JP7908028B2 - Phenolic resin compositions, cured products, and molded articles - Google Patents

Phenolic resin compositions, cured products, and molded articles

Info

Publication number
JP7908028B2
JP7908028B2 JP2022010653A JP2022010653A JP7908028B2 JP 7908028 B2 JP7908028 B2 JP 7908028B2 JP 2022010653 A JP2022010653 A JP 2022010653A JP 2022010653 A JP2022010653 A JP 2022010653A JP 7908028 B2 JP7908028 B2 JP 7908028B2
Authority
JP
Japan
Prior art keywords
lignin
phenolic resin
resin
resin composition
solid
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
JP2022010653A
Other languages
Japanese (ja)
Other versions
JP2023109242A (en
Inventor
尚史 齋藤
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Gun Ei Chemical Industry Co Ltd
Original Assignee
Gun Ei Chemical Industry Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Gun Ei Chemical Industry Co Ltd filed Critical Gun Ei Chemical Industry Co Ltd
Priority to JP2022010653A priority Critical patent/JP7908028B2/en
Priority to PCT/JP2023/001354 priority patent/WO2023145575A1/en
Publication of JP2023109242A publication Critical patent/JP2023109242A/en
Application granted granted Critical
Publication of JP7908028B2 publication Critical patent/JP7908028B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Description

本発明は、フェノール樹脂組成物、硬化物及び成形体に関する。 This invention relates to phenolic resin compositions, cured products, and molded articles.

固形レゾール型フェノール樹脂等のフェノール樹脂の硬化物は、機械特性、耐熱性等に優れている。このため、フェノール樹脂は、成形材料等として、電気、電子、建築、自動車等、幅広い分野で用いられている(例えば特許文献1)。 Cured phenolic resins, such as solid resol-type phenolic resins, exhibit excellent mechanical properties and heat resistance. Therefore, phenolic resins are used as molding materials in a wide range of fields, including electrical, electronic, construction, and automotive industries (see, for example, Patent Document 1).

近年、大気中の二酸化炭素量増加を抑制する観点から、植物等のバイオマス由来の原料を用いた材料が注目されている。フェノール樹脂等についても、バイオマス由来の原料を用いることが検討されている。
特許文献2には、植物由来率が30質量%以上、かつ重量平均分子量が10,000以上である固形レゾール型フェノール樹脂が提案されている。
In recent years, materials made from biomass-derived raw materials such as plants have attracted attention from the perspective of suppressing the increase in atmospheric carbon dioxide levels. The use of biomass-derived raw materials for phenolic resins and other materials is also being considered.
Patent Document 2 proposes a solid resol-type phenolic resin having a plant-derived content of 30% by mass or more and a weight-average molecular weight of 10,000 or more.

国際公開第2011/118147号International Publication No. 2011/118147 特開2013-23633号公報Japanese Patent Publication No. 2013-23633

しかし、本発明者の検討によれば、特許文献2の固形レゾール型フェノール樹脂は、植物由来率は高いものの、既存の化石資源由来の原料を用いた固形レゾール型フェノール樹脂に比べ、ゲル化時間が長く硬化性に劣ることがある。加えて、硬化物の物性にも改善の余地がある。 However, according to the inventors' research, the solid resol-type phenolic resin described in Patent Document 2, while having a high plant-derived content, sometimes exhibits longer gelation times and inferior curing properties compared to existing solid resol-type phenolic resins using fossil resource-derived raw materials. Furthermore, there is room for improvement in the physical properties of the cured product.

本発明は、バイオマス由来の原料を用いていながら硬化性が良好で、得られる硬化物の物性にも優れるフェノール樹脂組成物、その硬化物及び成形体を提供することを目的とする。 The present invention aims to provide a phenolic resin composition, its cured product, and a molded article that use biomass-derived raw materials while exhibiting good curability and excellent physical properties of the resulting cured product.

本発明は以下の態様を有する。
[1]フェノール樹脂とリグニンとフルフリルアルコールとを含む、フェノール樹脂組成物。
[2]前記フルフリルアルコール/前記リグニンで表される質量比が、40/60~95/5である前記[1]のフェノール樹脂組成物。
[3]前記リグニンと前記フルフリルアルコールとの合計の含有量が、前記フェノール樹脂の不揮発分と前記リグニンと前記フルフリルアルコールとの合計質量に対し、5~50質量%である前記[1]又は[2]のフェノール樹脂組成物。
[4]前記フェノール樹脂が固形フェノール樹脂である前記[1]~[3]のいずれかのフェノール樹脂組成物。
[5]前記固形フェノール樹脂が固形レゾール型フェノール樹脂である前記[4]のフェノール樹脂組成物。
[6]前記[1]~[5]のいずれかのフェノール樹脂組成物が硬化された硬化物。
[7]前記[6]の硬化物からなる成形体。
The present invention has the following aspects.
[1] A phenol resin composition comprising a phenol resin, lignin, and furfuryl alcohol.
[2] The phenol resin composition according to [1], wherein the mass ratio represented by furfuryl alcohol/lignin is 40/60 to 95/5.
[3] The phenol resin composition according to [1] or [2], wherein the total content of lignin and furfuryl alcohol is 5 to 50% by mass with respect to the total mass of the nonvolatile content of the phenol resin and the lignin and furfuryl alcohol.
[4] A phenol resin composition according to any of the above [1] to [3], wherein the phenol resin is a solid phenol resin.
[5] The phenol resin composition according to [4], wherein the solid phenol resin is a solid resol-type phenol resin.
[6] A cured product obtained by curing any of the phenol resin compositions described in [1] to [5] above.
[7] A molded body made of the cured product of [6].

本発明によれば、バイオマス由来の原料を用いていながら硬化性が良好で、得られる硬化物の物性にも優れるフェノール樹脂組成物、その硬化物及びその成形体を提供できる。 According to the present invention, it is possible to provide a phenolic resin composition, its cured product, and its molded article, which exhibit good curability and excellent physical properties despite using biomass-derived raw materials.

本発明の一実施形態に係るフェノール樹脂組成物(以下、「本樹脂組成物」とも記す。)は、フェノール樹脂と、リグニンと、フルフリルアルコール(以下、「FFA」とも記す。)とを含む。 A phenolic resin composition according to one embodiment of the present invention (hereinafter also referred to as "this resin composition") comprises a phenolic resin, lignin, and furfuryl alcohol (hereinafter also referred to as "FFA").

フェノール樹脂としては、ノボラック型フェノール樹脂、レゾール型フェノール樹脂、各種の変性フェノール樹脂、及びこれらの混合物等が挙げられる。
ノボラック型フェノール樹脂は、酸性触媒の存在下でフェノール類とアルデヒド類とを反応させて得られたフェノール樹脂である。以下、ノボラック型フェノール樹脂を「ノボラック樹脂」とも記す。
レゾール型フェノール樹脂は、塩基性触媒の存在下でフェノール類とアルデヒド類とを反応させて得られたフェノール樹脂である。以下、レゾール型フェノール樹脂を「レゾール樹脂」とも記す。
変性フェノール樹脂としては、ノボラック樹脂又はレゾール樹脂を、ホウ素変性、ケイ素変性、重金属変性、窒素変性、イオウ変性、油変性、ロジン変性等の公知の技法により変性させたものが挙げられる。
Examples of phenolic resins include novolac-type phenolic resins, resol-type phenolic resins, various modified phenolic resins, and mixtures thereof.
Novolac-type phenolic resins are phenolic resins obtained by reacting phenols and aldehydes in the presence of an acidic catalyst. Hereafter, novolac-type phenolic resins will also be referred to as "novolac resins."
Resol-type phenolic resins are phenolic resins obtained by reacting phenols with aldehydes in the presence of a basic catalyst. Hereafter, resol-type phenolic resins will also be referred to as "resol resins."
Modified phenolic resins include novolac resins or resol resins modified by known techniques such as boron modification, silicon modification, heavy metal modification, nitrogen modification, sulfur modification, oil modification, and rosin modification.

フェノール類としては、酸性又は塩基性触媒の存在下でアルデヒド類と反応させて各フェノール樹脂が得られるものであればよく、フェノール、o-クレゾール、m-クレゾール、p-クレゾール、2,3-キシレノール、3,5-キシレノール、m-エチルフェノール、m-プロピルフェノール、m-ブチルフェノール、p-ブチルフェノール、o-ブチルフェノール、レゾルシノール、ハイドロキノン、カテコール、3-メトキシフェノール、4-メトキシフェノール、3-メチルカテコール、4-メチルカテコール、メチルハイドロキノン、2-メチルレゾルシノール、2,3-ジメチルハイドロキノン、2,5-ジメチルレゾルシノール、2-エトキシフェノール、4-エトキシフェノール、4-エチルレゾルシノール、3-エトキシ-4-メトキシフェノール、2-プロペニルフェノール、2-イソプロピルフェノール、3-イソプロピルフェノール、4-イソプロピルフェノール、3,4,5-トリメチルフェノール、2-イソプロポキシフェノール、4-ピロポキシフェノール、2-アリルフェノール、3,4,5-トリメトキシフェノール、4-イソプロピル-3-メチルフェノール、ピロガロール、フロログリシノール、1,2,4-ベンゼントリオール、5-イソプロピル-3-メチルフェノール、4-ブトキシフェノール、4-t-ブチルカテコール、t-ブチルハイドロキノン、4-t-ペンチルフェノール、2-t-ブチル-5-メチルフェノール、2-フェニルフェノール、3-フェニルフェノール、4-フェニルフェノール、3-フェノキシフェノール、4-フェノキシフェノール、4-へキシルオキシフェノール、4-ヘキサノイルレゾルシノール、3,5-ジイソプロピルカテコール、4-ヘキシルレゾルシノール、4-ヘプチルオキシフェノール、3,5-ジ-t-ブチルフェノール、3,5-ジ-t-ブチルカテコール、2,5-ジ-t-ブチルハイドロキノン、ジ-sec-ブチルフェノール、4-クミルフェノール、ノニルフェノール、2-シクロペンチルフェノール、4-シクロペンチルフェノール、1-ナフトール、2-ナフトール、1,2-ジヒドロキシナフタレン、1,3-ジヒドロキシナフタレン、1,4-ジヒドロキシナフタレン、1,5-ジヒドロキシナフタレン、1,5-ジヒドロキシナフタレン、1,6-ジヒドロキシナフタレン、1,7-ジヒドロキシナフタレン、1,8-ジヒドロキシナフタレン、2,3-ジヒドロキシナフタレン、2,6-ジヒドロキシナフタレン、2,7-ジヒドロキシナフタレン、ビスフェノールA、ビスフェノールF等が挙げられる。
中でも、フェノール、o-クレゾール、m-クレゾール、p-クレゾール、ビスフェノールA、2,3-キシレノール、3,5-キシレノール、m-ブチルフェノール、p-ブチルフェノール、o-ブチルフェノール、4-フェニルフェノール、レゾルシノールが好ましく、フェノールが最も好ましい。
フェノール類は、一種を単独で用いてもよく二種以上を併用してもよい。
The phenols can be any phenols that can be reacted with aldehydes in the presence of an acidic or basic catalyst to obtain the respective phenolic resins, such as phenol, o-cresol, m-cresol, p-cresol, 2,3-xylenol, 3,5-xylenol, m-ethylphenol, m-propylphenol, m-butylphenol, p-butylphenol, o-butylphenol, resorcinol, hydroquinone, catechol, 3-methoxyphenol, 4-methoxyphenol, 3-methylcatechol, 4-methylcatechol, methylhydroquinone, 2-methylresorcinol, 2,3-dimethylhydroquinone 2,5-dimethylresorcinol, 2-ethoxyphenol, 4-ethoxyphenol, 4-ethylresorcinol, 3-ethoxy-4-methoxyphenol, 2-propenylphenol, 2-isopropylphenol, 3-isopropylphenol, 4-isopropylphenol, 3,4,5-trimethylphenol, 2-isopropoxyphenol, 4-pyropoxyphenol, 2-allylphenol, 3,4,5-trimethoxyphenol, 4-isopropyl-3-methylphenol, pyrogallol, phloroglycinol, 1,2,4-benzenetriol, 5-isopropyl-3-methylphenol 4-Butoxyphenol, 4-t-Butylcatechol, t-Butylhydroquinone, 4-t-Pentylphenol, 2-t-Butyl-5-Methylphenol, 2-Phenylphenol, 3-Phenylphenol, 4-Phenoxyphenol, 3-Phenoxyphenol, 4-Phenoxyphenol, 4-Hexyloxyphenol, 4-Hexanoylresorcinol, 3,5-Diisopropylcatechol, 4-Hexylresorcinol, 4-Heptyloxyphenol, 3,5-Di-t-Butylphenol, 3,5-Di-t-Butylcatechol, 2,5-Di-t-Butylhydroquinone, Di-sec-Butyl Examples include ciulphenol, 4-cumylphenol, nonylphenol, 2-cyclopentylphenol, 4-cyclopentylphenol, 1-naphthol, 2-naphthol, 1,2-dihydroxynaphthalene, 1,3-dihydroxynaphthalene, 1,4-dihydroxynaphthalene, 1,5-dihydroxynaphthalene, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 1,7-dihydroxynaphthalene, 1,8-dihydroxynaphthalene, 2,3-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, bisphenol A, bisphenol F, and the like.
Among these, phenol, o-cresol, m-cresol, p-cresol, bisphenol A, 2,3-xylenol, 3,5-xylenol, m-butylphenol, p-butylphenol, o-butylphenol, 4-phenylphenol, and resorcinol are preferred, with phenol being the most preferred.
Phenols may be used individually or in combination of two or more types.

アルデヒド類としては、ホルムアルデヒド、トリオキサン、フルフラール、パラホルムアルデヒド、ベンズアルデヒド、メチルヘミホルマール、エチルへミホルマール、プロピルへミホルマール、サリチルアルデヒド、ブチルヘミホルマール、フェニルへミホルマール、アセトアルデヒド、プロピルアルデヒド、フェニルアセトアルデヒド、α-フェニルプロピルアルデヒド、β-フェニルプロピルアルデヒド、o-ヒドロキシベンズアルデヒド、m-ヒドロキシベンズアルデヒド、p-ヒドロキシベンズアルデヒド、o-クロロベンズアルデヒド、o-ニトロベンズアルデヒド、m-ニトロベンズアルデヒド、p-ニトロベンズアルデヒド、o―メチルベンズアルデヒド、m-メチルベンズアルデヒド、p-メチルベンズアルデヒド、p-エチルベンズアルデヒド、p-n-ブチルベンズアルデヒド等が挙げられる。
中でも、ホルムアルデヒド、パラホルムアルデヒド、フルフラール、ベンズアルデヒド、サリチルアルデヒドが好ましく、ホルムアルデヒド、パラホルムアルデヒドが特に好ましい。アルデヒド類は、一種を単独で用いてもよく二種以上を併用してもよい。
Examples of aldehydes include formaldehyde, trioxane, furfural, paraformaldehyde, benzaldehyde, methylhemiformal, ethylhemiformal, propylhemiformal, salicylaldehyde, butylhemiformal, phenylhemiformal, acetaldehyde, propylaldehyde, phenylacetaldehyde, α-phenylpropylaldehyde, β-phenylpropylaldehyde, o-hydroxybenzaldehyde, m-hydroxybenzaldehyde, p-hydroxybenzaldehyde, o-chlorobenzaldehyde, o-nitrobenzaldehyde, m-nitrobenzaldehyde, p-nitrobenzaldehyde, o-methylbenzaldehyde, m-methylbenzaldehyde, p-methylbenzaldehyde, p-ethylbenzaldehyde, and p-n-butylbenzaldehyde.
Among these, formaldehyde, paraformaldehyde, furfural, benzaldehyde, and salicylaldehyde are preferred, with formaldehyde and paraformaldehyde being particularly preferred. Aldehydes may be used individually or in combination of two or more.

酸性触媒としては、塩酸、硫酸、リン酸、蟻酸、酢酸、蓚酸、酪酸、乳酸、ベンゼンスルフォン酸、p-トルエンスルフォン酸、硼酸、又は塩化亜鉛もしくは酢酸亜鉛などの金属との塩等が挙げられる。
酸性触媒は、一種を単独で用いてもよく、二種以上を併用してもよい。
酸性触媒は、フェノール類100質量%に対し、0.05~3.00質量%使用することが好ましく、0.05~1.00質量%使用することがより好ましい。
酸性触媒を用いた反応を終了させる際に中和する場合、中和液としては、水酸化ナトリウム溶液、アンモニア水、酢酸亜鉛、水酸化カリウム等を使用できる。
Examples of acidic catalysts include hydrochloric acid, sulfuric acid, phosphoric acid, formic acid, acetic acid, oxalic acid, butyric acid, lactic acid, benzenesulfonic acid, p-toluenesulfonic acid, boric acid, or salts with metals such as zinc chloride or zinc acetate.
The acidic catalyst may be used alone or in combination of two or more types.
The acidic catalyst is preferably used in an amount of 0.05 to 3.00% by mass, and more preferably in an amount of 0.05 to 1.00% by mass, relative to 100% by mass of phenols.
When neutralizing a reaction using an acidic catalyst to terminate it, sodium hydroxide solution, aqueous ammonia, zinc acetate, potassium hydroxide, etc., can be used as the neutralizing solution.

塩基性触媒としては、水酸化ナトリウム、水酸化リチウム等のアルカリ金属の水酸化物;水酸化カルシウム、水酸化バリウム等のアルカリ土類金属の水酸化物;水酸化アンモニウム;ジエチルアミン、トリエチルアミン、トリエタノールアミン、エチレンジアミン、ヘキサメチレンテトラミン等のアミン類等が挙げられる。
中でも固形のレゾール型フェノール樹脂を得やすいことから、アミン類が好ましく、アンモニア、ジエチルアミンから選択されるアミン類が特に好ましい。
塩基性触媒は、一種を単独で用いてもよく、二種以上を併用してもよい。
塩基性触媒は、フェノール類100質量%に対し、0.5~3.0質量%使用することが好ましく、0.8~2.0質量%使用することがより好ましい。
Examples of basic catalysts include alkali metal hydroxides such as sodium hydroxide and lithium hydroxide; alkaline earth metal hydroxides such as calcium hydroxide and barium hydroxide; ammonium hydroxide; and amines such as diethylamine, triethylamine, triethanolamine, ethylenediamine, and hexamethylenetetramine.
Among these, amines are preferred because they make it easier to obtain solid resol-type phenolic resins, and amines selected from ammonia and diethylamine are particularly preferred.
Basic catalysts may be used individually or in combination of two or more.
The basic catalyst is preferably used in an amount of 0.5 to 3.0% by mass, and more preferably in an amount of 0.8 to 2.0% by mass, relative to 100% by mass of phenols.

フェノール樹脂は固形フェノール樹脂でも液状フェノール樹脂でもよいが、粗砕、粉砕が可能であり、使用時のハンドリングが良好な点から、固形フェノール樹脂が好ましい。 The phenolic resin can be either solid or liquid, but solid phenolic resin is preferred because it can be coarsely crushed or pulverized, and offers good handling during use.

固形フェノール樹脂は、固形レゾール樹脂であることが好ましい。フェノール樹脂が固形ノボラック樹脂の場合、硬化剤を用いることで、ゲル化時間を短くすることが可能であるが、用途が制限されることがある。フェノール樹脂が固形レゾール樹脂であれば、硬化剤を用いずに硬化でき、本樹脂組成物を幅広い用途に使用できる。 The solid phenolic resin is preferably a solid resol resin. If the phenolic resin is a solid novolac resin, the gelation time can be shortened by using a curing agent, but this may limit its applications. If the phenolic resin is a solid resol resin, it can be cured without a curing agent, allowing the resin composition to be used in a wide range of applications.

固形レゾール樹脂の軟化点は、60~110℃が好ましく、80~100℃がより好ましい。軟化点が前記下限値以上であれば、室温で固形状態が保たれやすく、前記上限値以下であれば、天然由来成分を混合しやすい。
軟化点は、軟化点測定装置を使用し、5℃/分の昇温速度、30~150℃の温度範囲で測定される。
The softening point of the solid resol resin is preferably 60 to 110°C, and more preferably 80 to 100°C. If the softening point is above the lower limit, the solid state is easily maintained at room temperature, and if it is below the upper limit, natural components are easily mixed in.
The softening point is measured using a softening point measuring device at a heating rate of 5°C/min within a temperature range of 30 to 150°C.

固形フェノール樹脂は、固形ノボラック樹脂であってもよい。固形ノボラック樹脂は、固形レゾール樹脂に比べて熱安定性に優れ、溶融混合時の熱による意図しない重合が進みにくい。そのため、フェノール樹脂が固形ノボラック樹脂であれば、各種の形状への成形を安定して行うことができる。 The solid phenolic resin may also be a solid novolac resin. Solid novolac resins have superior thermal stability compared to solid resol resins, and unintended polymerization due to heat during melting and mixing is less likely to occur. Therefore, if the phenolic resin is a solid novolac resin, stable molding into various shapes can be achieved.

固形ノボラック樹脂の軟化点は、60~130℃が好ましく、80~100℃がより好ましい。軟化点が前記下限値以上であれば、室温で固形状態が保たれやすく、前記上限値以下であれば、天然由来成分を混合しやすい。 The softening point of the solid novolac resin is preferably 60 to 130°C, and more preferably 80 to 100°C. If the softening point is above the lower limit, the solid state is easily maintained at room temperature; if it is below the upper limit, natural components are easily mixed in.

リグニンとしては、公知の各種のリグニンを使用でき、例えば、リグニンスルホン酸、クラフトリグニン、ソーダリグニン、ソーダ-アントラキノンリグニン、オルガノソルブリグニン、爆砕リグニン、硫酸リグニンが挙げられる。これらのリグニンは、一種を単独で用いてもよく二種以上を併用してもよい。 Various known types of lignin can be used as the lignin, including, for example, ligninsulfonic acid, Kraft lignin, soda lignin, soda-anthraquinone lignin, organosorb lignin, explosion lignin, and sulfate lignin. These lignins may be used individually or in combination of two or more types.

本樹脂組成物は、本発明の効果を損なわない範囲で、必要に応じて、フェノール樹脂、リグニン及びFFA以外の他の成分をさらに含んでいてもよい。
他の成分としては、例えば、硬化剤、硬化助剤、フィラー、フィラーの表面処理剤、着色剤、離型剤、滑材、難燃剤、カップリング剤等が挙げられる。
This resin composition may further contain other components besides phenolic resin, lignin, and FFA, as necessary, to the extent that it does not impair the effects of the present invention.
Other components include, for example, hardeners, hardening aids, fillers, filler surface treatment agents, colorants, mold release agents, lubricants, flame retardants, and coupling agents.

硬化剤は、フェノール樹脂の硬化剤であり、水酸化アンモニウム、ジエチルアミン、トリエチルアミン、トリエタノールアミン、エチレンジアミン、ヘキサメチレンテトラミン等のアミン類、及びこれらの混合物等の塩基性触媒;塩酸、硫酸、リン酸、蟻酸、酢酸、蓚酸、酪酸、乳酸、ベンゼンスルフォン酸、p-トルエンスルフォン酸、硼酸、塩化亜鉛もしくは酢酸亜鉛等の金属との塩、及びこれらの混合物等の酸性触媒等が挙げられる。
硬化助剤は、フェノール樹脂の硬化助剤であり、水酸化カルシウム、酸化カルシウム、酸化マグネシウム等が挙げられる。
The curing agent is a curing agent for phenolic resins and includes basic catalysts such as ammonium hydroxide, diethylamine, triethylamine, triethanolamine, ethylenediamine, hexamethylenetetramine, and other amines, and mixtures thereof; and acidic catalysts such as hydrochloric acid, sulfuric acid, phosphoric acid, formic acid, acetic acid, oxalic acid, butyric acid, lactic acid, benzenesulfonic acid, p-toluenesulfonic acid, boric acid, salts with metals such as zinc chloride or zinc acetate, and mixtures thereof.
The curing aid is a curing aid for phenolic resins, and examples include calcium hydroxide, calcium oxide, and magnesium oxide.

フィラーとしては、ガラス繊維、炭素繊維、炭酸カルシウム、タルク、マイカ、クレー、シリカ、アルミナ等の無機フィラー;木粉、ヤシ殻、籾殻、パルプ、ケナフ、綿糸、綿布等の有機フィラー等が挙げられる。
フィラーの表面処理剤としては、カチオニック・アンモニウム塩、カップリング剤等が挙げられる。カップリング剤としては、例えば、アミノ基、エポキシ基、メルカプト基、カルボキシル基、又はビニル基等の不飽和二重結合を有するカップリング剤が挙げられる。これらの中でも、アミノ基を有するカップリング剤が好ましい。
Examples of fillers include inorganic fillers such as glass fibers, carbon fibers, calcium carbonate, talc, mica, clay, silica, and alumina; and organic fillers such as wood flour, coconut shells, rice husks, pulp, kenaf, cotton yarn, and cotton cloth.
Examples of surface treatment agents for fillers include cationic ammonium salts and coupling agents. Examples of coupling agents include those having unsaturated double bonds such as amino groups, epoxy groups, mercapto groups, carboxyl groups, or vinyl groups. Among these, coupling agents having amino groups are preferred.

着色剤としては、カーボンブラック、酸化チタン、硫酸バリウム、鉄黒、弁柄等の顔料;アニリンブラック、アリザニン等の染料等が挙げられる。
離型剤としては、合成ポリエチレンワックス、シリコーンワックス、カルナバワックス、モンタン酸ワックス等が挙げられる。
難燃剤としては、リン、水酸化アルミニウム等が挙げられる。
滑材としては、ステアリン酸亜鉛等の脂肪酸金属石鹸、脂肪酸エステル、脂肪酸アマイド等が挙げられる。
これらの成分は、一種を単独で用いてもよく二種以上を併用してもよい。
Examples of colorants include pigments such as carbon black, titanium dioxide, barium sulfate, iron black, and red iron oxide; and dyes such as aniline black and alizanin.
Examples of release agents include synthetic polyethylene wax, silicone wax, carnauba wax, and montanic acid wax.
Examples of flame retardants include phosphorus and aluminum hydroxide.
Examples of lubricants include fatty acid metal soaps such as zinc stearate, fatty acid esters, and fatty acid amides.
These ingredients may be used individually or in combination of two or more.

本樹脂組成物において、FFA/リグニンで表される質量比は、40/60~95/5が好ましく、40/60~90/10がより好ましく、40/60~70/30がさらに好ましく、40/60~60/40が特に好ましい。
本発明者の検討によれば、FFAは、リグニンを溶解し、フェノール樹脂とリグニンとの混和性を高める。FFA/リグニンが前記下限値以上であれば、リグニンとFFAとを混合したときにリグニンの全量がFFAに溶解可能であり、バイオマス由来率を高くしても(例えば、フェノール樹脂の不揮発分とリグニンとFFAとの合計質量に対するリグニンとFFAとの合計の含有量を50質量%以上にしても)、フェノール樹脂とリグニンとを均一に混合できる。これらを均一に混合できることで、硬化物の物性も向上する。
一方、FFA/リグニンが前記上限値以下であれば、得られる硬化物の物性(曲げ強度、曲げ弾性率等)、硬化速度がより優れる。また、フェノール樹脂が固形フェノール樹脂である場合に、樹脂組成物全体を固形にでき、取り扱いやすい。
In this resin composition, the mass ratio expressed as FFA/lignin is preferably 40/60 to 95/5, more preferably 40/60 to 90/10, even more preferably 40/60 to 70/30, and particularly preferably 40/60 to 60/40.
According to the inventors' research, FFA dissolves lignin and improves the miscibility between the phenolic resin and lignin. If the FFA/lignin ratio is above the aforementioned lower limit, the entire amount of lignin can be dissolved in the FFA when lignin and FFA are mixed, and the phenolic resin and lignin can be uniformly mixed even if the biomass-derived content is high (for example, even if the total content of lignin and FFA relative to the total mass of non-volatile components of the phenolic resin, lignin, and FFA is 50% by mass or more). By being able to mix them uniformly, the physical properties of the cured product are also improved.
On the other hand, if the FFA/lignin ratio is below the upper limit, the physical properties (flexural strength, flexural modulus, etc.) and curing speed of the resulting cured product are superior. Furthermore, if the phenolic resin is a solid phenolic resin, the entire resin composition can be solidified, making it easier to handle.

リグニンとFFAとの合計の含有量は、フェノール樹脂の不揮発分とリグニンとFFAとの合計質量に対し、5~50質量%が好ましく、5~40質量%がより好ましく、10~40質量%がさらに好ましく、10~30質量%が特に好ましい。リグニンとFFAとの合計の含有量が前記下限値以上であれば、バイオマス由来率、硬化物の物性(曲げ強度、曲げ弾性率等)がより優れ、前記上限値以下であれば、樹脂組成物の硬化性がより優れる。 The total content of lignin and FFA is preferably 5 to 50% by mass, more preferably 5 to 40% by mass, even more preferably 10 to 40% by mass, and particularly preferably 10 to 30% by mass, relative to the total mass of non-volatile components of the phenolic resin and the combined mass of lignin and FFA. If the total content of lignin and FFA is above the lower limit, the biomass-derived content and the physical properties of the cured product (flexural strength, flexural modulus, etc.) are superior. If it is below the upper limit, the curability of the resin composition is superior.

フェノール樹脂とリグニンとFFAとの合計の含有量は、本樹脂組成物の総質量に対し、5質量%以上が好ましく、30質量%以上がより好ましく、50質量%以上がさらに好ましく、100質量%であってもよい。 The total content of phenolic resin, lignin, and FFA is preferably 5% by mass or more, more preferably 30% by mass or more, even more preferably 50% by mass or more, and may also be 100% by mass, based on the total mass of the resin composition.

(フェノール樹脂組成物の製造方法)
本樹脂組成物は、例えば、フェノール樹脂とリグニンとFFAとを混合することによって得られる。このとき、必要に応じて、他の成分を添加してもよい。
フェノール樹脂、リグニン及びFFAは、一括して混合してもよく、順次混合してもよい。例えば予めリグニンとFFAとを混合し、得られた混合物とフェノール樹脂とを混合してもよい。
他の成分を添加する場合、フェノール樹脂とリグニンとFFAとの混合時に他の成分を添加してもよく、フェノール樹脂とリグニンとFFAとの混合後に添加してもよい。
(Method for producing phenolic resin composition)
This resin composition can be obtained, for example, by mixing a phenolic resin, lignin, and FFA. Other components may be added as needed.
The phenolic resin, lignin, and FFA may be mixed together or sequentially. For example, the lignin and FFA may be mixed beforehand, and the resulting mixture may be mixed with the phenolic resin.
If other components are to be added, they may be added when mixing the phenolic resin, lignin, and FFA, or they may be added after mixing the phenolic resin, lignin, and FFA.

フェノール樹脂が固形フェノール樹脂である場合、混合方法としては、溶融混合が好ましい。
溶融混合は、公知の溶融混合装置を用いて実施できる。
溶融混合温度は、80~140℃が好ましく、100~120℃がより好ましい。溶融混合温度が前記下限値以上であれば、フェノール樹脂が充分に軟化し、各成分を容易に混合できる。溶融混合温度が前記上限値以下であれば、フェノール樹脂の意図しない硬化を抑制できる。
溶融混合時間は、5~60分間が好ましく、10~30分間がより好ましい。溶融混合時間が前記下限値以上であれば、各成分をより均一に混合することができ、前記上限値以下であれば、フェノール樹脂の意図しない硬化を抑制できる。
When the phenolic resin is a solid phenolic resin, melt mixing is preferred as the mixing method.
Melt mixing can be carried out using a known melt mixing apparatus.
The melting and mixing temperature is preferably 80 to 140°C, and more preferably 100 to 120°C. If the melting and mixing temperature is above the lower limit, the phenolic resin will soften sufficiently, and each component can be easily mixed. If the melting and mixing temperature is below the upper limit, unintended hardening of the phenolic resin can be suppressed.
The melting and mixing time is preferably 5 to 60 minutes, and more preferably 10 to 30 minutes. If the melting and mixing time is above the lower limit, each component can be mixed more uniformly, and if it is below the upper limit, unintended hardening of the phenolic resin can be suppressed.

(用途)
本樹脂組成物は、加熱することによって硬化させ、硬化物とすることができる。
本樹脂組成物を硬化させる際の加熱温度(硬化温度)は、150~250℃が好ましく、180~220℃がより好ましい。加熱時間(硬化時間)は、0.5~60分間が好ましく、1.5~30分間がより好ましい。
(Application)
This resin composition can be cured by heating to produce a cured product.
The heating temperature (curing temperature) for curing this resin composition is preferably 150 to 250°C, and more preferably 180 to 220°C. The heating time (curing time) is preferably 0.5 to 60 minutes, and more preferably 1.5 to 30 minutes.

本樹脂組成物を硬化させる際には、(1)フェノール樹脂同士の反応、(2)リグニンとFFAとの反応、(3)フェノール樹脂とリグニンとFFAとの反応等が生じて硬化すると考えられる。得られる硬化物の骨格にリグニンが取り込まれることで、曲げ強度、曲げ弾性率等の物性が向上すると考えられる。 During the curing of this resin composition, it is believed that curing occurs through (1) reactions between phenolic resins, (2) reactions between lignin and FFA, and (3) reactions between phenolic resin, lignin, and FFA. It is thought that the incorporation of lignin into the framework of the resulting cured product improves physical properties such as flexural strength and flexural modulus.

本樹脂組成物はフェノール樹脂とリグニンとFFAとを含むため、硬化性に優れ、また、本樹脂組成物を硬化させた硬化物は、曲げ強度、曲げ弾性率等の物性に優れる。
したがって、本樹脂組成物は、成形材料として有用である。例えば、本樹脂組成物を任意の形状に成形し、硬化させることで、成形体を製造できる。成形工程と硬化工程を同時に行ってもよい。
成形方法としては、成形体の形状に応じて公知の成形方法を適用でき、例えばトランスファー成形法、圧縮成形法、プレス成形法、射出成形法、押出し成形法等が挙げられる。
成形体としては、特に限定するものではないが、例えばブレーカー、コンミテータ、樹脂ギアや軸受け等の摺動部材、プーリー、各種ケース類等が挙げられる。
ただし、本樹脂組成物の用途は成形材料に限定されるものではなく、他の用途、例えば磁石封止材、摩擦材料、レジノイド砥石等の用途に用いることができる。
Because this resin composition contains phenolic resin, lignin, and FFA, it exhibits excellent curability, and the cured product obtained by curing this resin composition has excellent physical properties such as flexural strength and flexural modulus.
Therefore, this resin composition is useful as a molding material. For example, a molded article can be manufactured by molding this resin composition into any shape and curing it. The molding and curing processes may be performed simultaneously.
As for the molding method, known molding methods can be applied depending on the shape of the molded body, and examples include transfer molding, compression molding, press molding, injection molding, and extrusion molding.
The molded parts are not particularly limited, but examples include breakers, commutators, sliding components such as resin gears and bearings, pulleys, and various types of cases.
However, the use of this resin composition is not limited to molding materials; it can also be used in other applications, such as magnetic encapsulants, friction materials, and resinoid grinding wheels.

以下、実施例によって本発明を具体的に説明するが、本発明は以下の記載によっては限定されない。以下において「%」は、特に言及がない限り、「質量%」を示す。 The present invention will be specifically described below with reference to examples, but the present invention is not limited to the following description. In the following, "%" refers to "mass%" unless otherwise specified.

<使用材料>
固形レゾール樹脂:群栄化学工業製「PS-6125」、軟化点80~92℃。
ノボラック樹脂:群栄化学工業製「PSM-5302」、軟化点119~127℃。
リグニン1:東京化成工業社製「リグニン(アルカリ)」、CAS RN:8068-05-1。
リグニン2:東京化成工業社製「リグニン(脱アルカリ)」、CAS RN:9005-53-2。
ガラス繊維:日東紡社製「チョップドストランドCS3J891S」、カット長3mm、フィラメント径10μm。
炭酸カルシウム:東洋ファインケミカル社製「ホワイトンH」、平均粒子径22μm。
滑材:ステアリン酸亜鉛、アデカ社製「AFCOCHEM CS-S」。
着色剤:カーボンブラック、三菱ケミカル社製「カーボンブラック♯30」。
カップリング剤:3-アミノプロピルトリメトキシシラン、信越化学工業社製「KBE-903」。
<Materials used>
Solid resol resin: Gun-ei Chemical Industry Co., Ltd. "PS-6125", softening point 80-92°C.
Novolac resin: "PSM-5302" manufactured by Gun-ei Chemical Industry Co., Ltd., softening point 119-127°C.
Lignin 1: "Lignin (Alkali)" manufactured by Tokyo Chemical Industry Co., Ltd., CAS RN: 8068-05-1.
Lignin 2: "Lignin (de-alkaliated)" manufactured by Tokyo Chemical Industry Co., Ltd., CAS RN: 9005-53-2.
Glass fiber: Nitto Boseki Co., Ltd. "Chopped Strand CS3J891S", cut length 3 mm, filament diameter 10 μm.
Calcium carbonate: "Whiten H" manufactured by Toyo Fine Chemical Co., Ltd., average particle size 22 μm.
Lubricant: Zinc stearate, Adeca's "AFCOCHEM CS-S".
Coloring agent: Carbon black, Mitsubishi Chemical Corporation's "Carbon Black #30".
Coupling agent: 3-aminopropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd., "KBE-903".

<試験例1>
固形レゾール樹脂をそのまま比較例1の樹脂組成物とした。
表1に示す組成となるように、固形レゾール樹脂とFFAとリグニン(リグニン1又はリグニン2)とをフラスコにて溶融混合することで、比較例2~4、実施例1~6の樹脂組成物を得た。溶融混合の条件は、100℃で10分間とした。
<Test Example 1>
The solid resol resin was used as the resin composition for Comparative Example 1.
The resin compositions of Comparative Examples 2-4 and Examples 1-6 were obtained by melt-mixing solid resol resin, FFA, and lignin (lignin 1 or lignin 2) in a flask to obtain the compositions shown in Table 1. The melt-mixing conditions were 100°C for 10 minutes.

表1に、各例の樹脂組成物の常温(本実施例では25℃)での形状、150℃でのゲルタイム(GT)、天然由来率を示す。ゲルタイムは、以下に示す測定方法により測定した。天然由来率は、樹脂組成物の総質量に対するFFAとリグニンの合計の含有量に相当する。 Table 1 shows the shape at room temperature (25°C in this example), the gel time (GT) at 150°C, and the natural origin percentage for each resin composition. The gel time was measured using the method described below. The natural origin percentage corresponds to the total content of FFA and lignin relative to the total mass of the resin composition.

[ゲルタイムの測定]
試料(樹脂組成物)0.5gを150℃の熱板上で溶融し、撹拌しながらゲル化するまでの時間を測定した。
[Measuring gel time]
0.5 g of the sample (resin composition) was melted on a hot plate at 150°C, and the time it took for it to gel while being stirred was measured.

実施例1~6の樹脂組成物は、バイオマス由来の原料を用いていながら、従来の固形レゾール樹脂(比較例1)と同等かそれよりも短いゲルタイムを有しており、硬化性が良好であった。また、常温で固形であり、粗砕、粉砕が可能であった。
一方、FFAを含まない比較例2では、固形レゾール樹脂とリグニンとの混合時に、ダマが発生したり粉末が残存したりして、それらを均一に混合できなかった。
リグニンを含まない比較例3では、得られた樹脂組成物が半固形で、表面に粘性がありブロッキングしやすく、取り回しが悪いものであった(粗砕、粉砕が不可)。
比較例3よりもFFAの量を増やした比較例4では、得られた樹脂組成物が超高粘度の液状であったため、同一の測定方法にてゲルタイムを測定できなかった。また、液状のため、粗砕、粉砕が不可能であった。
The resin compositions of Examples 1 to 6, while using biomass-derived raw materials, exhibited gel times equivalent to or shorter than those of conventional solid resol resins (Comparative Example 1), demonstrating good curability. Furthermore, they were solid at room temperature and could be coarsely crushed or pulverized.
On the other hand, in Comparative Example 2, which did not contain FFA, clumps formed and powder remained when the solid resol resin and lignin were mixed, making it impossible to mix them uniformly.
In Comparative Example 3, which did not contain lignin, the resulting resin composition was semi-solid, viscous on the surface, prone to blocking, and difficult to handle (coarse crushing and pulverization were not possible).
In Comparative Example 4, where the amount of FFA was increased compared to Comparative Example 3, the resulting resin composition was in an ultra-high viscosity liquid state, making it impossible to measure the gel time using the same measurement method. Furthermore, due to its liquid state, coarse crushing and pulverization were impossible.

<試験例2>
表2に示す配合に従って、各材料を二軸ロールにて混練し、得られた混練物を粗砕することで、比較例5~6、実施例7~12のコンパウンド(樹脂組成物)を得た。混練の条件は、95℃で3分間、次いで60~80℃で3分間とした。比較例5、比較例6、実施例7~12において、表2中の「樹脂分」は、比較例1、比較例3、実施例1~6それぞれの樹脂組成物と同じ組成とした。
<Test Example 2>
The compounds (resin compositions) of Comparative Examples 5-6 and Examples 7-12 were obtained by kneading each material in a twin-screw roller according to the formulations shown in Table 2, and then coarsely crushing the resulting mixture. The kneading conditions were 95°C for 3 minutes, followed by 60-80°C for 3 minutes. In Comparative Examples 5, 6, and Examples 7-12, the "resin content" in Table 2 was the same as the resin compositions of Comparative Examples 1, 3, and Examples 1-6, respectively.

得られたコンパウンドを、トランスファー成形機にて金型温度180℃、硬化時間5分、プレス圧力30kg/cm2の成形条件で成形し、曲げ強度測定用の成形物(100×10×3mm)を得た。
表3に、各例のコンパウンドに配合した樹脂分の天然由来率及び組成、得られた成形物の密度、曲げ強度及び曲げ弾性率を示す。曲げ強度及び曲げ弾性率は以下に示す測定方法により測定した。
The obtained compound was molded in a transfer molding machine under molding conditions of a mold temperature of 180°C, a curing time of 5 minutes, and a press pressure of 30 kg/cm² to obtain a molded product (100 × 10 × 3 mm) for bending strength measurement.
Table 3 shows the percentage of naturally derived resin and its composition in each compound, as well as the density, flexural strength, and flexural modulus of the resulting molded product. The flexural strength and flexural modulus were measured using the measurement methods described below.

[曲げ強度及び曲げ弾性率の測定]
成形物について、ストログラフV10-C(東洋精機製)を用い、JIS K 6911:1995に準じて曲げ試験を行い、曲げ強度及び曲げ弾性率を求めた。曲げ試験でのクロスヘッドスピードは、2mm/分とした。
[Measurement of flexural strength and flexural modulus]
For the molded products, bending tests were performed using a Strograph V10-C (manufactured by Toyo Seiki) in accordance with JIS K 6911:1995 to determine the bending strength and bending modulus. The crosshead speed during the bending test was set to 2 mm/min.

実施例7~12の成形物はいずれも、比較例5の成形物に比べ、曲げ強度及び曲げ弾性率が高かった。
リグニンを含まない比較例6の成形物は、比較例5の成形物に比べ、曲げ強度が低かった。曲げ弾性率についても、比較例5より高いものの、実施例7~12より低かった。
The molded articles of Examples 7 to 12 all had higher bending strength and bending modulus compared to the molded article of Comparative Example 5.
The molded article of Comparative Example 6, which did not contain lignin, had lower bending strength compared to the molded article of Comparative Example 5. Its bending modulus was also higher than that of Comparative Example 5, but lower than that of Examples 7-12.

<試験例3>
ノボラック樹脂をそのまま比較例7の樹脂組成物とした。
表4に示す組成となるように、ノボラック樹脂とFFAとリグニン1とをフラスコにて150℃で30分間溶融混合することで、実施例13~16の樹脂組成物を得た。
<Test Example 3>
Novolac resin was used as the resin composition for Comparative Example 7.
The resin compositions of Examples 13 to 16 were obtained by melt-mixing novolac resin, FFA, and lignin 1 in a flask at 150°C for 30 minutes to obtain the compositions shown in Table 4.

表4に、各例の樹脂組成物の常温(本実施例では25℃)での形状、150℃でのゲルタイム(GT)、天然由来率を示す。ゲルタイムは、得られた樹脂組成物に対して10%のヘキサメチレンテトラミンを粉砕混合してから、前記した測定方法により測定した。 Table 4 shows the shape at room temperature (25°C in this example), the gel time (GT) at 150°C, and the percentage of naturally derived materials for each resin composition. The gel time was measured using the measurement method described above after grinding and mixing 10% hexamethylenetetramine with the obtained resin composition.

実施例13~16の樹脂組成物は、バイオマス由来の原料を用いていながら、従来のノボラック樹脂(比較例7)よりも短いゲルタイムを有しており、硬化性が良好であった。また、常温で固形であり、粗砕、粉砕が可能であった。 The resin compositions of Examples 13-16, while using biomass-derived raw materials, exhibited shorter gel times and better curability than conventional novolac resins (Comparative Example 7). Furthermore, they were solid at room temperature and could be coarsely crushed or pulverized.

Claims (6)

フェノール樹脂とリグニンとフルフリルアルコールとを含み、
前記フェノール樹脂が固形フェノール樹脂である、フェノール樹脂組成物。
It contains phenolic resin, lignin, and furfuryl alcohol.
A phenolic resin composition wherein the phenolic resin is a solid phenolic resin .
前記フルフリルアルコール/前記リグニンで表される質量比が、40/60~95/5である請求項1に記載のフェノール樹脂組成物。 The phenolic resin composition according to claim 1, wherein the mass ratio of furfuryl alcohol to lignin is 40/60 to 95/5. 前記リグニンと前記フルフリルアルコールとの合計の含有量が、前記フェノール樹脂の不揮発分と前記リグニンと前記フルフリルアルコールとの合計質量に対し、5~50質量%である請求項1又は2に記載のフェノール樹脂組成物。 The phenolic resin composition according to claim 1 or 2, wherein the total content of lignin and furfuryl alcohol is 5 to 50% by mass relative to the total mass of the non-volatile content of the phenolic resin, the lignin, and the furfuryl alcohol. 前記固形フェノール樹脂が固形レゾール型フェノール樹脂である請求項1~3のいずれか一項に記載のフェノール樹脂組成物。 The phenol resin composition according to any one of claims 1 to 3, wherein the solid phenol resin is a solid resol-type phenol resin. 請求項1~4のいずれか一項に記載のフェノール樹脂組成物が硬化された硬化物。 A cured product obtained by curing the phenol resin composition according to any one of claims 1 to 4 . 請求項5に記載の硬化物からなる成形体。 A molded article made of the cured product according to claim 5 .
JP2022010653A 2022-01-27 2022-01-27 Phenolic resin compositions, cured products, and molded articles Active JP7908028B2 (en)