C-3 is a mixture of polymer compounds neutralized with sodium hydroxide obtained by condensation of naphthalene sulfonic acids with formaldehyde. Available in dry (brown powder) and liquid form.

Обоснование количественных пределов пластифицирующей добавки.Justification of the quantitative limits of plasticizing additives.

Применение пластификатора в меньшем количестве, чем минимальное значение (0,03 кг на 1 м3 смеси), приводит к неэффективности добавки, т.к. она практически не оказывает влияния на свойства смеси.The use of plasticizer in a smaller amount than the minimum value (0.03 kg per 1 m 3 of the mixture) leads to the inefficiency of the additive, because it has practically no effect on the properties of the mixture.

Превышение верхнего значения количества пластификатора (1,40 кг на 1 м3 смеси) приводит к повышенному трещинообразованию из-за усадочных напряжений.Exceeding the upper value of the amount of plasticizer (1.40 kg per 1 m 3 of the mixture) leads to increased cracking due to shrink stresses.

Полиакриламид предназначен для улучшения условий объединения частиц дробленого или гранулированного полистирола, покрытых слоем затворенного минерального вяжущего, с хризотил-асбестовым волокном в конгломераты. В практических целях используют 10%-ный водный раствор полиакриламида, который необходим для структурирования и консолидации зерен пенополистирола. Без применения полиакриламида зерна полистирола трудно поддаются перемешиванию с вяжущим из-за разницы в объемной массе. Добавление водного раствора полиакриламида позволяет сформировать единую структуру из зерен полистирола и обеспечить хорошее перемешивание. Совместно с армированием хризотил-асбестовым волокном полиакриламид хорошо структурирует массив заполнителя и не позволяет зернам всплывать в массиве вяжущего при перемешивании.Polyacrylamide is intended to improve the conditions for combining particles of crushed or granular polystyrene coated with a layer of closed mineral binder with chrysotile asbestos fiber into conglomerates. For practical purposes, use a 10% aqueous solution of polyacrylamide, which is necessary for the structuring and consolidation of polystyrene grains. Without the use of polyacrylamide, polystyrene grains are difficult to mix with a binder due to the difference in bulk density. Adding an aqueous solution of polyacrylamide allows you to form a single structure of polystyrene grains and provide good mixing. Together with reinforcement with chrysotile asbestos fiber, polyacrylamide well structures the aggregate mass and does not allow the grains to float in the binder mass with stirring.

Обоснование количественного диапазона структурообразующей добавки (полиакриламида).The rationale for the quantitative range of structure-forming additives (polyacrylamide).

Нижнее значение количества 10%-ного водного раствора полиакриламида (0,40 кг на 1 м3 смеси) обусловлено необходимостью смачивания и обволакивания зерен полистирола раствором с минимальной толщиной пленки. Выход за нижнее значение количества раствора полиакриламида приводит к тому, что его недостаточно для смачивания всей массы зерен полистирола, и часть ее остается необработанной и не структурированной.The lower value of the amount of a 10% aqueous solution of polyacrylamide (0.40 kg per 1 m 3 of the mixture) is due to the need for wetting and enveloping the polystyrene grains with a solution with a minimum film thickness. Going beyond the lower value of the amount of polyacrylamide solution leads to the fact that it is not enough to wet the entire mass of polystyrene grains, and part of it remains untreated and unstructured.

Верхнее значение количества водного раствора полиакриламида (0,60 кг на 1 м3 смеси) обусловлено тем, что при большем количестве полистирола требуется и большее количество структурообразующей добавки. Превышение указанного количества приводит к затруднению условий перемешивания без улучшения структуры полистирольного массива.The upper value of the amount of an aqueous solution of polyacrylamide (0.60 kg per 1 m 3 of the mixture) is due to the fact that with a larger amount of polystyrene, a larger amount of a structure-forming additive is required. Exceeding the specified amount leads to difficult mixing conditions without improving the structure of the polystyrene array.

Применение 10%-ного водного раствора полиакриламида в указанном количественном диапазоне позволяет получить гипсополистирольную смесь и изделия из нее с заданными теплотехническими и физико-механическими характеристиками, соответствующими задачам изобретения.The use of a 10% aqueous solution of polyacrylamide in the indicated quantitative range makes it possible to obtain a gypsum-polystyrene mixture and products from it with specified thermal and physical-mechanical characteristics corresponding to the objectives of the invention.

Стабилизатор-пластификатор предназначен для придания смеси свойств пластичности и удобоукладываемости при изготовлении изделий из армированного гипсополистиролбетона, а также стабилизации химических реакций при наборе прочности. В качестве стабилизатора-пластификатора может быть использована метилцеллюлоза (водорастворимый эфир целлюлозы) или метилцеллюлоза строительная, или карбоксиметилированный крахмал.The stabilizer-plasticizer is intended to impart a mixture of plasticity and workability properties in the manufacture of products from reinforced gypsum polystyrene concrete, as well as stabilizing chemical reactions during curing. Methylcellulose (a water-soluble cellulose ether) or construction methylcellulose, or carboxymethylated starch can be used as a plasticizer stabilizer.

Обоснование количественных пределов стабилизатора-пластификатора.Justification of the quantitative limits of the stabilizer-plasticizer.

Выход за нижний предел количества (0,01 кг на 1 м3 смеси) водорастворимого эфира целлюлозы, или карбоксиметилированного крахмала, или их бинарной смеси приводит к тому, что в процессе твердения изделия и набора прочности наблюдается образование трещин из-за быстрого изменения усадочных деформаций, что приводит к значительному снижению теплотехнических, физико-механических характеристик армированного гипсополистиролбетона.Exceeding the lower limit of the amount (0.01 kg per 1 m 3 of the mixture) of water-soluble cellulose ether or carboxymethylated starch, or their binary mixture, leads to the formation of cracks during the hardening of the product and the set of strength due to a rapid change in shrinkage deformations , which leads to a significant decrease in heat engineering, physico-mechanical characteristics of reinforced gypsum-polystyrene concrete.

Применение стабилизатора-пластификатора больше верхнего предела (0,05 кг на 1 м3 смеси) приводит к чрезмерной пластификации смеси и к значительному торможению набора прочности после твердения смеси в изделии.The use of a stabilizer-plasticizer greater than the upper limit (0.05 kg per 1 m 3 of the mixture) leads to excessive plasticization of the mixture and to a significant inhibition of the set of strength after hardening of the mixture in the product.

Регулятор сроков схватывания, например, винная кислота, или лимонная кислота, или оксиэтилидендифосфоновая кислота, предназначен для обеспечения возможности замедления скорости химических реакций армированной гипсополистиролбетонной смеси и, соответственно, регулирования технологического процесса изготовления изделий.The setting time regulator, for example, tartaric acid, or citric acid, or hydroxyethylidene diphosphonic acid, is designed to provide the ability to slow down the rate of chemical reactions of reinforced gypsum-polystyrene concrete mixture and, accordingly, regulate the technological process of manufacturing products.

Обоснование количественного диапазона регулятора сроков схватывания.Justification of the quantitative range of the setting time regulator.

Использование винной, или лимонной кислоты, или оксиэтилидендифосфоновой кислоты в количестве меньше, чем нижнее значение (0,01 кг на 1 м3 смеси), приводит к тому, что скорость схватывания гипса практически не изменяется.The use of tartaric or citric acid or hydroxyethylidene diphosphonic acid in an amount less than the lower value (0.01 kg per 1 m 3 of the mixture) leads to the fact that the setting speed of gypsum practically does not change.

Применение винной или лимонной, или оксиэтилидендифосфоновая кислоты в большем количестве, чем верхнее значение (0,2 кг на 1 м3 смеси), приводит к неоправданному увеличению сроков схватывания и твердения смеси, обусловливая ничтожность эффективности гипса как минерального вяжущего.The use of tartaric or citric or hydroxyethylidene diphosphonic acid in a larger quantity than the upper value (0.2 kg per 1 m 3 of the mixture) leads to an unjustified increase in the setting and hardening of the mixture, causing the effectiveness of gypsum as a mineral binder.

Вода необходима для затворения минерального вяжущего и химических реакций между компонентами смеси.Water is necessary for mixing mineral binder and chemical reactions between the components of the mixture.

Обоснование количественного диапазона водыJustification of the quantitative range of water

Нижнее значение количества воды (20 л на 1 м3 смеси) обусловлено необходимостью создания условий не только для химических реакций, но и обеспечения подвижности и удобоукладываемости смеси. Выход за пределы указанного значения приводит к снижению подвижности смеси, затруднению ее перемешивания без значимого улучшения качественных показателей изготавливаемых изделий.The lower value of the amount of water (20 l per 1 m 3 of the mixture) is due to the need to create conditions not only for chemical reactions, but also to ensure mobility and workability of the mixture. Going beyond the specified value leads to a decrease in the mobility of the mixture, the difficulty of mixing it without a significant improvement in the quality indicators of manufactured products.

Верхнее значение указанного количества воды (140 л на 1 м3 смеси) обусловлено необходимостью минимизировать усадочные деформации, а также необходимостью создания требуемой подвижности и удобоукладываемости смеси при использовании больших количеств компонентов смеси. Превышение указанного количества приводит к образованию значительных усадочных деформаций, следствием которых являются трещины в изделиях и неоднородность структуры материала.The upper value of the indicated amount of water (140 l per 1 m 3 of the mixture) is due to the need to minimize shrinkage deformation, as well as the need to create the required mobility and workability of the mixture when using large quantities of mixture components. Exceeding the specified amount leads to the formation of significant shrinkage deformations, which result in cracks in the products and heterogeneity of the material structure.

Использование смесей указанного состава с компонентами в указанных диапазонах позволяет изготавливать гипсополистирольные изделия с прочностью на сжатие 0,1-3,0 МПа с коэффициентом теплопроводности 0,071-0,082 Вт/(мК).The use of mixtures of the specified composition with components in the indicated ranges makes it possible to produce gypsum-polystyrene products with a compressive strength of 0.1-3.0 MPa with a thermal conductivity of 0.071-0.082 W / (mK).

Рецептура и количественные параметры компонентов армированной гипсополистиролбетонной смеси обусловлены конкретными требованиями, предъявляемыми к изделиям из нее. Например, количество портландцемента и его марка (400, 500, 600), количество гипса полуводного или ангидрита и их марка (Г-2, Г-3, Г-4, Г-5÷Г-25), количество дробленого полистирола, количество винной, или лимонной, или оксиэтилидендифосфоновой кислоты и др. составляют основу изготавливаемых изделий по объемной массе, по теплопроводности, по прочности, по технологичности и по другим показателям.The formulation and quantitative parameters of the components of the reinforced gypsum-polystyrene concrete mixture are determined by the specific requirements for products from it. For example, the amount of Portland cement and its grade (400, 500, 600), the amount of semi-aquatic gypsum or anhydrite and their grade (G-2, G-3, G-4, G-5 ÷ G-25), the amount of crushed polystyrene, the amount tartaric, or citric, or hydroxyethylidene diphosphonic acid, etc., make up the basis of manufactured products by volumetric mass, thermal conductivity, strength, manufacturability, and other indicators.

Варианты реализации армированных гипсополистиролбетонных смесей с различными характеристиками получаемых изделий представлены следующими примерами:Implementation options for reinforced gypsum-polystyrene concrete mixtures with various characteristics of the products obtained are presented by the following examples:

Пример 1 (на 1 м3 смеси)Example 1 (per 1 m 3 mixture)

Портландцемент марки 400Portland cement brand 400 10 кг10 kg Гипс полуводный Г5Gypsum semi-aquatic G5 60 кг60 kg ОпокаFlask 7 кг7 kg Дробленый полистиролCrushed polystyrene 0,90 м3 0.90 m 3 Хризотил-асбестовое волокноChrysotile Asbestos Fiber 12 кг12 kg Пластифицирующая добавка С-3Plasticizing additive C-3 0,03 кг0.03 kg 10%-ный раствор полиакриламида10% polyacrylamide solution 0,35 кг0.35 kg Целлюлоза строительнаяConstruction pulp 0,015 кг0.015 kg Винная кислотаWine acid 0,015 кг0.015 kg ВодаWater 23 л23 l

При перемешивании в растворосмесителе отмечена большая разрозненность частиц дробленого полистирола, а также расслоение полистирола и минерального вяжущего. При детальном анализе установлено, что многие зерна полистирола остались не покрыты пленкой из водного раствора полиакриламида. Это привело к невозможности объединения частиц в конгломераты и структуры, в которых частицы полистирола были бы связаны между собой посредством хризотил-асбестового волокна в присутствии минерального вяжущего.When mixing in a mortar mixer, a large disintegration of crushed polystyrene particles was noted, as well as separation of polystyrene and mineral binder. A detailed analysis found that many polystyrene grains were not covered by a film from an aqueous solution of polyacrylamide. This led to the impossibility of combining particles into conglomerates and structures in which polystyrene particles would be interconnected via chrysotile asbestos fiber in the presence of a mineral binder.

При ручном перемешивании данного состава в лабораторных условиях указанные недостатки были несколько снижены. Однако полученное изделие характеризуется низкой гомогенностью. В целом полученная смесь в нормально сухом состоянии характеризуется осадкой конуса в среднем 7 см, сроком схватывания в среднем 31 мин. Изделия, полученные из данного состава смеси, имеют объемную массу в среднем 109 кг/м3 и прочность при сжатии 0,09 МПа, коэффициент теплопроводности 0,052 Вт/(м К).With manual mixing of this composition in laboratory conditions, these disadvantages were slightly reduced. However, the resulting product is characterized by low homogeneity. In general, the mixture obtained in a normally dry state is characterized by an average cone draft of 7 cm and a setting time of 31 minutes on average. Products obtained from this mixture composition have an average bulk density of 109 kg / m 3 and a compressive strength of 0.09 MPa, a thermal conductivity of 0.052 W / (m K).

Пример 2 (на 1 м3 смеси)Example 2 (per 1 m 3 mixture)

Портландцемент марки 500Portland cement brand 500 30 кг30 kg Гипс полуводный Г5Gypsum semi-aquatic G5 160 кг160 kg ТрепелTripoli 50 кг50 kg Вспененный полистиролPolystyrene foam 0,820 м3 0.820 m 3 Хризотил-асбестовое волокноChrysotile Asbestos Fiber 18 кг18 kg Пластифицирующая добавка С-3Plasticizing additive C-3 0,1 кг0.1 kg 10%-ный раствор полиакриламида10% polyacrylamide solution 0,40 кг0.40 kg Эфир метилцеллюлозы водорастворимыйWater soluble methyl cellulose ether 0,015 кг0.015 kg Лимонная кислотаLemon acid 0,06 кг0.06 kg ВодаWater 82 л82 l

При перемешивании в растворосмесителе полученного состава установлено, что гипсополиситрольная смесь гомогенна, частицы полистирола распределены равномерно. Полученная смесь имеет следующие свойства: осадка конуса в среднем 7 см, срок схватывания в среднем 42 мин. В нормально сухих условиях изделия, полученные из данного состава смеси, имеют объемную массу в среднем 290 кг/м3 и прочность при сжатии 0,35 МПа, коэффициент теплопроводности 0,071 Вт/(м К).When mixing in the mortar mixer of the obtained composition, it was found that the gypsopolysitrol mixture is homogeneous, the polystyrene particles are evenly distributed. The resulting mixture has the following properties: cone draft on average 7 cm, setting time on average 42 minutes. Under normally dry conditions, products obtained from this mixture composition have an average bulk density of 290 kg / m 3 and a compressive strength of 0.35 MPa, a thermal conductivity of 0.071 W / (m K).

Пример 3 (на 1 м3 смеси)Example 3 (per 1 m 3 mixture)

Портландцемент марки 500Portland cement brand 500 40 кг40 kg Смесь гипса полуводного Г5 и ангидрита (40:60%)A mixture of gypsum semi-aquatic G5 and anhydrite (40: 60%) 150 кг150 kg ДиатомитDiatomite 50 кг50 kg Смесь дробленого и вспененногоA mixture of crushed and foamed полистирола (50:50%)polystyrene (50: 50%) 0,820 м3 0.820 m 3 Хризотил-асбестовое волокноChrysotile Asbestos Fiber 18 кг18 kg Пластифицирующая добавка С-3Plasticizing additive C-3 0,1 кг0.1 kg 10%-ный раствор полиакриламида10% polyacrylamide solution 0,60 кг0.60 kg Карбоксиметилированный крахмалCarboxymethyl starch 0,04 кг0.04 kg Оксиэтилдендифосфоновая кислотаHydroxyethyl diphosphonic acid 0,15 кг0.15 kg ВодаWater 90 л90 l

При перемешивании полученного состава отмечено некоторое снижение подвижности смеси. Полученная смесь имеет следующие свойства: осадка конуса в среднем 8 см, срок схватывания в среднем 47 мин. Изделия, полученные из данного состава смеси, имеют объемную массу в среднем 310 кг/м3 и прочность при сжатии 0,65 МПа, коэффициент теплопроводности 0,08 Вт/(м К).When mixing the resulting composition, a slight decrease in the mobility of the mixture was noted. The resulting mixture has the following properties: cone draft on average 8 cm, setting time on average 47 minutes. Products obtained from this mixture composition have an average bulk density of 310 kg / m 3 and a compressive strength of 0.65 MPa, a thermal conductivity of 0.08 W / (m K).

Пример 4 (на 1 м3 смеси)Example 4 (per 1 m 3 mixture)

Портландцемент марки 400Portland cement brand 400 55 кг55 kg Смесь гипса полуводного Г5 и ангидрита (70:30%)A mixture of gypsum semi-aquatic G5 and anhydrite (70: 30%) 220 кг220 kg Смесь трепела и диатомита (40:60%)A mixture of tripoli and diatomite (40: 60%) 30 кг30 kg Смесь дробленого и вспененногоA mixture of crushed and foamed полистирола (85:15%)polystyrene (85: 15%) 0,8 м3 0.8 m 3 Хризотил-асбестовое волокноChrysotile Asbestos Fiber 20 кг20 kg Пластифицирующая добавка С-3Plasticizing additive C-3 0,20 кг0.20 kg 10%-ный раствор полиакриламида10% polyacrylamide solution 0,50 кг0.50 kg Целлюлоза строительнаяConstruction pulp 0,015 кг0.015 kg Винная кислотаWine acid 0,07 кг0.07 kg ВодаWater 120 л120 l

Полученная смесь характеризуется осадкой конуса в среднем 7 см, срок схватывания в среднем 6 мин. Изделия, полученные из данного состава смеси, имеют объемную массу в среднем 355 кг/м3 и прочность при сжатии 0,9 МПа, коэффициент теплопроводности 0,080 Вт/(м К).The resulting mixture is characterized by a cone draft of 7 cm on average, a setting time of 6 minutes on average. Products obtained from this mixture composition have an average bulk density of 355 kg / m 3 and a compressive strength of 0.9 MPa, a thermal conductivity of 0.080 W / (m K).

Пример 5 (на 1 м3 смеси)Example 5 (per 1 m 3 mixture)

Портландцемент марки 500Portland cement brand 500 40 кг40 kg Смесь гипса полуводного Г5 и ангидрита (50:50%)A mixture of gypsum semi-aquatic G5 and anhydrite (50: 50%) 150 кг150 kg Смесь трепела, диатомита и опоки (25:25:50%)A mixture of tripoli, diatomite and flask (25: 25: 50%) 50 кг50 kg Дробленый полистиролCrushed polystyrene 0,820 м3 0.820 m 3 Хризотил-асбестовое волокноChrysotile Asbestos Fiber 18 кг18 kg Пластифицирующая добавка С-3Plasticizing additive C-3 0,1 кг0.1 kg 10%-ный раствор полиакриламида10% polyacrylamide solution 0,55 кг0.55 kg Карбоксиметилированный крахмалCarboxymethyl starch 0,04 кг0.04 kg Оксиэтилдендифосфоновая кислотаHydroxyethyl diphosphonic acid 0,15 кг0.15 kg ВодаWater 90 л90 l

Полученная смесь имеет следующие свойства: осадка конуса в среднем 7 см, срок схватывания в среднем 41 мин. Изделия, полученные из данного состава смеси, имеют объемную массу в среднем 303 кг/м3 и прочность при сжатии 0,6 МПа, коэффициент теплопроводности 0,074 Вт/(м К).The resulting mixture has the following properties: cone draft on average 7 cm, setting time on average 41 minutes. Products obtained from this mixture composition have an average bulk density of 303 kg / m 3 and a compressive strength of 0.6 MPa, a thermal conductivity of 0.074 W / (m K).

Claims (1)

Армированная гипсополистиролбетонная смесь, включающая портландцемент, полистирольный заполнитель, щелочестойкое минеральное волокно, полиакриламид, пластифицирующую добавку С-3, регулятор твердения, воду, отличающаяся тем, что дополнительно содержит гипс полуводный, или ангидрит, или их смесь в любой пропорции, трепел или опоку, или диатомит, или их смесь в любой пропорции, водорастворимый эфир метилцеллюлозы или целлюлозу строительную, или карбоксиметилированный крахмал, а в качестве полистирольного заполнителя - дробленый полистирол или смесь в любой пропорции со вспененным полистиролом, в качестве щелочестойкого минерального волокна - хризотил-асбестовое волокно, в качестве регулятора твердения - винную или лимонную, или оксиэтилидендифосфоновую кислоту, компоненты имеют следующее соотношение на 1 м3 смеси:
портландцемент, кг 10,0-50,0 гипс или ангидрит или их смесь в любой пропорции, кг 60,0-250,0 трепел, или опока, или диатомит, или их смесь в любой пропорции, кг 7-75 дробленый полистирол или смесь в любой пропорции со вспененным гранулированным полистиролом, м3 0,70-0,98 хризотил-асбестовое волокно, кг 10,0-25,0 пластифицирующая добавка С-3, кг 0,03-1,40 10%-ный раствор полиакриламида, кг 0,40-0,60 водорастворимый эфир метилцеллюлозы, или целлюлоза строительная, или карбоксиметилированный крахмал, кг 0,01-0,05 винная, или лимонная, или оксиэтилидендифосфоновая кислота, кг 0,01-0,20 вода, л 20,0-140,0
Reinforced gypsum-polystyrene concrete mixture, including Portland cement, polystyrene aggregate, alkali-resistant mineral fiber, polyacrylamide, plasticizing additive C-3, hardening regulator, water, characterized in that it additionally contains semi-aquatic gypsum or anhydrite, or any mixture in any proportion, tripoli or flask, or diatomite, or a mixture thereof in any proportion, water-soluble methyl cellulose ether or construction cellulose, or carboxymethyl starch, and crushed polystyrene as a polystyrene filler l or a mixture in any proportion with foamed polystyrene, as the alkali-resistant mineral fiber - chrysotile asbestos fiber, as a hardening regulator - tartaric or citric acid, or oksietilidendifosfonovuyu acid components have the following relation to 1 m 3 of mix:
Portland cement, kg 10.0-50.0 gypsum or anhydrite or their mixture in any proportion, kg 60.0-250.0 tripoli, or flask, or diatomaceous earth, or their mixture in any proportions, kg 7-75 crushed polystyrene or mixture in any proportion with granulated polystyrene foam, m 3 0.70-0.98 chrysotile asbestos fiber, kg 10.0-25.0 plasticizing additive C-3, kg 0.03-1.40 10% solution of polyacrylamide, kg 0.40-0.60 water soluble methyl cellulose ether, or cellulose building or carboxymethyl starch, kg 0.01-0.05 wine, or lemon, or hydroxyethylidene diphosphonic acid, kg 0.01-0.20 water, l 20.0-140.0
RU2014148875/03A 2014-12-04 2014-12-04 Reinforced plaster-polysterene concrete mixture RU2577348C1 (en)