JPS61195563A - 積層乾電池 - Google Patents
積層乾電池Info
- Publication number
- JPS61195563A JPS61195563A JP60035933A JP3593385A JPS61195563A JP S61195563 A JPS61195563 A JP S61195563A JP 60035933 A JP60035933 A JP 60035933A JP 3593385 A JP3593385 A JP 3593385A JP S61195563 A JPS61195563 A JP S61195563A
- Authority
- JP
- Japan
- Prior art keywords
- current collector
- carbon plate
- glassy carbon
- corrosion
- battery
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。
め要約のデータは記録されません。
Description
【発明の詳細な説明】
〔発明の技術分野〕
この発明は陽極集電体を改良した積層乾電池に関する。
複数の素電池群を積層してなる所謂積層乾電池は陽極側
端部に陽極集電体を当接して設けている。
端部に陽極集電体を当接して設けている。
しかして、従来このような積層乾電池における陽極集電
体は第2図に示すように金属板1の片面に電池内部の活
物質との反応を防止するための導電塗膜2を形成すると
ともに周縁部を熱収縮性チューブ3にて被覆したものが
ある。この場合、電池内部の電解液がチューブ3と導電
塗膜2との間を通って外部に漏出するのを防止するため
この間に接着剤4を介在させている。
体は第2図に示すように金属板1の片面に電池内部の活
物質との反応を防止するための導電塗膜2を形成すると
ともに周縁部を熱収縮性チューブ3にて被覆したものが
ある。この場合、電池内部の電解液がチューブ3と導電
塗膜2との間を通って外部に漏出するのを防止するため
この間に接着剤4を介在させている。
ところが接着剤4を適量で且つ均一に介在させるのは難
しく、例えば少なすぎるとチューブ3と導電塗膜2の間
の接着が不安定になって電解液の漏出原因となり、また
逆に多すぎると余分な接着剤4が流出し導電面を狭め電
気抵抗が上昇してしまう欠点があった。
しく、例えば少なすぎるとチューブ3と導電塗膜2の間
の接着が不安定になって電解液の漏出原因となり、また
逆に多すぎると余分な接着剤4が流出し導電面を狭め電
気抵抗が上昇してしまう欠点があった。
そこで、従来実公昭49−43702号公報にみられる
ように集電体として鉄板の両面に亜鉛を引きしたトタン
板を用いたものがある。このものを用いれば耐腐食性が
若干良くなるが、トタン板を所定寸法に打抜く除虫じる
断面は腐食し易く、しかもトタン板の導電性塗料を塗布
する側は一般にブラスト加工等を施して塗料の付着状態
を良好にしているため表面が活性化されており、このた
め塗膜にピンホールが存在すると、これが原因で腐食が
生じるおそれがあった。実際問題として塗布面のピンホ
ールを皆無にすることは難しく、上述の原因によるトタ
ン板の腐食は避けられなかった。
ように集電体として鉄板の両面に亜鉛を引きしたトタン
板を用いたものがある。このものを用いれば耐腐食性が
若干良くなるが、トタン板を所定寸法に打抜く除虫じる
断面は腐食し易く、しかもトタン板の導電性塗料を塗布
する側は一般にブラスト加工等を施して塗料の付着状態
を良好にしているため表面が活性化されており、このた
め塗膜にピンホールが存在すると、これが原因で腐食が
生じるおそれがあった。実際問題として塗布面のピンホ
ールを皆無にすることは難しく、上述の原因によるトタ
ン板の腐食は避けられなかった。
このことば集電板腐食による電気特性劣化を招き保存性
が著しく悪化する欠点があった。さらに塗問題もあった
。
が著しく悪化する欠点があった。さらに塗問題もあった
。
この発明は上記欠点を除去するためなされたもので集電
体腐食による電気特性劣化がなく保存性にすぐれた積層
乾電池を提供することを目的とする。
体腐食による電気特性劣化がなく保存性にすぐれた積層
乾電池を提供することを目的とする。
この発明にかかる積層乾電池は陽極集電体としてガラス
状カーボン部材を用いるようにしている。
状カーボン部材を用いるようにしている。
この発明によれば陽極集電体にガラス状カーボン部材を
用いたので集電体での腐食を皆無にでき電気特性の劣化
が全くなく保存性にすぐれている。
用いたので集電体での腐食を皆無にでき電気特性の劣化
が全くなく保存性にすぐれている。
しかも集電体はガラス状カーボン部材単体よりなるので
集電体組立工程が全く必要なくその分電池全体の組立工
数を減らすことができコスト的にも安価にできる。
集電体組立工程が全く必要なくその分電池全体の組立工
数を減らすことができコスト的にも安価にできる。
以下、この発明の一実施例を図面に従い説明する。
第1図はこの発明の積層乾電池に用いられる陽極集電体
を示している。図において11は陽極集電体としての板
状のガラス状カーボン部材である。
を示している。図において11は陽極集電体としての板
状のガラス状カーボン部材である。
このガラス状カーボン部材11はガラス状カーボンマト
リックス中に補強剤を分散し成形焼成したもので具体的
にはグラファイト又はカーボンブラックと熱硬化性のフ
ェノール樹脂を加熱焼成することにより得ている。そし
て、例えばレーザカッティングなどにより所定の大きさ
に形成している。
リックス中に補強剤を分散し成形焼成したもので具体的
にはグラファイト又はカーボンブラックと熱硬化性のフ
ェノール樹脂を加熱焼成することにより得ている。そし
て、例えばレーザカッティングなどにより所定の大きさ
に形成している。
なお、このようなガラス状カーボン部材11は体積固有
抵抗が小さい程望ましいが実際成形性や強度の関係から
補強剤の混入量も確保しなければならないので10−4
〜108Ωcm程度のものが用いられる。
抵抗が小さい程望ましいが実際成形性や強度の関係から
補強剤の混入量も確保しなければならないので10−4
〜108Ωcm程度のものが用いられる。
しかして、このように陽極集電体として板状のガラス状
カーボン部材を用いるとかかるカーボン部材は充分の導
電性を有するので集電体としての機能を確実にはだすこ
とができ、しかもカーボン部材自身電池内部の活物質と
反応するこ吉がなく腐食が全く生じることがないので電
池の開路電圧や短絡電流などの電気特性の劣化が全くな
く保存性能を飛躍的に高めることができる。また集電体
は板状のガラス状カーボン部材単体で構成されるのでか
かる集電体の組立工程を全く不要にでき電池全体の組立
工数を減らすことができ、その分価格的に安価にできる
。
カーボン部材を用いるとかかるカーボン部材は充分の導
電性を有するので集電体としての機能を確実にはだすこ
とができ、しかもカーボン部材自身電池内部の活物質と
反応するこ吉がなく腐食が全く生じることがないので電
池の開路電圧や短絡電流などの電気特性の劣化が全くな
く保存性能を飛躍的に高めることができる。また集電体
は板状のガラス状カーボン部材単体で構成されるのでか
かる集電体の組立工程を全く不要にでき電池全体の組立
工数を減らすことができ、その分価格的に安価にできる
。
ちなみに陽極集電体上して本発明によるガラス状カーボ
ン部材を用いた6F22型積層乾電池と従来の金属板の
片面に導電性塗膜を形成するとともに周縁部を接着剤を
介して熱収縮性チューブにて被覆した集電体を用いた同
型の積層乾電池を用意し、これら電池を夫々常温で6ケ
月間貯蔵した場合と、45°中で3ケ月貯蔵した場合の
開路電圧と短絡電流を調べたところ下記の結果が得られ
た。
ン部材を用いた6F22型積層乾電池と従来の金属板の
片面に導電性塗膜を形成するとともに周縁部を接着剤を
介して熱収縮性チューブにて被覆した集電体を用いた同
型の積層乾電池を用意し、これら電池を夫々常温で6ケ
月間貯蔵した場合と、45°中で3ケ月貯蔵した場合の
開路電圧と短絡電流を調べたところ下記の結果が得られ
た。
以下余白
しかして上表より本発明電池は従来電池に比べ保存性能
が優れていることが判った。これは従来電池は集電体の
腐食により集電体をなす金属板と電池内の活物質とが反
応しこれが原因で開路電圧が下がり、さらにこの反応に
より電池内の水分が減ることから短絡電流も下がるよう
になるが本発明電池は腐食が全く生じないだけでなく電
池自活物質と反応することがないためである。
が優れていることが判った。これは従来電池は集電体の
腐食により集電体をなす金属板と電池内の活物質とが反
応しこれが原因で開路電圧が下がり、さらにこの反応に
より電池内の水分が減ることから短絡電流も下がるよう
になるが本発明電池は腐食が全く生じないだけでなく電
池自活物質と反応することがないためである。
なおこの発明は上記実施例にのみ限定されず要旨を変更
しない範囲で適宜変形して実施できる。
しない範囲で適宜変形して実施できる。
第1図はこの発明の一実施例に用いられる集電体を示す
側面図、第2図は従来の積層乾電池に用いられる集電体
を示す断面図である。
側面図、第2図は従来の積層乾電池に用いられる集電体
を示す断面図である。
Claims (1)
- 単位素電池を複数個積重してなる積層乾電池において陽
極集電体にガラス状カーボンを用いたことを特徴とする
積層乾電池。