JPS6072628A - Production of cooling plate for walking bar - Google Patents

Production of cooling plate for walking bar

Info

Publication number
JPS6072628A
JPS6072628A JP17826683A JP17826683A JPS6072628A JP S6072628 A JPS6072628 A JP S6072628A JP 17826683 A JP17826683 A JP 17826683A JP 17826683 A JP17826683 A JP 17826683A JP S6072628 A JPS6072628 A JP S6072628A
Authority
JP
Japan
Prior art keywords
cooling plate
walking bar
hollow
water
plate
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP17826683A
Other languages
Japanese (ja)
Inventor
Tsutomu Ariga
有賀 勉
Tetsuo Taniguchi
谷口 哲男
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
JFE Engineering Corp
Original Assignee
NKK Corp
Nippon Kokan Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by NKK Corp, Nippon Kokan Ltd filed Critical NKK Corp
Priority to JP17826683A priority Critical patent/JPS6072628A/en
Publication of JPS6072628A publication Critical patent/JPS6072628A/en
Pending legal-status Critical Current

Abstract

PURPOSE:To manufacture a good cooling plate for a walking bar which has no weak points such as weld zones or the like by extruding a hollow blank material, which is formed by heating and punching a billet, by a hot extruder to form a pipe material having approximately prescribed rectangular section and finishing further the outside surface thereof. CONSTITUTION:A mechanically punched billet is first heated and is made into a hollow blank material by a suitable punching installation in the production of a cooling plate for a walking bar mechanism which supports and guides a continuous casting billet. The hollow blank material is extruded by a hot extruder and is made into a hollow plate material having a prescribed hollow rectangular sectional shape. The outside surface thereof is finished by machining, etc. to a prescribed shape. The conventional cooling plate for the walking bar is made of a hollow plate by welding and has a weak point in the weld zone, but the weak point is eliminated by the above-mentioned method and the good water cooling plate for the walking bar is obtd.

Description

【発明の詳細な説明】 この発明は、連続鋳造装置において、モールドから引抜
かれた鋳片を支持し案内するだめのウオーキングバー機
構におけるウオーキングバー水冷板の製造方法に関する
ものである。。
DETAILED DESCRIPTION OF THE INVENTION The present invention relates to a method for manufacturing a water-cooled walking bar plate in a continuous casting apparatus that supports and guides a slab drawn from a mold. .

連続鋳造装置において、モールドから引抜かれだ鋳片を
支持し案内するだめの手段の一つとして、モールドの直
下にウオーキングバー機構が設けられている。
In a continuous casting apparatus, a walking bar mechanism is provided directly below the mold as one means for supporting and guiding the slab pulled out from the mold.

第1図はウオーキングバー機構の概略平面図で、ウオー
キングバー機構は、モールドから引抜かれた鋳片1を挾
む両側に、各々複数枚のウオーキングバー2および2′
が対向して列設され、図示しない駆動機構によるウオー
キングパー2および2′のウオーキングモーションによ
って、91片1を支持し案内して二次冷却帯に送シこむ
ようになっている。
FIG. 1 is a schematic plan view of the walking bar mechanism.
are arranged in rows facing each other, and the 91 piece 1 is supported and guided to be fed into the secondary cooling zone by the walking motion of the walking parlors 2 and 2' by a drive mechanism (not shown).

ウオーキングパー2および2′は、その針1片1と接す
る部分に、水冷板3,3′が増刊けられており、水冷板
3,3′内を循環する冷却水によって、aJj片1を冷
却支持し案内している。、 第2図は水冷板の正面図、第31メ1はその横断面図で
、水冷板3は横断面がほぼ矩形状で、その内γrlIS
VCは冷却水が循環するQlぼ矩形状の冷却水循環孔4
が設けられている3、 このような水冷板は、従来第3図に示すように4枚の鋼
板3a 、3b 、3c 、3dによって矩形状に形成
し、その各接続部5を溶接によって一体的に結合するこ
とにより・製造していた。
The walking parlors 2 and 2' are provided with additional water cooling plates 3 and 3' at the portions that contact the needle piece 1, and the aJj piece 1 is cooled by the cooling water circulating within the water cooling plates 3 and 3'. Support and guide. , Fig. 2 is a front view of the water-cooled plate, and Fig. 31 is its cross-sectional view.
VC is a rectangular cooling water circulation hole 4 through which cooling water circulates.
3. Such a water-cooled plate is conventionally formed into a rectangular shape by four steel plates 3a, 3b, 3c, and 3d, as shown in FIG. Manufactured by combining with.

そのため、接続部5の溶接強度上、鉄板3a。Therefore, in terms of the welding strength of the connection part 5, the iron plate 3a is used.

3b 、3c 、3dの厚みをある程度大にする必要が
あり、その結果、従来の水冷板には、冷却温度分布が不
均一になって、鋼板3a+3b+3c。
It is necessary to increase the thickness of 3b, 3c, and 3d to some extent, and as a result, in the conventional water-cooled plate, the cooling temperature distribution becomes uneven, and the steel plate 3a+3b+3c.

3dおよびその接続部5に亀裂が発生し、内部を循環す
る冷却水が漏出する問題があった。
3d and its connection portion 5, causing a problem in which the cooling water circulating inside leaked out.

この発明は、上述のような観点から、溶接を不要とし、
亀裂などの発生によって冷却水が漏出することのないウ
オーキングバー水冷板の製造方法を捉供するもので、鋼
片を所定温度に加熱した後、その中心に所定径の孔を穿
孔して中空素材を調製し、次いで、前記中空素材を熱間
押出し機により押出して、断面がほぼ矩形状の冷却水循
環孔を形成し、次いで、仕上加工を施して所定形状の水
冷板とすることに特徴を有するものである。
From the above-mentioned viewpoints, this invention eliminates the need for welding,
This method provides a method for manufacturing a walking bar water-cooled plate that prevents cooling water from leaking due to the occurrence of cracks, etc. After heating a steel piece to a predetermined temperature, a hole of a predetermined diameter is drilled in the center to form a hollow material. The hollow material is then extruded using a hot extruder to form cooling water circulation holes with a substantially rectangular cross section, and then finished to form a water-cooled plate of a predetermined shape. It is.

次に、この発明を図面を参照しながら説明する。Next, the present invention will be explained with reference to the drawings.

第4図はこの発明の製造方法の一例を示す工程径aが2
60調、長さtが689mmの断面が円形のビレット6
を使用し、このビレット6の軸線に沿って、第4図(ロ
)に示すように直径すが47 mmで一端に直径Cが1
00爺の開口1を有する孔7を機械加工により形成した
FIG. 4 shows an example of the manufacturing method of the present invention, where the process diameter a is 2.
60 scale, billet 6 with a circular cross section and a length t of 689 mm
Along the axis of this billet 6, as shown in Figure 4 (B), a diameter C of 47 mm is placed at one end.
A hole 7 having an opening 1 of 0.00 mm was formed by machining.

次いで、上記により孔7が形成されたビレット6を所定
温度に加熱した後、穿孔プレス機により第4図t−iに
示すようにその軸線に沿って直径dが155mmの孔8
を有する長さt2が961咽の中空素材9を調製した。
Next, after heating the billet 6 in which the holes 7 have been formed as described above to a predetermined temperature, holes 8 having a diameter d of 155 mm are formed along the axis of the billet 6 using a punching press as shown in FIG.
A hollow material 9 having a length t2 of 961 mm was prepared.

次いで上記の中空素材9を所定温度に再加熱した後、熱
間押出し機により押出して、第4図に)および拡大断面
図である第4図(ホ)に示すように、長辺eが177胴
、短辺fが61m++で、長さt3が4.000 +m
nの断面矩形状で、その軸線に沿って長辺gが139晒
、短辺りが1(5wnの断面矩形状の冷却水循環孔10
が形成された水冷板1]を製造した。
Next, the hollow material 9 is reheated to a predetermined temperature and extruded using a hot extruder to form a material with a long side e of 177 mm as shown in FIG. 4) and an enlarged cross-sectional view of FIG. Body, short side f is 61m++, length t3 is 4.000 +m
The cooling water circulation hole 10 has a rectangular cross section of n and has a rectangular cross section with a long side g of 139 and a short side of 1 (5wn) along its axis.
A water-cooled plate 1] was manufactured.

このようにして製造された水冷板11は、更にその四面
の機械加工、曲げ加工、前後端の切断、ボルト穴の加工
等の仕上加工を施し、所定形状の製品とした。
The water-cooled plate 11 manufactured in this manner was further subjected to finishing processes such as machining on its four sides, bending, cutting at the front and rear ends, and forming bolt holes to form a product in a predetermined shape.

このようにして製造された水冷板には溶接部分がないか
ら、その断面形状を自由にコントロールすることができ
、熱応力を緩和することができる。
Since the water-cooled plate manufactured in this manner has no welded parts, its cross-sectional shape can be freely controlled and thermal stress can be alleviated.

従って水冷板に亀裂が生ずることはなくなり、冷却水が
漏出するおそれはない。
Therefore, cracks will not occur in the water-cooled plate, and there is no risk of cooling water leaking.

第5図は、との発明の方法によシ製造された水冷板の他
の例を示す横断面図である。この水冷板12は、鋳片と
の接触面12a側の肉厚がそのコーナ部分12b 、 
12cにおいても均一となるように、冷却水循環孔13
Ωコ一ナ部分に耳部13a 、i3bが設けられている
。従って、冷却温度の分布をより完全に均一化すること
ができる。
FIG. 5 is a cross-sectional view showing another example of a water-cooled plate manufactured by the method of the invention. This water-cooled plate 12 has a wall thickness on the side of the contact surface 12a with the slab at the corner portion 12b,
The cooling water circulation hole 13 is also made uniform in 12c.
Ear portions 13a and i3b are provided at the Ω corner portion. Therefore, the distribution of cooling temperature can be made more completely uniform.

以上説明したように、この発明の方法によれば、石接部
のない均一な薄肉のウオーキングバー水冷板を容易に製
造することができ、製品は使用中に亀裂が発生して冷却
水が漏出するおそれはない等の優れた効果がもたらされ
る。
As explained above, according to the method of the present invention, it is possible to easily manufacture a uniform thin-walled walking bar water-cooled plate without stone contact parts, and the product cracks during use and leaks cooling water. Excellent effects such as there being no risk of damage are brought about.

【図面の簡単な説明】[Brief explanation of the drawing]

第1図はウオーキング・(−機構の概略平面図、第2図
は従来の水冷板の正面図、第31図はその横断面図、第
4図はこの発明の製造方法の−914を示す工程図、第
5図はこの発明の方法で製造された水冷板の他゛の例を
示す横断面図である。図1niにおいて、 1・・・鋳片、 2 、2’・・・ウオーキングノく−
、3.3′・・・水冷板、 4・・・冷却水循珪1孔、
5・・・接続部、 6・・ビレット) 7.8・・・孔、 9・・中空素材、 10 、13・・・冷却水循環孔、 11 、12・・・水冷板。 出願人 日本鋼管株式会社 代理人 潮 谷 4ミ汁人(他2名)
Fig. 1 is a schematic plan view of the walking mechanism, Fig. 2 is a front view of a conventional water cooling plate, Fig. 31 is a cross-sectional view thereof, and Fig. 4 is a process showing -914 of the manufacturing method of the present invention. 5 are cross-sectional views showing other examples of water-cooled plates manufactured by the method of the present invention. In FIG. −
, 3.3'...water cooling plate, 4...cooling water circulation 1 hole,
5... Connection portion, 6... Billet) 7.8... Hole, 9... Hollow material, 10, 13... Cooling water circulation hole, 11, 12... Water cooling plate. Applicant Nippon Kokan Co., Ltd. Agent Shiotani 4 Mijiruto (2 others)

Claims (1)

【特許請求の範囲】[Claims] 鋼片を所定温度に加熱した後、その中心に所定径の孔を
穿孔して中空素材を調製し、次いで、前記中空素材を熱
間押出し機により押出して、断面がほぼ矩形状の冷却水
循環孔を形成し、次いで、仕上加工を施して所定形状の
水冷板とすることを特徴とするウオーキングバー水冷板
の製造方法。
After heating a steel piece to a predetermined temperature, a hole of a predetermined diameter is bored in the center to prepare a hollow material, and then the hollow material is extruded using a hot extruder to form a cooling water circulation hole with a substantially rectangular cross section. 1. A method of manufacturing a walking bar water-cooled plate, comprising: forming a water-cooled plate, and then finishing the water-cooled plate to form a water-cooled plate having a predetermined shape.
JP17826683A 1983-09-28 1983-09-28 Production of cooling plate for walking bar Pending JPS6072628A (en)