JPS6148489A - 気泡コンクリ−トの製造方法 - Google Patents

気泡コンクリ−トの製造方法

Info

Publication number
JPS6148489A
JPS6148489A JP16824084A JP16824084A JPS6148489A JP S6148489 A JPS6148489 A JP S6148489A JP 16824084 A JP16824084 A JP 16824084A JP 16824084 A JP16824084 A JP 16824084A JP S6148489 A JPS6148489 A JP S6148489A
Authority
JP
Japan
Prior art keywords
weight
parts
water
strength
present
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP16824084A
Other languages
English (en)
Inventor
峯垣内 勝
寛 中山
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
HAI UOOLE KK
Original Assignee
HAI UOOLE KK
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by HAI UOOLE KK filed Critical HAI UOOLE KK
Priority to JP16824084A priority Critical patent/JPS6148489A/ja
Publication of JPS6148489A publication Critical patent/JPS6148489A/ja
Pending legal-status Critical Current

Abstract

(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。

Description

【発明の詳細な説明】 (産業上の利用分野) 本発明は、気泡コンクリートの製造方法の改良に関し、
主VC建築業、構条業の産業分野で利用されるものであ
る。
(従来技術) 近時、建築物、構築物の@量化、工期の短縮化。
省エネルギー化等を目的として、所謂r A、L、CJ
(軽量気泡コンクリート)が益々大素に使用されて来て
いることは周矧のことである。
このA、L、C,は、軽量性のみでなく、切断の容易性
、打釘の容易性等々数多くの利点全有しているが、その
反面、防水性が皆無であると共に、透水性が甚だしいと
いう大きな欠点があり、したがって乾燥時には優秀な断
熱性全示すにも拘らず。
雨天などの場合は直ちに湿潤してしまうため、その断熱
性及び強度性は大巾に低下し、°°省エネルギー”建築
材料としての期待に全く沿い得ない場合のあることもよ
く知られている。
さらに、  A、L、C,には多数の気泡が内在してい
るため強度が著しく劣質であり、鉄筋を入れて補強して
も角g6などは僅かなgR撃によって破壊してしまう欠
点がある。
(本発明の目的) 本発明は、従来のA、 L、 C,の有する上記の欠点
を除去するために研究開発されたもので、A、L、C。
固有の軽量性、切断の容易性、打釘の容易性等の特性を
少しも損なうことなく、而も防水性、非透水性、湿潤W
pKおけるUr熱性全大巾に改良すると共に強度性全増
大して、A、L、C,の有用性を一層向上し得る新規な
製造方法全提供することを目的とするものである。
(本発明の溝底) 本発明に係る気泡コンクリートの製造方法は、セメント
100重金部に対して、撥水性アスファルトエマルシコ
ンlO〜50重量部全添加し、これに所要量の水、骨材
、発泡剤等を加えて収る未硬化コンクリート混合物全常
法にし比かって発泡、硬化させること全特徴としている
(本発明の実施例) セメントtoo重ifi、アスファルトエマルジョ1 
           ン60チとパラフィンエマルン
ヨン40%とから収る撥水性アスファルト系エマルンヨ
ン加重量部、珪石粉末8号70重量部、珪石粉末5号1
30重量部、加水分解タン白質系発泡剤2重量部、水5
0重量部、耐アルカリ性ガラス繊維0.O1重量部全十
分に混練し1強度測定用型枠に流し込んで四日間養生し
て気泡コンクリートを得之。 この本発明、による製品
上市販のA、L、C,との性能を比較した結果を次(※
+oxtOx2flyM柱の下部3 cmf 7 Q 
Hr氷水中浸漬)上表より明らかなように2本発明によ
る製品は吸水率を大巾に抑制改善できたのみでなく1強
度、特に曲げ強fvi−著しく顕著に向上できたことが
確認された〇 なお、本発明において、セメント100重量部に対する
撥水性アスファルト系エマルジ1ンの添加量を10〜5
0重量部の範囲に規定したのは次の理由による。
Ion量部よりも少ないと1曲げ強度はl0Kr/i以
下に低下すると共に、吸水率は5〜10’/ volと
なって所期の目的?構収し難く、1覧50重量部を超え
ると、−1!メント固有の強度が著しく低下し、セメン
トのみで製造し次気泡コンクリートのEEM強度は42
 N’f / clJ (絶乾比重0.6に設定)であ
るのに対して、その圧縮強度は20 Kp / ca程
度まで低下するという理由に基くものである。
(本発明の効果) 上記のよ5に、本発明によれば、気泡コンクリートの製
造IC際して、−t!メントに特定範囲量の撥水性アス
ファルト系エマルシコンを添加することにより、製品に
優れ乏防水性及び非透水性を付与し得るのみでなく1強
度、特に曲げ強度を著しく顕著に向上でき、従来よりA
、L、C,の最大の欠陥とされてい九高吸水性による強
度低下及び断熱性低下の問題を簡単な手段により確実に
解決できる多大な利点があり、更に、製品はアスファル
ト特有の黒色?呈するので、白色を呈していた従来のA
、L、C,に較べ、吸熱保温性を格段に良好に保ち得て
、建築材としての使用価値全一層向上できるものである
特許出願人 ハイクオール株式会社 同 上  系垣内  勝

Claims (1)

    【特許請求の範囲】
  1. セメント100重量部に対して、撥水性アスファルト系
    エマルジョン10〜50重量部を添加し、これに所要量
    の水、骨材、発泡剤等を加えて成る未硬化コンクリート
    混合物を常法にしたがつて発泡、硬化させることを特徴
    とする気泡コンクリートの製造方法。
JP16824084A 1984-08-10 1984-08-10 気泡コンクリ−トの製造方法 Pending JPS6148489A (ja)