JP5029072B2 - Reinforced fiber substrate laminate and method for producing the same - Google Patents

Reinforced fiber substrate laminate and method for producing the same Download PDF

Info

Publication number
JP5029072B2
JP5029072B2 JP2007056815A JP2007056815A JP5029072B2 JP 5029072 B2 JP5029072 B2 JP 5029072B2 JP 2007056815 A JP2007056815 A JP 2007056815A JP 2007056815 A JP2007056815 A JP 2007056815A JP 5029072 B2 JP5029072 B2 JP 5029072B2
Authority
JP
Japan
Prior art keywords
reinforcing fiber
laminate
fiber base
preform
resin
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
JP2007056815A
Other languages
Japanese (ja)
Other versions
JP2007276453A (en
Inventor
悟 長岡
知行 篠田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Toray Industries Inc
Original Assignee
Toray Industries Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toray Industries Inc filed Critical Toray Industries Inc
Priority to JP2007056815A priority Critical patent/JP5029072B2/en
Publication of JP2007276453A publication Critical patent/JP2007276453A/en
Application granted granted Critical
Publication of JP5029072B2 publication Critical patent/JP5029072B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Description

本発明は強化繊維プラスチックを樹脂注入成形法、特にレジントランスファーモールディング法(以下、RTM法という)により製造する際の中間基材であるプリフォームを作製するための強化繊維基材積層体およびその製造方法に関する。   The present invention relates to a reinforced fiber substrate laminate for producing a preform as an intermediate substrate when a reinforced fiber plastic is produced by a resin injection molding method, particularly a resin transfer molding method (hereinafter referred to as RTM method), and its production. Regarding the method.

炭素繊維などを強化繊維とした複合材料は、優れた力学特性、軽量特性を満たすことから主に航空、宇宙、スポーツ用途に用いられてきた。これらの代表的な製造方法として、RTM法などの樹脂注入成形法が挙げられ複雑な形状を有する大型の部材を短時間で成形することができる。   Composite materials using carbon fibers and the like as reinforcing fibers have been used mainly for aviation, space, and sports applications because they have excellent mechanical properties and light weight properties. A typical example of these production methods is a resin injection molding method such as the RTM method, and a large member having a complicated shape can be molded in a short time.

かかるRTM成形法では、強化繊維からなるプリフォームを成形型の中に配置して、液状のマトリックス樹脂を注入することにより強化繊維中にマトリックス樹脂を含浸させ、その後、加熱硬化して強化繊維プラスチックを得ることができる。   In this RTM molding method, a preform made of reinforcing fibers is placed in a mold, and a liquid matrix resin is injected to impregnate the reinforcing fibers with the matrix resin. Can be obtained.

RTM法などの樹脂注入成形法に適用するプリフォームは従来、平面状の強化繊維が配列した強化繊維基材を一枚一枚厚み方向に配置した強化繊維基材積層体を最終製品形状に準ずる形をした賦形型の上に搬送、配置して作成していた。しかしながら該強化繊維基材積層体を用いてプリフォームを作成する場合、該強化繊維基材積層体の積層層間は接合されていないことから、型への沿い性という点では優れるものの、賦形型への搬送中に該強化繊維基材積層体の配向角がずれたり、型に配置しているときに強化繊維基材がすべり落ちたりするなど、作業性が悪いこと、信頼性の高い強化繊維プラスチックが得にくいことに問題があった。   A preform applied to a resin injection molding method such as the RTM method conventionally conforms to a final shape of a reinforcing fiber substrate laminate in which reinforcing fiber substrates in which flat reinforcing fibers are arranged are arranged one by one in the thickness direction. It was created by transporting and placing it on a shaped shaping mold. However, when a preform is produced using the reinforcing fiber base laminate, the laminated layers of the reinforcing fiber base laminate are not joined. The reinforcing fiber base laminate is misaligned during transport to the fiber, and the reinforcing fiber base slips down when placed in a mold. There was a problem that it was difficult to obtain plastic.

そこで予め何らかの手段で強化繊維基材積層体の積層層間を接合した強化繊維基材積層体を製造することが試みられている。例えば、熱可塑性樹脂を含む樹脂材料により積層層間が接合された強化繊維基材積層体が提案されている(特許文献1)。該強化繊維基材積層体は、各強化繊維基材積層層間の厚み方向の接合力がある値以上であることから3次元形状の型に配置しても強化繊維基材が滑り落ちたりすることがなく、また強化繊維基材積層層間に樹脂材料を配置していることから衝撃付与後の圧縮強度などの力学特性に優れるなど、信頼性の高い強化繊維プラスチックを得ることができる。しかしながら、該強化繊維基材積層体を曲率半径の小さい部分に沿わせる場合、積層層間の滑りが円滑に起こらないために、皺が発生するなどの問題があった。   Therefore, an attempt has been made to produce a reinforcing fiber base laminate in which the layers between the reinforcing fiber base laminates are bonded in advance by some means. For example, a reinforcing fiber base laminate in which laminated layers are joined by a resin material containing a thermoplastic resin has been proposed (Patent Document 1). Since the reinforcing fiber base laminate has a bonding strength in the thickness direction between the reinforcing fiber base laminate layers of a certain value or more, the reinforcing fiber base may slide down even when arranged in a three-dimensional mold. In addition, since the resin material is arranged between the reinforcing fiber base laminate layers, a highly reliable reinforcing fiber plastic such as excellent mechanical properties such as compressive strength after application of impact can be obtained. However, when the reinforcing fiber base laminate is placed along a portion having a small radius of curvature, there is a problem that wrinkles occur because sliding between the laminated layers does not occur smoothly.

また別の例として、ニードルパンチにより強化繊維を起毛処理して、強化繊維基材積層体同士がブリッジングされたものが提案されている(特許文献2)。該強化繊維基材積層体においても、曲率半径の小さい部分に沿わせる場合、同様に皺が発生するなどの問題があった。   As another example, there has been proposed one in which reinforcing fibers are raised by needle punching and the reinforcing fiber base laminates are bridged together (Patent Document 2). The reinforcing fiber substrate laminate also has a problem that wrinkles are generated when it is along a portion having a small curvature radius.

一方、積層層間の滑りが円滑に起こる強化繊維基材積層体として、端部のみが熱可塑性樹脂で接合された強化繊維基材積層体が提案されている(特許文献3)。該強化繊維基材積層体を3次元形状に賦形した場合、端部の接合部を基点として各積層層間が滑動するため、皺のないプリフォームを作製することができる。しかしながら、該強化繊維基材積層体は、端部以外は接合されておらず、型に搬送している際や賦形しているときに強化繊維基材がめくれたり、配向角がずれたりするなどの問題があり、3次元形状のプリフォームを正確かつ効率よく作製するという点で不十分なものであった。
特開2004−114586号公報 特開2004−60058号公報 特開平5−185539号公報
On the other hand, a reinforcing fiber base laminate in which only end portions are joined with a thermoplastic resin has been proposed as a reinforcing fiber base laminate in which sliding between laminated layers smoothly occurs (Patent Document 3). When the reinforcing fiber base laminate is shaped into a three-dimensional shape, each laminated layer slides with the joint portion at the end as a base point, so that a preform without wrinkles can be produced. However, the reinforcing fiber base laminate is not joined except at the end, and the reinforcing fiber base is turned up or the orientation angle is shifted when being conveyed to a mold or when it is shaped. However, it was insufficient in that a three-dimensional shape preform was accurately and efficiently produced.
JP 2004-114586 A JP 2004-60058 A Japanese Patent Laid-Open No. 5-185539

本発明の目的は、かかる問題点を解決し、取り扱い性に優れ、3次元形状にも皺無く賦形できるとともに、優れた力学特性を有する強化繊維プラスチックが得られる強化繊維基材積層体を提供することにある。 An object of the present invention is to provide a reinforced fiber base laminate that solves such problems, has excellent handleability, can be shaped without difficulty even in a three-dimensional shape, and provides a reinforced fiber plastic having excellent mechanical properties. There is to do.

本発明はかかる課題を解決するために以下の構成を採るものである。すなわち、
(1)強化繊維基材を複数枚積層してなる平面状の強化繊維基材積層体であって、該強化繊維基材の積層層間の全面にわたって接合部が分布しており、該接合部は、ガラス転移温度Tgが0℃〜95℃である熱可塑性樹脂を含有する樹脂が2g/m〜40g/m付着しており、かつ、前記積層層間を形成する前記強化繊維基材両方に融着することにより形成されているとともに、前記積層層間が、接合力が500〜1000N/mである高接合領域と、前記高接合領域より接合部の分布する密度が低い低接合領域から形成されることを特徴とする強化繊維基材積層体。
The present invention adopts the following configuration in order to solve such a problem. That is,
(1) A planar reinforcing fiber substrate laminate formed by laminating a plurality of reinforcing fiber substrates, wherein joints are distributed over the entire surface between the laminated layers of the reinforcing fiber substrates, , a glass transition temperature Tg resin containing a thermoplastic resin is 2g / m 2 ~40g / m 2 are attached is a 0 ° C. to 95 ° C., and the both reinforcing fiber substrates forming the laminated layers In addition to being formed by fusing, the stacked layers are formed from a high bonding region having a bonding force of 500 to 1000 N / m 2 and a low bonding region in which the density of distribution of bonding portions is lower than that of the high bonding region. Reinforced fiber base laminate characterized by being made.

(2)前記高接合領域の積層層間における割合が1〜10%である前記(1)に記載の強化繊維基材積層体。   (2) The reinforcing fiber substrate laminate according to (1), wherein a ratio of the highly bonded region between the laminated layers is 1 to 10%.

(3)前記高接合領域が強化繊維基材積層体の端部からの幅1〜5cmの領域である前記(1)または(2)に記載の強化繊維基材積層体。   (3) The reinforcing fiber base laminate according to (1) or (2), wherein the high bonding region is a region having a width of 1 to 5 cm from an end of the reinforcing fiber base laminate.

(4)前記高接合領域の層間の接合力が低接合領域の層間の接合力に対して、1.5〜5倍である前記(1)〜(3)のいずれかに記載の強化繊維基材積層体。   (4) The reinforcing fiber group according to any one of (1) to (3), wherein a bonding force between the layers in the high bonding region is 1.5 to 5 times a bonding force between the layers in the low bonding region. Material laminate.

(5)前記(1)〜(4)のいずれかに記載の強化繊維基材積層体を賦形して得た強化繊維体積率Vpfが40%〜62%であるプリフォーム。   (5) A preform having a reinforcing fiber volume fraction Vpf of 40% to 62% obtained by shaping the reinforcing fiber substrate laminate according to any one of (1) to (4).

(6)強化繊維基材層間の全面にわたり、前記熱可塑性樹脂を含有する樹脂によって接着されている前記(5)に記載のプリフォーム。   (6) The preform according to (5), wherein the preform is bonded to the entire surface between the reinforcing fiber base layers with a resin containing the thermoplastic resin.

(7)前記(5)または(6)に記載のプリフォームに、マトリックス樹脂を注入、含浸、硬化して得られる強化繊維体積率Vfが35%〜72%の範囲内である繊維強化プラスチック成形品。   (7) Fiber reinforced plastic molding in which the reinforcing fiber volume fraction Vf obtained by injecting, impregnating and curing the matrix resin into the preform described in (5) or (6) is in the range of 35% to 72%. Goods.

(8)強化繊維基材の少なくとも片側の表面に、ガラス転移温度Tgが0℃〜95℃である熱可塑性樹脂を含有する樹脂が、2g/m〜40g/mの範囲内で付着されている強化繊維基材を用い、少なくとも次の工程(A)から(F)を経て強化繊維基材積層体を製造することを特徴とする繊維強化基材積層体の製造方法。
(A)強化繊維基材を所定の形状に裁断する裁断工程。
(B)前記所定の形状に裁断された強化繊維基材を、所定の積層構成に基づいて、順次、平面上に搬送・配置する積層工程。
(C)(B)で得られた積層体を加熱工程へ間欠的に搬送する搬送工程。
(D)搬送された積層体を加熱する加熱工程。
(E)該積層体を、加圧治具の一定面積当たりに有する加圧部の面積割合が、高い領域を1〜10%有する加圧治具を用いて加圧し、強化繊維基材の表面に付着している前記熱可塑性樹脂を含有する樹脂により、加圧部の強化繊維基材同士を厚み方向に接着する加圧接着工程。
(F)該積層体を冷却する冷却工程。
(8) on at least one surface of the reinforcing fiber substrate, resin containing a thermoplastic resin having a glass transition temperature Tg of 0 ° C. to 95 ° C. is deposited within a range of 2g / m 2 ~40g / m 2 A method for producing a fiber reinforced substrate laminate, comprising producing a reinforced fiber substrate laminate through at least the following steps (A) to (F) using the reinforcing fiber substrate.
(A) A cutting step of cutting the reinforcing fiber base into a predetermined shape.
(B) A laminating process in which the reinforcing fiber base material cut into the predetermined shape is sequentially transported and arranged on a plane based on a predetermined laminating configuration.
(C) The conveyance process which conveys the laminated body obtained by (B) intermittently to a heating process.
(D) The heating process which heats the conveyed laminated body.
(E) The surface of the reinforcing fiber substrate is pressed using a pressing jig having a region where the area ratio of the pressing part having a high area per fixed area of the pressing jig is 1 to 10%. A pressure bonding step in which the reinforcing fiber bases of the pressure portion are bonded in the thickness direction with the resin containing the thermoplastic resin adhering to the surface.
(F) A cooling step for cooling the laminate.

(9)強化繊維基材積層体の端部からの幅1〜5cmである端部領域を加圧する加圧治具の一定面積当たりの加圧部の面積割合が、前記端部領域以外を加圧する加圧治具の一定面積当たりの加圧部の面積割合に対して、1.5〜5倍である前記(8)に記載の繊維強化基材積層体の製造方法。   (9) The area ratio of the pressurizing unit per fixed area of the pressurizing jig that pressurizes the end region having a width of 1 to 5 cm from the end portion of the reinforcing fiber base laminate is other than the end region. The method for producing a fiber-reinforced substrate laminate according to (8), which is 1.5 to 5 times the area ratio of the pressing portion per fixed area of the pressing jig to be pressed.

本発明の強化繊維基材積層体は、取り扱い性が良好で、3次元形状にも優れた賦形性を有し、かつ、本発明の強化繊維基材積層体を用いた成形品は優れた力学特性を有する。   The reinforcing fiber base laminate of the present invention has good handleability, excellent shapeability even in a three-dimensional shape, and a molded article using the reinforcing fiber base laminate of the present invention is excellent. Has mechanical properties.

以下、本発明について、図を参照し、具体的に説明する。   Hereinafter, the present invention will be specifically described with reference to the drawings.

図1は、本発明の強化繊維基材積層体の一例を、図2は、本発明の強化繊維基材積層体における高接合領域の一例を示す斜視図である。図3は、本発明の強化繊維基材積層体の一例を示す断面図である。   FIG. 1 is a perspective view showing an example of a reinforcing fiber base laminate of the present invention, and FIG. 2 is an example of a highly bonded region in the reinforcing fiber base laminate of the present invention. FIG. 3 is a cross-sectional view showing an example of the reinforcing fiber base laminate of the present invention.

本発明の強化繊維基材積層体2は、シート状の強化繊維基材1を複数枚積層してなるものである。   The reinforcing fiber substrate laminate 2 of the present invention is formed by laminating a plurality of sheet-like reinforcing fiber substrates 1.

強化繊維基材1の形態としては、織物(一方向、多軸)、編物が挙げられる。中でも高い力学特性の成形品が得られることから一方向または2〜4軸の織物が好ましい。また多軸の織物としては、2軸の平織りを使用すると意匠面の要望が強い自動車用途を始め、各種産業用途に使用することできることから好ましい。   Examples of the form of the reinforcing fiber base 1 include woven fabric (unidirectional, multiaxial) and knitted fabric. Among them, a unidirectional or 2- to 4-axis woven fabric is preferable because a molded product having high mechanical properties can be obtained. In addition, it is preferable to use a biaxial plain weave as a multiaxial woven fabric because it can be used for various industrial applications including automotive applications where design demands are strong.

かかる強化繊維基材1の目付は、取り扱い性が良く、製造するコストが安くできることから、100〜1000g/m未満であることが好ましい。また該強化繊維基材積層体2で作成した成形品の所望の力学特性が得られる範囲ならば、適宜目付の異なる強化繊維基材1を組み合わせた構成にしても良い。 The basis weight of the reinforcing fiber substrate 1 is preferably 100 to less than 1000 g / m 2 because the handleability is good and the manufacturing cost can be reduced. Moreover, as long as the desired mechanical characteristics of the molded article made with the reinforcing fiber base laminate 2 can be obtained, the reinforcing fiber bases 1 having different basis weights may be appropriately combined.

強化繊維基材1の強化繊維としては、マルチフィラメントであり、特にその種類に制限はないが、例えば、ガラス繊維、アルミナ繊維、炭化ケイ素繊維、金属繊維、有機(ポリアラミド、PBO、液晶ポリマー繊維、PVA、PEポリフェニレンサルファイド繊維など)繊維または炭素繊維などが好ましく使用できる。これらの中でも、とくに炭素繊維は比強度および比弾性率に優れ、耐吸水性に優れるので、航空機や自動車などの構造材の強化繊維として好ましく用いられる。中でも、高靱性炭素繊維であると、成形される強化繊維プラスチックの衝撃吸収エネルギーが大きくなるので、各種産業用途はもとより航空機1次構造材としても適用が可能となる。   The reinforcing fiber of the reinforcing fiber base 1 is a multifilament, and the type thereof is not particularly limited. For example, glass fiber, alumina fiber, silicon carbide fiber, metal fiber, organic (polyaramid, PBO, liquid crystal polymer fiber, PVA, PE polyphenylene sulfide fiber, etc.) fiber or carbon fiber can be preferably used. Among these, carbon fibers are particularly preferred as reinforcing fibers for structural materials such as aircraft and automobiles because carbon fibers are excellent in specific strength and specific elastic modulus and excellent in water absorption resistance. Among them, when the tough carbon fiber is used, the impact-absorbing energy of the reinforced fiber plastic to be molded becomes large, so that it can be applied not only to various industrial uses but also as an aircraft primary structural material.

また、本発明の強化繊維基材積層体2は、平面状とするのが好ましい。ここでいう平面状とは、紙管などに巻いたとしても、解反したときに平面状に戻れば平面状と規定する。このように、紙管などに強化繊維基材積層体を巻き、解反した場合においては、多少の巻き癖が残り、厳密な平面とはならないこともあるが、かかる場合においては、強化繊維基材積層体が一次曲面形状であり、かつ、その50%以上の部分において曲率半径が、50cm以上であれば、平面と見なすものとする。   Moreover, it is preferable that the reinforcing fiber base laminate 2 of the present invention has a planar shape. The flat shape here is defined as a flat shape if it is wound around a paper tube or the like and then returns to a flat shape when unwound. As described above, when the reinforcing fiber base laminate is wound around a paper tube and then unwound, some curl may remain and may not be a strict flat surface. If the material laminate has a primary curved surface shape and the radius of curvature is 50 cm or more in a portion of 50% or more, it is regarded as a flat surface.

また、本発明の強化繊維基材積層体2は、その積層層間3の、全面にわたって接合部が分布しているものである。接合部とは、各層間3を構成している強化繊維基材1と強化繊維基材1とを固定することをいい、手段としては、樹脂による接着、起毛した繊維の絡み合い、ステッチ糸による固定等が挙げられる。中でも樹脂による接着が機械的に接合を外したり、加熱加圧することにより、再度接合できることから好ましい。また、接合部が全面にわたって分布しているとは、全面が隙間なく接合しているのではなく、接合部と非接合部が全面に混在していることをいう。かかる分布形態としては、接合部が連続した中に、非接合部が点在していても良いし、非接合部が連続した中に接合部が点在していても良いが、後者であれば、接続部の層間に占める割合をコントロールし易いため、後述する高接合領域と低接合領域を容易に設定できることから好ましい。   Further, the reinforcing fiber base laminate 2 of the present invention has joints distributed over the entire surface of the laminated layer 3. The joint means that the reinforcing fiber base 1 and the reinforcing fiber base 1 constituting each interlayer 3 are fixed. As a means, adhesion by resin, entanglement of raised fibers, fixing by stitch yarn Etc. Among them, the adhesion by the resin is preferable because it can be joined again by mechanically removing the joining or heating and pressing. Also, the fact that the joints are distributed over the entire surface means that the entire surface is not joined without a gap, but the joints and non-joint parts are mixed on the entire surface. As such distribution form, non-joined portions may be interspersed while the joined portions are continuous, or joint portions may be interspersed while the non-joined portions are continuous. For example, since the ratio of the connection portion between the layers can be easily controlled, a high bonding region and a low bonding region described later can be easily set.

本発明の強化繊維基材積層体2は、上記層間の接合形態として、接合力が500〜1000N/mである高接合領域と前記高接合領域より接合部の分布する密度が低い低接合領域から形成される。かかる2領域からなることで、プリフォーム化する際の形状への追随性と持ち運び等のハンドリング時に層間の接合が外れ難いという取扱い性を両立することが可能となったものである。すなわち、高接合領域5を、強化繊維基材積層体2を手、道具、機械などで搬送するときや型にセットするときに基材が剥離しやすい箇所(強化繊維基材1の端部や図2に示す基材と基材との継ぎ合わせ部7など)に設定することで、特に上記取扱い性を向上させることができるので好ましい。また、後のプリフォーム工程において、該強化繊維基材積層体2を所望の形状にカットする箇所に高接合領域5を設定すれば、形状カット後も基材の剥離を予防することができる。かかる高接合領域の接合力は500〜1000N/mであることが必要である。高接合領域5の接合力が500N/m未満であると、強化繊維基材積層体2の搬送中や取り扱い時に強化繊維基材1の端部が起点となり剥離してしまい、1000N/mを超えると賦形時に曲げ部分に沿うようなすべりが発生しにくくなり皺が発生してしまうためである。 The reinforcing fiber base laminate 2 of the present invention includes a high bonding region having a bonding force of 500 to 1000 N / m 2 and a low bonding region in which the density of distribution of bonding portions is lower than that of the high bonding region as the bonding form between the layers. Formed from. By comprising such two regions, it is possible to achieve both the following property to the shape when forming into a preform and the handling property that it is difficult to disconnect the layers during handling such as carrying. That is, when the high-bond region 5 is transported with a hand, a tool, a machine, or the like, or when it is set on a mold, the high-bonding region 5 is easily peeled off (such as the end of the reinforcing fiber base 1 or It is preferable to set the base material to the base material joining portion 7 shown in FIG. 2 because the handling property can be particularly improved. Further, in the subsequent preforming step, if the high bonding region 5 is set at a location where the reinforcing fiber base laminate 2 is cut into a desired shape, peeling of the base material can be prevented even after the shape cut. The bonding force in such a high bonding area needs to be 500 to 1000 N / m 2 . When the bonding force of the high bonding region 5 is less than 500 N / m 2 , the reinforcing fiber base material 2 is peeled from the end of the reinforcing fiber base material 1 during transportation or handling, resulting in 1000 N / m 2. This is because slipping along the bent portion is less likely to occur during shaping and wrinkles occur.

ここでいう接合力とは、積層層間3を剥がすのに要する応力をいう。以下に接合力を測定する方法を、図6を参照しながら説明する。   The term “bonding force” as used herein refers to the stress required to peel off the laminated layer 3. Hereinafter, a method of measuring the bonding force will be described with reference to FIG.

まず強化繊維基材積層体2から試験片(N数5、標準的には、100mm角だが、適宜変更可)を切り出し、該試験片の上下両面に十分な剛性を有するSUS板27(試験片とほぼ同形状)を全面にわたり両面テープ28などの粘着剤で接着させ試験体29を作製する。該両面テープ28の粘着力は、試験中に強化繊維基材積層体2の層間より先に試験片と上下両面の板が剥がれないように接着できれば、特に限定されるものではないが、JIS Z 0237(2000)に準拠した(90度粘着力、対SUS板)測定方法で30N/25mm以上あるのが好ましい。   First, a test piece (N number 5, standard 100 mm square, but can be changed as appropriate) is cut out from the reinforcing fiber base laminate 2 and a SUS plate 27 (test piece) having sufficient rigidity on both upper and lower surfaces of the test piece. The test body 29 is manufactured by adhering the entire surface with an adhesive such as a double-sided tape 28. The adhesive strength of the double-sided tape 28 is not particularly limited as long as it can be adhered so that the test piece and the upper and lower double-sided plates are not peeled off before the interlayer of the reinforcing fiber base laminate 2 during the test. It is preferable that it is 30 N / 25mm or more by the measuring method based on 0237 (2000) (90 degree | times adhesive force, SUS board).

次に該試験体29の下面を引っ張り試験機の台座30に前記両面テープ28で固定し、上面の中心位置に引っ張り試験機用取り付け治具31を前記両面テープ28で接着する。ここでは試験体29と取り付け治具31の中心軸が一直線上になるように注意する。
最後に取り付け治具31を引っ張り試験機にセットし、中心軸に平行に25mm/minの速度で荷重をかけ、層間3が剥がれたときの最大荷重(N)を読みとる。
Next, the lower surface of the test body 29 is fixed to the pedestal 30 of the tensile tester with the double-sided tape 28, and the tensile tester mounting jig 31 is bonded to the center of the upper surface with the double-sided tape 28. Here, care is taken that the central axes of the test body 29 and the mounting jig 31 are aligned.
Finally, the mounting jig 31 is set in a tensile testing machine, a load is applied parallel to the central axis at a speed of 25 mm / min, and the maximum load (N) when the interlayer 3 is peeled is read.

試験結果は以下の算出式から計算し接合力を求める。   The test result is calculated from the following calculation formula to obtain the bonding force.

Figure 0005029072
Figure 0005029072

高接合領域5と低接合領域6の見分け方は、図8を用いて以下の通りに説明される。   How to distinguish the high junction region 5 and the low junction region 6 will be described as follows with reference to FIG.

まず、強化繊維基材積層体2の長手方向32(すなわち、強化繊維基材積層体2の中で最も長い方向を意味し、例えば長方形の場合は長辺の方向を意味するが、正方形の場合はいずれか任意の辺の方向、多角形の場合は最も長い辺の方向、楕円の場合は長径の方向、円の場合は任意の方向など、長手方向と評価される得る方向を含む)を特定し、その方向に直角の方向を幅方向33とする。長さ方向に端部から少なくとも10mm以上の距離を有し、幅方向33にもっとも多くの試験片を切り出せる箇所において、強化繊維基材積層体2から幅方向33にわたり、幅50mm、長さ150mmの試験片34を等間隔に切り出し、上記測定方法に基づき、幅方向33の接合力の分布を求める。試験片34の数を10個以上作成できない幅であった場合は、試験片の数が10個となる大きさの試験片34(長さは幅の3倍とする)を作成する。   First, the longitudinal direction 32 of the reinforcing fiber base laminate 2 (that is, the longest direction in the reinforcing fiber base laminate 2, for example, in the case of a rectangle means the direction of the long side, but in the case of a square Specifies the direction of any side, the direction of the longest side in the case of a polygon, the direction of the major axis in the case of an ellipse, and the direction that can be evaluated as the longitudinal direction in the case of a circle) A direction perpendicular to the direction is defined as a width direction 33. At a location having a distance of at least 10 mm or more from the end in the length direction and the largest number of test pieces being cut out in the width direction 33, the reinforcing fiber base laminate 2 extends in the width direction 33, and the width is 50 mm and the length is 150 mm. The test pieces 34 are cut out at equal intervals, and the distribution of the bonding force in the width direction 33 is obtained based on the measurement method. If the width is such that ten or more test pieces 34 cannot be created, a test piece 34 (the length is three times the width) is created so that the number of test pieces is ten.

その後、強化繊維基材積層体2の面積を、これらの試験片34を用いて上記測定方法に基づき測定した接合力が500〜1000N/mの試験片34(高接合領域5)の数、およびその試験片34に含まれる接合部4の分布する密度(すなわち、単位面積あたりに対する接合部の面積または数)を求める。 Thereafter, the number of test pieces 34 (high bonding region 5) having a bonding force of 500 to 1000 N / m 2 , which is obtained by measuring the area of the reinforcing fiber base laminate 2 based on the measurement method using these test pieces 34, And the density (namely, the area or number of the junction part per unit area) which the junction part 4 contained in the test piece 34 distributes is calculated | required.

本発明では、上記の測定の結果、500〜1000N/mの試験片34に含まれる接合部4の分布する密度より、その他の試験片34に含まれる接合部4の分布する密度(すなわち、単位面積あたりに対する接合部の面積または数)が低くなっていれば良く、この場合、接合力が500〜1000N/mの高接合領域5と、高接合領域5より接合部の分布する密度が低い低接合領域4が形成されていると評価できる。 In the present invention, as a result of the above measurement, the density of the joints 4 included in the other test pieces 34 (that is, the density of the joints 4 included in the other test pieces 34 (ie, the density of the joints 4 included in the test pieces 34 of 500 to 1000 N / m 2 )). The area or the number of joints per unit area) only needs to be low. In this case, the joint strength is 500 to 1000 N / m 2 and the density of joints distributed from the high joint area 5 is high. It can be evaluated that the low low junction region 4 is formed.

高接合領域5は積層層間3で1〜10%有していることが好ましい。高接合領域5の範囲が1%未満であると、基材の剥離を予防する効果が小さく、10%より上であると、賦形時に曲げ部分に沿うような積層層間のすべりが発生しにくくなり、条件を厳密に設定しないと皺が発生する場合がある。なお、ここで言う、高接合領域5の積層層間における割合は、接合力が500〜1000N/mの試験片(高接合領域5)の数を、試験片の総数で除した割合とする。 It is preferable that the high junction region 5 is 1 to 10% in the laminated layer 3. If the range of the high bonding region 5 is less than 1%, the effect of preventing the peeling of the base material is small, and if it is above 10%, it is difficult for slippage between the laminated layers along the bent portion to occur during shaping. Therefore, if the conditions are not set strictly, there is a case where wrinkles occur. In addition, the ratio between the lamination | stacking layers of the high junction area | region 5 said here shall be the ratio which remove | divided the number of the test pieces (high junction area | region 5) whose joining force is 500-1000 N / m < 2 > by the total number of test pieces.

前記強化繊維基材積層体2の積層層間3の接合部4の分布は上述の効果が得られ、かつ高接合領域5の接合力が500〜1000N/mであれば、特に限定されるものではないが、層間の全面にわたりある間隔をもって分布していると好ましい。ある間隔をもって接合部が分布していることにより、層間3の接合も部分的になり自由度が生まれ、結果として賦形時に曲げ部分に皺なく沿うような積層層間のすべりが発生しやすくなる。 The distribution of the joint portions 4 between the laminated layers 3 of the reinforcing fiber base laminate 2 is particularly limited as long as the above-described effects are obtained and the joint strength of the high joint region 5 is 500 to 1000 N / m 2. However, it is preferable that it is distributed with a certain interval over the entire surface between the layers. Since the joints are distributed at a certain interval, the joints between the layers 3 are also partially made, and a degree of freedom is created. As a result, slipping between the laminated layers that easily follows the bent part is likely to occur during shaping.

接合部4の間隔は、接合する際の作業性が良いこと、所望の接合力が得やすいことから、高接合領域5においては、1〜30mmが好ましく、より好ましくは3〜10mmである。また低接合領域6においては接合部4の間隔は、15〜100mmが好ましい。接合部4の間隔が100mmより大きいと、接合間隔が広すぎるため、部分的に接合する効果が得られず、搬送中に基材の層間がすべり積層角度がずれてしまうため好ましくない。   The interval between the joining portions 4 is preferably 1 to 30 mm, more preferably 3 to 10 mm in the high joining region 5 because workability at the time of joining is good and a desired joining force is easily obtained. Moreover, in the low joining area | region 6, the space | interval of the junction part 4 has preferable 15-100 mm. If the distance between the joining portions 4 is larger than 100 mm, the joining distance is too wide, so that the effect of partial joining cannot be obtained, and the interlayer of the base material slips during conveyance, which is not preferable.

接合部4の個々の形状は、所望の接合力が得られるならば特に限定されず、球状もしくは角を面取りした矩形状のものが好ましい。接合部の面積は、あまり大きくし過ぎると層間の自由度が小さくなり皺を防止するような層間のすべりが生じにくくなり、また接合部の面積を小さくし過ぎると所望の接合力を得るために加圧部を増やす必要があることから、1〜100mmが好ましく、1〜50mmであればより好ましい。 The individual shape of the joint portion 4 is not particularly limited as long as a desired joining force can be obtained, and a spherical shape or a rectangular shape with chamfered corners is preferable. If the area of the joint is too large, the degree of freedom between the layers will be reduced and it will be difficult for slippage between layers to prevent wrinkles. If the area of the joint is too small, the desired bonding strength will be obtained. Since it is necessary to increase a pressurizing part, 1-100 mm < 2 > is preferable and if it is 1-50 mm < 2 >, it is more preferable.

図3は図1における接合部が前述の樹脂による場合を表した断面図である。かかる態様においては、前述の積層層間を接着する樹脂は、ガラス転移温度Tgが0〜95℃である熱可塑性樹脂を含有する樹脂(以下接着樹脂と記すこともある)であることが好ましい。該強化繊維基材の積層層間3の全面にわたってガラス転移温度Tgが0〜95℃である熱可塑性樹脂を含有する樹脂8が2g/m〜40g/mの範囲内で付着しており、かつ、接合部は、層間3にある樹脂8に熱を加えて軟化あるいは融解した状態にしてから、圧力を加えて強化繊維基材1と強化繊維基材1の両方に圧着または融着することにより形成されている。 FIG. 3 is a cross-sectional view showing the case where the joint in FIG. In such an embodiment, the above-described resin for bonding the laminated layers is preferably a resin containing a thermoplastic resin having a glass transition temperature Tg of 0 to 95 ° C. (hereinafter sometimes referred to as an adhesive resin). Resin 8 having a glass transition temperature Tg over the whole surface of the stacked layers 3 of reinforcing fiber base material contains a thermoplastic resin is 0 to 95 ° C. are attached within the 2g / m 2 ~40g / m 2 , In addition, the bonded portion is made to be in a softened or melted state by applying heat to the resin 8 in the interlayer 3 and then pressure-bonded or fused to both the reinforcing fiber base 1 and the reinforcing fiber base 1. It is formed by.

また、本発明の強化繊維基材1は、少なくとも片面の表面に、ガラス転移温度Tgが0℃〜95℃である熱可塑性樹脂を含有する樹脂8が、2g/m〜40g/mで付着されていることを特徴とする。かかる熱可塑性樹脂を含有する樹脂を配することにより、後述する力学特性の向上はもとより、強化繊維基材間の積層層間を、該熱可塑性樹脂を含有する樹脂で接着接合することができる。該熱可塑性樹脂を含有する樹脂8のTgが0℃未満であると、常温でべたつくため、取り扱いにくい強化繊維基材1となってしまう。一方、該樹脂のTgが95℃を越えると、常温でべたつきはないものの、強化繊維基材1同士を接合させるための加熱温度を高くする必要があり、接合させにくいものとなる。なお、ここで言うTgとは、示差走査熱量分析計DSC(Differential scanning calorimetry)により測定した値をいう。具体的には、JIS−K7121(1987)に従って、測定装置にPyris1 DSC(Perkin Elmer社製)を用いて、窒素雰囲気下にて昇温速度40℃/分で測定する。 Further, the reinforcing fiber base material 1 of the present invention, on at least one side surface, the resin 8 containing a thermoplastic resin having a glass transition temperature Tg of 0 ° C. to 95 ° C. is at 2g / m 2 ~40g / m 2 It is characterized by being attached. By arranging the resin containing such a thermoplastic resin, not only the mechanical properties described later can be improved, but also the laminated layers between the reinforcing fiber bases can be adhesively bonded with the resin containing the thermoplastic resin. When the Tg of the resin 8 containing the thermoplastic resin is less than 0 ° C., the resin 8 is sticky at room temperature, resulting in a reinforced fiber substrate 1 that is difficult to handle. On the other hand, when the Tg of the resin exceeds 95 ° C., there is no stickiness at room temperature, but it is necessary to increase the heating temperature for joining the reinforcing fiber bases 1 to each other, which makes it difficult to join. Here, Tg refers to a value measured by a differential scanning calorimeter DSC (Differential scanning calorimetry). Specifically, according to JIS-K7121 (1987), the measurement is performed using a Pyris1 DSC (manufactured by Perkin Elmer) at a heating rate of 40 ° C./min in a nitrogen atmosphere.

また、とりわけ、航空機の一次構造材用の材料においては、飛翔物の衝突や修理中における工具の落下による損傷の影響を受けにくいように、好ましくは衝撃後の残存圧縮強さ(Compression After Impact、以下CAIと記す)が高いことが要求される。   In particular, the material for the primary structural material of the aircraft is preferably subjected to a compression after impact (Compression After Impact), so that it is not easily affected by the impact of the flying object or the damage of the tool during the repair. (Hereinafter referred to as CAI) is required to be high.

前記熱可塑性樹脂を含有する樹脂8は、強化繊維基材1の表面に付着しているため、FRPの成形後においても、FRPを構成する強化繊維基材1の層間に含まれ、前記樹脂8を用いない場合に比べて、層間3を形成しやすい。この層間3は、マトリックス樹脂の他に前記樹脂8を含むため、熱可塑性樹脂に高靭性なものを用いた場合には、層間を選択的に高靱性化することが可能である。かかる層間の高靱性化により、FRPに衝撃を加えた時に、層間が変形もしくは破壊することにより、エネルギーを吸収することができるため、CAIを向上することができる。そのため、強化繊維基材1の表面に付着させる樹脂8を最適化することにより、接合性のみならず、耐衝撃吸収特性も向上させることができる。   Since the resin 8 containing the thermoplastic resin adheres to the surface of the reinforcing fiber base 1, it is contained between the layers of the reinforcing fiber base 1 constituting the FRP even after molding of the FRP. It is easier to form the interlayer 3 than in the case where no is used. Since the interlayer 3 includes the resin 8 in addition to the matrix resin, when a high-toughness thermoplastic resin is used, the interlayer can be selectively made tough. By increasing the toughness between layers, energy can be absorbed by deformation or destruction of the layers when an impact is applied to the FRP, so that CAI can be improved. Therefore, by optimizing the resin 8 to be attached to the surface of the reinforcing fiber base 1, not only the bondability but also the impact resistance absorption characteristics can be improved.

熱可塑性樹脂を含有する樹脂8の付着量が2g/m未満であると、付着量が少なすぎて、十分な接着接合が発現されない。一方、付着量が40g/mよりも多いと、付着量が多すぎて、FRPの重量が増加し、軽量化を損なう。この強化繊維基材1の表面に付着している熱可塑性樹脂を含有する樹脂8は、熱硬化性樹脂との混合物を使用することができる。強化繊維基材間の接着接合のみが要求されている場合においては、かかる樹脂8として、熱可塑性樹脂を単独で用いてもよいが、CAIなどの耐衝撃性が要求される場合においては、靱性の優れた熱可塑性樹脂と低粘度化しやすく強化繊維基材への接着が容易な熱硬化性樹脂との混合物を用いると、適度の靱性を有しながら強化繊維基材1への接着性を有することができる。 When the adhesion amount of the resin 8 containing the thermoplastic resin is less than 2 g / m 2 , the adhesion amount is too small and sufficient adhesive bonding is not exhibited. On the other hand, when the adhesion amount is more than 40 g / m 2 , the adhesion amount is too large, the weight of FRP increases, and the weight reduction is impaired. As the resin 8 containing a thermoplastic resin adhering to the surface of the reinforcing fiber base 1, a mixture with a thermosetting resin can be used. In the case where only adhesive bonding between the reinforcing fiber bases is required, a thermoplastic resin may be used alone as the resin 8, but in the case where impact resistance such as CAI is required, toughness When using a mixture of an excellent thermoplastic resin and a thermosetting resin that is easily reduced in viscosity and easy to adhere to the reinforcing fiber base, it has adhesiveness to the reinforcing fiber base 1 while having appropriate toughness be able to.

かかる熱硬化性樹脂としては、エポキシ樹脂、不飽和ポリエステル樹脂、ビニルエステル樹脂、フェノール樹脂などを使用することができる。また、熱可塑性樹脂としては、ポリ酢酸ビニル、ポリカーボネイト、ポリアセタール、ポリフェニレンオキシド、ポリフェニレンスルフィド、ポリアリレート、ポリエステル、ポリアミド、ポリアミドイミド、ポリイミド、ポリエーテルイミド、ポリスルホン、ポリエーテルスルホン、ポリエーテルエーテルケトン、ポリアラミド、ポリベンゾイミダゾール、ポリエチレン、ポリプロピレン、酢酸セルロースなどを使用することができる。   As such a thermosetting resin, an epoxy resin, an unsaturated polyester resin, a vinyl ester resin, a phenol resin, or the like can be used. The thermoplastic resins include polyvinyl acetate, polycarbonate, polyacetal, polyphenylene oxide, polyphenylene sulfide, polyarylate, polyester, polyamide, polyamideimide, polyimide, polyetherimide, polysulfone, polyethersulfone, polyetheretherketone, polyaramid. Polybenzimidazole, polyethylene, polypropylene, cellulose acetate and the like can be used.

熱可塑性樹脂を含有する樹脂8の形態としては、例えば粒子状、繊維状、フィルム状のものが挙げられる。中でも、プリフォームにおける強化繊維体積率を高くすることができる点から粒子の形態が好ましい。該粒子は、平均直径(楕円形の場合は平均短径)が小さければ、小さいほど均一に強化繊維基材積層体2の表面に分散させることが可能となるため、1mm以下が好ましく、250μm以下であればより好ましく、50μm以下がさらに好ましい。強化繊維基材積層体2の表面に配置した粒子の径が大きいほど表面の凹凸が大きくなり、強化繊維が屈曲する可能性があるので、強化繊維が配列した強化繊維基材積層体2表面における粒子の平均厚さは、5〜250μmの範囲であることが好ましい。   Examples of the form of the resin 8 containing a thermoplastic resin include particles, fibers, and films. Especially, the form of particle | grains is preferable from the point which can make the reinforcement fiber volume ratio in a preform high. If the average diameter (average short diameter in the case of an ellipse) is small, the particles can be uniformly dispersed on the surface of the reinforcing fiber base laminate 2, and therefore, the diameter is preferably 1 mm or less, preferably 250 μm or less. Is more preferable, and 50 μm or less is more preferable. As the diameter of the particles arranged on the surface of the reinforcing fiber base laminate 2 increases, the surface unevenness increases and the reinforcing fibers may be bent. Therefore, the surface of the reinforcing fiber base laminate 2 on which the reinforcing fibers are arranged The average thickness of the particles is preferably in the range of 5 to 250 μm.

高接合領域5は強化繊維基材積層体の端部からの幅1〜5cmであることが好ましい。端部からの幅を5cmより上にすると、賦形時に曲げ部分に沿うようなすべりが発生しにくいことがあり、1cm未満であると、基材端部の剥離を防止する効果が得にくいことがある。   The high bonding region 5 preferably has a width of 1 to 5 cm from the end of the reinforcing fiber base laminate. If the width from the edge is higher than 5 cm, slipping along the bent part may not occur easily during shaping, and if it is less than 1 cm, it is difficult to obtain the effect of preventing peeling of the substrate edge. There is.

ここでいう端部とは、長手方向または幅方向の端部のことであり、所望の効果が得られる範囲で適宜選択することができる。またプリフォーム作製時に端部領域の幅が1〜5cmであると、端部領域の中央付近をカットしていくときに作業性がよい。   The term “end portion” as used herein refers to an end portion in the longitudinal direction or the width direction, and can be appropriately selected within a range in which a desired effect can be obtained. Further, when the preform has a width of 1 to 5 cm at the end region, workability is good when the vicinity of the center of the end region is cut.

また強化繊維基材積層体2の幅1〜5cmの端部領域の接合力は、低接合領域に対して1.5〜5倍であると、基材端部の剥離がなく取り扱い性が良いこと、賦形時に曲げ部分に皺なく沿うような積層層間のすべりが発生しやすいことから好ましい。   In addition, the bonding strength of the end region having a width of 1 to 5 cm of the reinforcing fiber substrate laminate 2 is 1.5 to 5 times that of the low bonding region, so that the end of the substrate is not peeled and the handleability is good. In particular, it is preferable because slippage between the laminated layers is likely to occur along the bent portion at the time of shaping.

前記強化繊維基材積層体2の積層層間の全面にわたる接合として、所望の接合力が得られるならば特に限定されるものではなく、ステッチ糸による縫合一体化も可能である。ステッチ糸で縫合一体化すると各層間は滑りが発生する自由度があるので、曲面に沿わせても強化繊維糸条が局部的に屈曲するようなことはないので好ましい。   The joining over the entire surface of the laminated layers of the reinforcing fiber base laminate 2 is not particularly limited as long as a desired joining force can be obtained, and stitching integration with stitch yarns is also possible. When the stitches are stitched together with stitch yarns, there is a degree of freedom for slippage between the respective layers. Therefore, the reinforcing fiber yarns are not locally bent even if they are along the curved surface.

縫合一体化にあたってのステッチ糸が形成する縫い組織としては、単環縫い、トリコット編みが挙げられる。また高接合領域5においてステッチ糸の打ち込み密度を他の領域よりも大きくすれば所望の接合力が得られやすく都合が良い。ここでいうステッチ糸の打ち込み密度とは、単位面積当たりのステッチ糸の打ち込み数の程度をいい、ここでは長さ方向の打ち込みピッチと幅方向の打ち込みピッチで定義する。
高接合領域5においては、取り扱い時に基材が剥離しないこと、賦形性が損なわれないことから長さ方向の打ち込みピッチは1〜6mmが好ましく、幅方向の打ち込みピッチは2〜10mmが好ましい。またそれ以外の領域においては、ステッチ糸に強化繊維基材積層体2の層間の拘束が甘く形態が不安定となり、運搬の際に層がずれることから、長さ方向の打ち込みピッチは3〜10mmが好ましく、幅方向の打ち込みピッチは3〜40mmが好ましい。
Examples of the stitch structure formed by the stitch yarn upon the stitching integration include single ring stitching and tricot stitching. In addition, if the stitching density of the stitch yarn is made larger in the high bonding area 5 than in other areas, it is easy to obtain a desired bonding force. The stitch yarn driving density here refers to the number of stitch yarns driven per unit area, and is defined by the driving pitch in the length direction and the driving pitch in the width direction.
In the high bonding region 5, since the base material does not peel during handling and the shapeability is not impaired, the driving pitch in the length direction is preferably 1 to 6 mm, and the driving pitch in the width direction is preferably 2 to 10 mm. In the other regions, the stitching yarn is loosely restrained between the layers of the reinforcing fiber base laminate 2 and the form becomes unstable, and the layer is displaced during transportation, so the driving pitch in the length direction is 3 to 10 mm. The driving pitch in the width direction is preferably 3 to 40 mm.

また、ステッチ糸による縫合一体化による積層層間の接合の場合においても、該強化繊維基材の積層層間3の全面にわたってガラス転移温度Tgが0〜95℃である熱可塑性樹脂を含有する樹脂8が2g/m〜40g/mの範囲内で付着していることが、後述するプリフォーム化後の形態固定を可能とする。 In addition, even in the case of joining between laminated layers by stitching integration with stitch yarn, a resin 8 containing a thermoplastic resin having a glass transition temperature Tg of 0 to 95 ° C. over the entire surface of the laminated layers 3 of the reinforcing fiber base is it allows for form fixed after preform of which will be described later adhered within the 2g / m 2 ~40g / m 2 .

本発明の強化繊維基材積層体2は、FRPを構成する積層構成となっていることが好ましいが、FRPを構成する積層構成の積層枚数が非常に多い場合には、強化繊維基材積層体2は、FRPを構成する積層構成の一部を構成する積層構成であっても構わない。例えば、FRPを構成する積層構成が[(45/0/−45/90)]の場合(Xは任意の整数)、繰り返しの積層単位である(45/0/−45/90)の積層構成を有する強化繊維基材積層体2を必要分だけ積層しても構わない。 It is preferable that the reinforcing fiber base laminate 2 of the present invention has a laminated configuration that constitutes the FRP. However, when the number of laminates constituting the FRP is very large, the reinforcing fiber substrate laminate is provided. 2 may be a laminated structure constituting a part of the laminated structure constituting the FRP. For example, when the laminated structure constituting the FRP is [(45/0 / −45 / 90) x ] s (X is an arbitrary integer), it is a repetitive laminated unit (45/0 / −45 / 90) You may laminate | stack the reinforcement fiber base material laminated body 2 which has a laminated structure only for a required part.

このように本発明の強化繊維基材積層体2は賦形性及び取り扱い性に優れるため、高品質なプリフォームを得ることができる。本発明においてプリフォームとは、平面状の強化繊維基材積層体ではなく、賦形型もしくはそれに類似の型などを用いて最終製品の成形品の形状もしくはそれに近い形状のように整えた中間体のことを意味する。   Thus, since the reinforcing fiber base laminate 2 of the present invention is excellent in formability and handleability, a high-quality preform can be obtained. In the present invention, the preform is not a flat reinforcing fiber base material laminate, but an intermediate that is shaped like the shape of the final product or a shape close to it using a shaping die or a similar die. Means that.

本発明のように、プリフォームにマトリックス樹脂を注入してFRPを成形する方法においては、FRPの品質の善し悪しはプリフォームで決まると言っても過言ではないため、高品質なプリフォームを得ることができる強化繊維基材積層体2は、非常に重要である。   In the method of molding the FRP by injecting the matrix resin into the preform as in the present invention, it is not an exaggeration to say that the quality of the FRP is determined by the preform, so a high quality preform is obtained. The reinforcing fiber base laminate 2 that can be used is very important.

本発明のプリフォームは、上記本発明の強化繊維基材積層体2を賦形して得られ、且つ強化繊維体積率Vpfが40%〜62%の範囲内であることが好ましい。   The preform of the present invention is preferably obtained by shaping the reinforcing fiber substrate laminate 2 of the present invention, and the reinforcing fiber volume fraction Vpf is preferably in the range of 40% to 62%.

該強化繊維体積率Vpfが40%未満であると、プリフォームが嵩高となるので、成形品であるFRPの強化繊維体積率が低下することがある。一方、該強化繊維体積率Vpfが62%よりも大きいと、マトリックス樹脂が含浸しにくくなり、未含浸やボイドなどの欠陥が発生しやすくなることがある。プリフォームの強化繊維体積率は、強化繊維基材積層体2を賦形型などを用いて賦形した後、熱可塑性樹脂を含有する樹脂のガラス転移温度以上に加熱した状態において、真空圧やプレス圧などの圧力を一定時間かけることにより、向上させることができる。この場合、加熱温度、圧力が高く、加熱・加圧時間が長い程、強化繊維体積率を向上させることができる。これらの加熱温度、圧力、加熱加圧時間を適切に制御することにより、プリフォームの強化繊維体積率を制御することが可能である。   If the reinforcing fiber volume fraction Vpf is less than 40%, the preform becomes bulky, and the reinforcing fiber volume fraction of the FRP that is a molded product may be lowered. On the other hand, when the reinforcing fiber volume fraction Vpf is larger than 62%, it is difficult to impregnate the matrix resin, and defects such as non-impregnation and voids are likely to occur. The volume ratio of the reinforcing fiber in the preform is such that, after the reinforcing fiber base laminate 2 is shaped using a shaping mold or the like, it is heated at a temperature higher than the glass transition temperature of the resin containing the thermoplastic resin, It can be improved by applying pressure such as pressing pressure for a certain period of time. In this case, the higher the heating temperature and pressure and the longer the heating / pressurizing time, the higher the reinforcing fiber volume fraction can be improved. By appropriately controlling the heating temperature, pressure, and heating and pressing time, it is possible to control the reinforcing fiber volume fraction of the preform.

さらに本発明のプリフォームは、強化繊維基材層間が実質的に全面にわたり接着していることが好ましいかかるプリフォームの具体的な製造方法の一例について以下に述べる。   Further, the preform of the present invention will be described below with reference to an example of a specific method for producing such a preform in which the reinforcing fiber base layer is preferably bonded substantially over the entire surface.

まず、該強化繊維基材積層体2を所望の形状にカットする。このとき予め形状カット箇所を含む領域を高接合領域5に設定しておけば、形状カット後も基材剥離がなく取り扱い性の低下を予防することができる。次に該形状カット後の強化繊維基材積層体2を賦形型などに配置した後、強化繊維基材積層体全体をバギングフィルム(もしくはラバーシート)で覆い、バギングフィルムと強化繊維基材積層体との間を真空吸引して、強化繊維基材積層体全体に大気圧をかけることにより賦形型に密着させて作製する。もしくは、賦形型とプレス機を用いて、強化繊維基材積層体に圧力をかけて、プリフォームを作製することも可能である。このように、プリフォームは最終製品もしくはそれに近い形状に整えられるため、一度形状を整えた後は、マトリックス樹脂を注入してFRPに成形するまで、形状を保持している必要がある。そのため、該強化繊維基材1もしくは該強化繊維基材積層体2を賦形型などに賦形して、プリフォーム形状に整えた後、該強化繊維基材層間を実質的に全面にわたり接着させることは、プリフォームの形状を保持しやすくなるため好ましい。   First, the reinforcing fiber base laminate 2 is cut into a desired shape. At this time, if the region including the shape cut portion is set as the high bonding region 5 in advance, the base material is not peeled after the shape cut, and the handling property can be prevented from being lowered. Next, the reinforcing fiber base laminate 2 after the shape cut is placed in a shaping mold, and then the entire reinforcing fiber base laminate is covered with a bagging film (or rubber sheet) to laminate the bagging film and the reinforcing fiber base. A vacuum is drawn between the body and the whole of the reinforcing fiber base laminate is made to be in close contact with the shaping mold by applying atmospheric pressure. Alternatively, a preform can be produced by applying pressure to the reinforcing fiber base laminate using a shaping mold and a press. Thus, since the preform is adjusted to a final product or a shape close thereto, after the shape is adjusted, it is necessary to maintain the shape until the matrix resin is injected and molded into FRP. Therefore, the reinforcing fiber base material 1 or the reinforcing fiber base material laminate 2 is shaped into a shaping mold or the like and arranged into a preform shape, and then the reinforcing fiber base material layers are bonded substantially over the entire surface. This is preferable because the shape of the preform is easily retained.

次に、本発明のFRPの製造方法は、本発明で好ましく用いられる強化繊維体積率40%〜62%のプリフォームにマトリックス樹脂を注入し、真空吸引口からマトリックス樹脂が排出された後に、注入口からマトリックス樹脂の注入を中止し、真空吸引口からのマトリックス樹脂の排出量を調整すれば、FRPの強化繊維体積率Vfを35%〜72%に成形することができる。   Next, in the FRP production method of the present invention, a matrix resin is injected into a preform having a reinforcing fiber volume ratio of 40% to 62% that is preferably used in the present invention, and the matrix resin is discharged from the vacuum suction port. If the injection of the matrix resin from the inlet is stopped and the discharge amount of the matrix resin from the vacuum suction port is adjusted, the FRP reinforcing fiber volume fraction Vf can be molded to 35% to 72%.

得られるFRPの強化繊維体積率Vfに特に制限はないが、35%よりも低いと、FRPとして強度、弾性率が低くなりやすく、所定の力学特性を発現するためには、厚みが必要となり、結果として軽量化の効果が小さくなる懸念がある。   There is no particular limitation on the reinforcing fiber volume fraction Vf of the FRP to be obtained, but if it is lower than 35%, the strength and elastic modulus of the FRP tend to be low, and a thickness is required to express the predetermined mechanical properties. As a result, there is a concern that the effect of weight reduction is reduced.

一方、強化繊維体積率Vfが72%よりも高いと、マトリックス樹脂の量が少なすぎることにより、ボイドなどの欠陥が発生しやすくなる場合がある。   On the other hand, if the reinforcing fiber volume fraction Vf is higher than 72%, defects such as voids may easily occur due to the amount of the matrix resin being too small.

また、FRPを構成する強化繊維基材の積層枚数が20枚以上のように、積層枚数が多いFRPを成形する場合においては、マトリックス樹脂の硬化特性を考慮し、プリフォームへの注入時間を確保した上で、マトリックス樹脂を加熱、粘度を低下させて注入することも好ましい。また、同時にマトリックス樹脂を注入するプリフォームを加熱しておくことも好ましい。比較的高い強化繊維体積率VfのFRPを成形するために、高強化繊維体積率Vfのプリフォームを使用する場合、プリフォームの強化繊維密度が高くなるため、マトリックス樹脂の含浸性が低下する傾向にある。この場合においても、マトリックス樹脂を加熱することにより粘度を低下させて、注入、含浸させることが好ましい。   In addition, when molding FRP with a large number of laminated sheets, such as the number of laminated reinforcing fiber bases constituting the FRP, more than 20 sheets, ensuring the injection time into the preform in consideration of the curing characteristics of the matrix resin In addition, it is also preferable to inject the matrix resin while heating and reducing the viscosity. It is also preferable to heat the preform into which the matrix resin is injected at the same time. When a preform having a high reinforcing fiber volume fraction Vf is used to form an FRP having a relatively high reinforcing fiber volume fraction Vf, the reinforcing fiber density of the preform increases, and the impregnation property of the matrix resin tends to decrease. It is in. Even in this case, it is preferable to lower the viscosity by heating the matrix resin, and to inject and impregnate it.

より好ましくは、注入口からマトリックス樹脂の注入を中止した後、該注入口を真空吸引し、該注入口および従来の真空吸引口の両方からマトリックス樹脂を吸引、排出し、且つマトリックス樹脂の排出量を調整して、FRPの強化繊維体積率Vfが35%〜72%に成形することである。   More preferably, after stopping the injection of the matrix resin from the injection port, the injection port is vacuumed, the matrix resin is sucked and discharged from both the injection port and the conventional vacuum suction port, and the discharge amount of the matrix resin To adjust the FRP reinforcing fiber volume fraction Vf to 35% to 72%.

マトリックス樹脂を注入口および/もしくは真空吸引口から排出させる時に、プリフォームに外部より加圧して、より短時間でマトリックス樹脂を排出することも好ましい。   When discharging the matrix resin from the injection port and / or the vacuum suction port, it is also preferable to pressurize the preform from the outside and discharge the matrix resin in a shorter time.

また、FRPの強化繊維体積率Vfは、プリフォームの強化繊維体積率Vpf―5%〜Vpf+20%に調節することが好ましい。FRPの強化繊維体積率は、プリフォームにマトリックス樹脂を注入した後、吸引口および/もしくは真空吸引口からマトリックス樹脂を吸引する時間や温度、さらにはプリフォームへの外部からの加圧などにより、マトリックス樹脂の排出量を制御することが可能である。   Further, the reinforcing fiber volume fraction Vf of FRP is preferably adjusted to the reinforcing fiber volume fraction Vpf−5% to Vpf + 20% of the preform. The reinforcing fiber volume fraction of FRP is determined by the time and temperature at which the matrix resin is sucked from the suction port and / or the vacuum suction port after injecting the matrix resin into the preform, and further the external pressurization to the preform. It is possible to control the discharge amount of the matrix resin.

本発明に用いる強化繊維基材1には、表面に熱可塑性樹脂を含有する樹脂8が付着しており、該樹脂は強化繊維基材同士を接着して、強化繊維基材積層体2およびプリフォームの形状保持性などの取り扱い性を向上させる機能の他に、CAIなどの耐衝撃性能を向上させる機能を発現する。かかる接着樹脂に耐衝撃性能の向上を期待する場合には、FRPを成形後に、強化繊維層間に、接着樹脂を含む層が形成されていることが好ましい。   The reinforcing fiber base 1 used in the present invention has a resin 8 containing a thermoplastic resin attached to the surface, and the resin adheres the reinforcing fiber bases to each other, and the reinforcing fiber base laminate 2 and the plug. In addition to the function of improving the handleability such as the shape retention of the reform, the function of improving the impact resistance performance such as CAI is developed. When such an adhesive resin is expected to have improved impact resistance, it is preferable that a layer containing the adhesive resin is formed between the reinforcing fiber layers after molding the FRP.

一方、FRPの製造時に、マトリックス樹脂の排出量を増加することにより、FRPの強化繊維体積率Vfを向上させることができるが、マトリックス樹脂を注入するときには、前述のようにマトリックス樹脂および/もしくはプリフォームを加熱して注入する場合がある。加熱温度が強化繊維基材1の表面に付着している熱可塑性樹脂を含有する樹脂のガラス転移温度を超える場合は、該樹脂が軟化して、強化繊維基材1の表面から脱落し、強化繊維基材1の層間3を形成するマトリックス樹脂の中に配置する場合がある。   On the other hand, the FRP reinforcing fiber volume fraction Vf can be improved by increasing the discharge amount of the matrix resin at the time of manufacturing the FRP. However, when the matrix resin is injected, the matrix resin and / or the plug as described above are used. The reform may be heated and poured. When the heating temperature exceeds the glass transition temperature of the resin containing the thermoplastic resin adhering to the surface of the reinforcing fiber base 1, the resin softens and falls off from the surface of the reinforcing fiber base 1 and strengthens. In some cases, it is disposed in a matrix resin that forms the interlayer 3 of the fiber substrate 1.

かかる場合には、FRPの強化繊維体積率Vfをプリフォームの強化繊維体積率Vpf+20%を越えるような高強化繊維体積率Vf化するために、マトリックス樹脂の排出量を増やすと、強化繊維基材の表面に付着していた接着樹脂が脱落してマトリックス樹脂内に配置、もしくはマトリックス樹脂に相溶するなどして、マトリックス樹脂内に含まれている場合に、マトリックス樹脂の排出に伴い、多量の熱可塑性樹脂を含有する樹脂も排出してしまう懸念がある。マトリックス樹脂の排出に伴う熱可塑性樹脂を含有する樹脂8の排出は、該樹脂8の機能が、FRPを成形するまでの強化繊維基材積層体2および/もしくはプリフォームの取り扱い性他を向上させることのみで、FRPを構成する要素としての機能が無い場合には問題ないが、熱可塑性樹脂を含有する樹脂はFRPの耐衝撃特性を向上させるなどの機能を発現することを期待する場合には、好ましくない。   In such a case, if the discharge amount of the matrix resin is increased in order to make the reinforcing fiber volume fraction Vf of the FRP higher than that of the preform reinforcing fiber volume fraction Vpf + 20%, If the adhesive resin attached to the surface of the resin falls off and is placed in the matrix resin or is compatible with the matrix resin, it is contained in the matrix resin. There is a concern that a resin containing a thermoplastic resin may also be discharged. The discharge of the resin 8 containing the thermoplastic resin accompanying the discharge of the matrix resin is such that the function of the resin 8 improves the handling of the reinforcing fiber base laminate 2 and / or the preform until the FRP is molded. However, there is no problem when there is no function as an element constituting FRP, but when a resin containing a thermoplastic resin is expected to exhibit functions such as improving the impact resistance characteristics of FRP. It is not preferable.

一方、熱可塑性樹脂を含有する樹脂8の機能が、FRPを成形するまでの強化繊維基材および/もしくはプリフォームの取り扱い性他を向上させるのみで、FRPを構成する要素としての機能を期待しない場合には、マトリックス樹脂、プリフォームを加熱して、該樹脂8を強化繊維基材の表面から脱落もしくはマトリックス樹脂に相溶させるなどして、マトリックス樹脂を排出すると共に、該樹脂8を積極的に排出することも好ましい様態の一つである。上述のように、該樹脂8はFRPを構成する強化繊維基材1の層間3を形成しやすいため、FRPの耐衝撃特性を向上させる反面、FRPの強化繊維体積率Vf向上を阻害する懸念があり、FRPの高強化繊維体積率Vf化による圧縮および/もしくは引張特性の向上を阻害する懸念がある。そのため、接着樹脂を積極的に排出して、層間の厚みの増加を抑制し、高強化繊維体積率Vf化することによって、圧縮および/もしくは引張特性を向上することが可能となる。   On the other hand, the function of the resin 8 containing the thermoplastic resin only improves the handleability of the reinforcing fiber base and / or preform until the FRP is molded, and does not expect a function as an element constituting the FRP. In such a case, the matrix resin and the preform are heated, and the resin 8 is removed from the surface of the reinforced fiber base material or is dissolved in the matrix resin. It is also a preferable aspect to discharge the water. As described above, since the resin 8 easily forms the interlayer 3 of the reinforcing fiber base 1 constituting the FRP, the impact resistance characteristic of the FRP is improved, but there is a concern that the improvement of the reinforcing fiber volume fraction Vf of the FRP is hindered. Yes, there is a concern that the compression and / or tensile property improvement due to the high reinforcing fiber volume fraction Vf of FRP is hindered. For this reason, it is possible to improve the compression and / or tensile properties by positively discharging the adhesive resin to suppress an increase in the thickness between the layers and obtaining a high reinforcing fiber volume fraction Vf.

また、プリフォームにマトリックス樹脂を注入し、真空吸引口からマトリックス樹脂が排出された後に、注入口からマトリックス樹脂の注入を中止し、注入口も真空吸引することにより、注入口および真空吸引口からのマトリックス樹脂の排出量を調整して、FRPの強化繊維体積率Vfが35%〜72%にすることも好ましい。   In addition, after the matrix resin is injected into the preform and the matrix resin is discharged from the vacuum suction port, the injection of the matrix resin is stopped from the injection port, and the injection port is also vacuumed, so that the injection port and the vacuum suction port It is also preferable to adjust the discharge amount of the matrix resin so that the reinforcing fiber volume fraction Vf of the FRP is 35% to 72%.

なお、本発明における「プリフォームの強化繊維体積率Vpf」とは、以下により定義されて測定される値であり、プリフォームとはマトリックス樹脂を注入する以前の状態のものをいう。
すなわち、プリフォームの強化繊維体積率Vpfは、プリフォームに大気圧相当の圧力0.1MPaをかけた状態におけるプリフォームの厚み(t)から、次の式を用いて表すことができる。
The “preform reinforcing fiber volume fraction Vpf” in the present invention is a value defined and measured as follows, and the preform refers to a state before the matrix resin is injected.
That is, the reinforcing fiber volume fraction Vpf of the preform can be expressed by using the following formula from the thickness (t) of the preform in a state where a pressure equivalent to atmospheric pressure of 0.1 MPa is applied to the preform.

プリフォームの強化繊維体積率Vpf=F×p/ρ/t/10 (%)
ここで、
F:基材目付(g/m
p:基材の積層枚数(枚)
ρ:強化繊維の密度(g/cm
t:プリフォームの厚み(mm)。
Preform reinforcing fiber volume fraction Vpf = F × p / ρ / t / 10 (%)
here,
F: Base material weight (g / m 2 )
p: Number of laminated substrates (sheets)
ρ: Density of reinforcing fiber (g / cm 3 )
t: Preform thickness (mm).

具体的なプリフォームの厚みの測定方法としては、JIS R 7602(1995)に記載の炭素繊維織物試験方法に記載の厚さの測定方法にて圧力を0.1MPaに変更して、測定することにより得ることができる。真空圧を利用したVaRTM成形方法においては、プリフォームに大気圧をかけた状態において、マトリックス樹脂を注入、含浸させるため、大気圧相当の0.1MPaの圧力をかけたときのプリフォームの強化繊維体積率を制御しておくことが好ましいのである。プリフォームが複雑な形状をしていて、JIS R 7602(1995)に基づいて測定ができない場合には、プリフォームからサンプルを切り出して、測定してもよい。この場合、切り出すことにより、プリフォームの厚みが変化しないように注意してサンプルを切り出すことが必要である。また、サンプルの切り出しも不可能な場合は、プリフォームを賦形した金型ごとバギングフィルムを用いて、真空バッグすることにより、プリフォームに大気圧をかけた状態にて、プリフォーム、金型、バギングフィルムの合計の総厚みを測定し、総厚みから金型、バギングフィルムの厚みを差し引くことにより、プリフォームの厚みを測定することも可能である。   As a specific method for measuring the thickness of the preform, the pressure should be changed to 0.1 MPa by the thickness measuring method described in the carbon fiber fabric test method described in JIS R 7602 (1995). Can be obtained. In the VaRTM molding method using vacuum pressure, the preform reinforcing fiber when pressure of 0.1 MPa corresponding to atmospheric pressure is applied to inject and impregnate the matrix resin in a state where atmospheric pressure is applied to the preform. It is preferable to control the volume ratio. When the preform has a complicated shape and cannot be measured based on JIS R 7602 (1995), a sample may be cut out from the preform and measured. In this case, it is necessary to cut out the sample with care so that the thickness of the preform does not change by cutting out. In addition, if it is impossible to cut out the sample, the preform and mold are placed under a pressure applied to the preform by vacuum bagging with a bagging film together with the mold shaped preform. It is also possible to measure the thickness of the preform by measuring the total thickness of the bagging film and subtracting the thickness of the mold and bagging film from the total thickness.

また、本発明における「FRPの強化繊維体積率Vf」とは、以下により定義されて測定される値であり、プリフォームに対してマトリックス樹脂を注入、硬化した後の状態でのものをいう。すなわち、FRPの強化繊維体積率Vfの測定は、FRPの厚み(t)から、上記と同様に下記する式を用いて表すことができる。
FRPの強化繊維体積率Vf=F×p/ρ/t/10(%)
ここで、tはFRPの厚み(mm)であるが、他のパラメータは、上記のプリフォームの強化繊維体積率Vpfを求めるときのパラメータ値と同様である。
F:基材目付(g/m
p:基材の積層枚数(枚)
ρ:強化繊維の密度(g/cm
t:FRPの厚み(mm)。
The “FRP reinforcing fiber volume fraction Vf” in the present invention is a value defined and measured by the following, and refers to a state after the matrix resin is injected into the preform and cured. That is, the measurement of the reinforcing fiber volume fraction Vf of FRP can be expressed from the thickness (t) of the FRP using the following formula in the same manner as described above.
Reinforced fiber volume fraction of FRP Vf = F × p / ρ / t / 10 (%)
Here, t is the thickness (mm) of the FRP, but the other parameters are the same as the parameter values for obtaining the reinforcing fiber volume fraction Vpf of the preform.
F: Base material weight (g / m 2 )
p: Number of laminated substrates (sheets)
ρ: Density of reinforcing fiber (g / cm 3 )
t: FRP thickness (mm).

なお、基材目付Fや基材の積層枚数、強化繊維の密度が明らかでない場合は、JIS K 7075(1991)に基づく燃焼法もしくは硝酸分解法、硫酸分解法のいずれかにより、FRPの強化繊維体積率を測定する。この場合に用いる強化繊維の密度は、JIS R 7603(1999)に基づき測定した値を用いる。   If the basis weight F, the number of laminated base materials, and the density of the reinforcing fibers are not clear, the FRP reinforcing fibers can be obtained by either the combustion method based on JIS K 7075 (1991), the nitric acid decomposition method, or the sulfuric acid decomposition method. The volume ratio is measured. As the density of the reinforcing fiber used in this case, a value measured based on JIS R 7603 (1999) is used.

具体的なFRPの厚みの測定方法としては、FRPの厚みを正しく測定できる方法であれば、特に限定されるものではないが、JIS K 7072(1991)に記載されているようにJIS B 7502(1994)に規定のマイクロメーターまたはこれと同等以上の精度をもつもので測定することが好ましい。FRPが複雑な形状をしていて、測定ができない場合には、FRPからサンプル(測定用としてのある程度の形と大きさを有しているサンプル)を切り出して、測定してもよい。   A specific method for measuring the thickness of FRP is not particularly limited as long as it can correctly measure the thickness of FRP. However, as described in JIS K 7072 (1991), JIS B 7502 ( It is preferable to measure with a micrometer specified in 1994) or with a precision equivalent to or better than that. If the FRP has a complicated shape and cannot be measured, a sample (a sample having a certain shape and size for measurement) may be cut out from the FRP and measured.

従来の真空吸引口に加え、注入口からマトリックス樹脂を吸引、排出することにより、マトリックス樹脂の排出時間を短縮することができるため好ましい。   In addition to the conventional vacuum suction port, suction and discharge of the matrix resin from the injection port is preferable because the discharge time of the matrix resin can be shortened.

また、真空吸引口からのみマトリックス樹脂を吸引、排出する場合、真空吸引口に近い箇所のプリフォーム内に含浸しているマトリックス樹脂を吸引しやすいが、注入口に近いプリフォーム内に含浸しているマトリックス樹脂は、吸引しにくいため、排出することが困難である。そのため、結果として、注入口に近い箇所のFRPの強化繊維体積率は、真空吸引口に近い箇所のFRPの強化繊維体積率に比べて、低くなる懸念がある。そのため、マトリックス樹脂をプリフォームに注入後、注入口からもマトリックス樹脂を吸引、排出することにより、FRPの各箇所における強化繊維体積率のばらつきを向上することができ、好ましい。   In addition, when the matrix resin is sucked and discharged only from the vacuum suction port, it is easy to suck the matrix resin impregnated in the preform near the vacuum suction port, but it is impregnated in the preform near the injection port. Since the matrix resin is difficult to suck, it is difficult to discharge. Therefore, as a result, there is a concern that the reinforcing fiber volume ratio of the FRP near the inlet is lower than the reinforcing fiber volume ratio of the FRP near the vacuum suction port. For this reason, after the matrix resin is injected into the preform, the matrix resin is sucked and discharged also from the injection port, so that the variation in the reinforcing fiber volume ratio in each part of the FRP can be improved.

本発明の強化繊維基材の製造方法は、強化繊維基材の少なくとも片側の表面にガラス転移温度Tgが0℃〜95℃である熱可塑性樹脂を含有する樹脂が、2g/m〜40g/mの範囲内で付着されている強化繊維基材積層体を製造することを特徴とするものである。
強化繊維基材積層体の製造方法は、少なくとも次の工程(A)から(F)を経て製造することを特徴とするものである。
(A)強化繊維基材を所定の形状に裁断する裁断工程。
(B)前記所定の形状に裁断された強化繊維基材を、所定の積層構成に基づいて、順次、平面上に搬送・配置する積層工程。
(C)(B)で得られた積層体を加熱工程へ間欠的に搬送する搬送工程。
(D)搬送された積層体を加熱する加熱工程。
(E)該積層体を、加圧治具の一定面積当たりに有する加圧部の面積割合が、高い領域を1〜10%有する加圧治具を用いて加圧し、強化繊維基材の表面に付着している前記熱可塑性樹脂を含有する樹脂により、加圧部の強化繊維基材同士を厚み方向に接着する加圧接着工程。
(F)該積層体を冷却する冷却工程。
In the method for producing a reinforcing fiber base of the present invention, a resin containing a thermoplastic resin having a glass transition temperature Tg of 0 ° C. to 95 ° C. on the surface of at least one side of the reinforcing fiber base is 2 g / m 2 to 40 g / The reinforcing fiber base laminate adhered within the range of m 2 is manufactured.
The method for producing a reinforcing fiber base laminate is characterized by producing at least the following steps (A) to (F).
(A) A cutting step of cutting the reinforcing fiber base into a predetermined shape.
(B) A laminating process in which the reinforcing fiber base material cut into the predetermined shape is sequentially transported and arranged on a plane based on a predetermined laminating configuration.
(C) The conveyance process which conveys the laminated body obtained by (B) intermittently to a heating process.
(D) The heating process which heats the conveyed laminated body.
(E) The surface of the reinforcing fiber substrate is pressed using a pressing jig having a region where the area ratio of the pressing part having a high area per fixed area of the pressing jig is 1 to 10%. A pressure bonding step in which the reinforcing fiber bases of the pressure portion are bonded in the thickness direction with the resin containing the thermoplastic resin adhering to the surface.
(F) A cooling step for cooling the laminate.

(A)で言うところの強化繊維基材の所定の形状とは、各層の積層角度に強化繊維基材1が繊維配向を有し、一定幅で連続長さを有する形状である。一定幅で連続長さを有する強化繊維基材積層体2を得ることにより、得られた強化繊維基材積層体2を紙管などに巻いて、効率よく保管することができ、後に適用する部材の幅が該強化繊維基材積層体の幅以内である場合、部材の形状に合わせて裁断することにより、あらゆる部材に適用することができるためである。   The predetermined shape of the reinforcing fiber base referred to in (A) is a shape in which the reinforcing fiber base 1 has fiber orientation at a lamination angle of each layer, and has a constant width and a continuous length. By obtaining the reinforcing fiber base laminate 2 having a constant width and a continuous length, the obtained reinforcing fiber base laminate 2 can be wound around a paper tube and efficiently stored, and a member to be applied later This is because, when the width is within the width of the reinforcing fiber base laminate, it can be applied to any member by cutting according to the shape of the member.

また(B)で言うところの所定の積層構成とは、該強化繊維基材積層体2を適用する各部材に共通の積層構成であることをいう。共通の積層構成の積層体を製造することにより、より多くの部材に強化繊維基材積層体2を使用することができる。   In addition, the predetermined laminated structure referred to in (B) means a laminated structure common to the respective members to which the reinforcing fiber base laminate 2 is applied. By manufacturing a laminate having a common laminate configuration, the reinforcing fiber base laminate 2 can be used for more members.

次に、図4により、本発明の製造装置の一形態を示し、製造方法を説明する。   Next, FIG. 4 shows an embodiment of the manufacturing apparatus of the present invention, and the manufacturing method will be described.

すなわち、図4では、例として、積層構成[45/0/−45/90](ここでSは鏡面対称を意味する)の強化繊維基材積層体2を作製する装置の一例を示す。 That is, in FIG. 4, as an example, an example of an apparatus for producing the reinforcing fiber base laminate 2 having a laminated configuration [45/0 / −45 / 90] s (where S means mirror symmetry) is shown.

(A)の裁断工程における強化繊維基材の裁断は、市販されている自動裁断機を用いることが可能である。   A commercially available automatic cutting machine can be used for cutting the reinforcing fiber base in the cutting step (A).

(B)の積層工程においては、裁断した強化繊維基材1を、ロボットアーム9を用いて、コンベア10の所定の位置に搬送、配置することが好ましい。ロボットアーム9の先端には、前記強化繊維基材1を保持できるハンド装置11が取り付けられている。ハンド装置11は、前記強化繊維基材1の品質を損なうことなく、搬送・配置することのできる機能を有していれば、特に限定されない。例えば、真空吸引装置やブロア装置をハンド装置につないで、吸引により前記強化繊維基材1を保持する方式や、ピンにより前記強化繊維基材1を引っかけて保持する方法、及びこれら二つの方法を組み合わせた方法などが適用可能である。   In the lamination step (B), it is preferable that the cut reinforcing fiber base material 1 is transported and arranged at a predetermined position of the conveyor 10 by using the robot arm 9. A hand device 11 that can hold the reinforcing fiber base 1 is attached to the tip of the robot arm 9. The hand apparatus 11 will not be specifically limited if it has the function which can be conveyed and arrange | positioned, without impairing the quality of the said reinforced fiber base material 1. FIG. For example, a method of holding the reinforcing fiber substrate 1 by suction by connecting a vacuum suction device or a blower device to a hand device, a method of hooking and holding the reinforcing fiber substrate 1 by a pin, and these two methods A combined method or the like is applicable.

特に真空吸引装置やブロア装置を用いたハンド装置11は、強化繊維基材をピンなどにより引っかけることもなく、強化繊維基材の品質を低下させる懸念がないため、好ましい。   In particular, the hand device 11 using a vacuum suction device or a blower device is preferable because the reinforcing fiber base material is not caught by a pin or the like, and there is no fear of reducing the quality of the reinforcing fiber base material.

自動裁断機13で裁断された積層角度45°の前記強化繊維基材14をコンベア10の所定の位置に配置した後、コンベア10を稼働させて進行方向に移動させ、先に配置した積層角度45°の前記強化繊維基材14の隣のスペースに同様に積層角度45°の強化繊維基材14を配置していく。その積層角度45°の強化繊維基材14の上に、積層構成に基づき、積層角度0°の強化繊維基材を配置する。0°の強化繊維基材は、裁断することなく、原料のロール12から直接配置、積層するのが好ましい。0°の強化繊維基材を積層した後、同様にコンベア10を稼働させて、45°/0°の強化繊維基材が積層された上に、自動裁断機17によって裁断された−45°の強化繊維基材18を搬送、積層する。以下、同様に自動裁断機15によって裁断された90°の強化繊維基材16、自動裁断機17によって裁断された−45°の強化繊維基材18、0°の強化繊維基材を積層構成に基づいて積層していく。
このように各層を構成する強化繊維基材を配置しては、コンベアで移動するという、間欠的な強化繊維基材の移動を行う。また、移動した先でさらにその上に積層される強化繊維基材を配置するため、ロボットアーム9はコンベア10の進行に伴い、同一の方向に移動することのできるスライダー19の上に設置され、それぞれの強化繊維基材をコンベア上の所定位置に搬送できることが好ましい。
After the reinforcing fiber base material 14 having a lamination angle of 45 ° cut by the automatic cutter 13 is disposed at a predetermined position of the conveyor 10, the conveyor 10 is operated and moved in the traveling direction, and the previously disposed lamination angle 45 is disposed. Similarly, the reinforcing fiber base material 14 having a lamination angle of 45 ° is arranged in a space adjacent to the reinforcing fiber base material 14. A reinforcing fiber substrate having a lamination angle of 0 ° is arranged on the reinforcing fiber substrate 14 having a lamination angle of 45 ° based on the lamination configuration. The 0 ° reinforcing fiber substrate is preferably arranged and laminated directly from the raw material roll 12 without cutting. After laminating the 0 ° reinforcing fiber base material, the conveyor 10 was operated in the same manner, and the 45 ° / 0 ° reinforcing fiber base material was laminated, and was cut by the automatic cutter 17 at −45 °. The reinforcing fiber substrate 18 is conveyed and laminated. Similarly, the 90 ° reinforcing fiber base material 16 cut by the automatic cutter 15, the −45 ° reinforcing fiber base material 18 cut by the automatic cutter 17, and the 0 ° reinforcing fiber base material are laminated. Laminate based on.
In this way, the reinforcing fiber base material constituting each layer is arranged, and the reinforcing fiber base material is moved intermittently, which is moved by a conveyor. Moreover, in order to arrange the reinforcing fiber base material to be further laminated on the moved destination, the robot arm 9 is installed on the slider 19 that can move in the same direction as the conveyor 10 advances, It is preferable that each reinforcing fiber substrate can be conveyed to a predetermined position on the conveyor.

すべての強化繊維基材を1台の自動裁断機により裁断しても構わないが、図5のように複数の自動裁断機を用いてそれぞれの積層角度の強化繊維基材を裁断することにより、裁断工程にかかる時間を短縮することができるため好ましい。   Although all the reinforcing fiber bases may be cut by a single automatic cutting machine, by cutting the reinforcing fiber bases of each lamination angle using a plurality of automatic cutting machines as shown in FIG. This is preferable because the time required for the cutting process can be shortened.

このように所定の積層構成に基づく強化繊維基材を、自動裁断機にて裁断、ロボットアームにて搬送・配置、コンベア10にて移動を繰り返すことにより、自動で且つ精度良く、連続的に強化繊維基材を積層することができるため、好ましい。かかる精度としては、強化繊維基材の配向角度は、±1°以内であることが好ましく、先に配置した強化繊維基材の隣に次の強化繊維基材を配置する場合の隙間は0〜1mmであることが好ましい。   In this way, the reinforcing fiber base based on a predetermined laminated configuration is automatically and accurately reinforced continuously by repeating cutting with an automatic cutting machine, transportation and placement with a robot arm, and movement with a conveyor 10. Since a fiber base material can be laminated | stacked, it is preferable. As such accuracy, the orientation angle of the reinforcing fiber base is preferably within ± 1 °, and the gap when the next reinforcing fiber base is placed next to the previously placed reinforcing fiber base is 0 to 0. It is preferably 1 mm.

(C)搬送工程においては、(B)の積層工程にて得られた積層体を(D)の加熱工程へ搬送する。図5においては、コンベア10上に配置されている所定の積層構成を有する強化繊維基材積層体2は、コンベア10を間欠的に進行方向に稼働させることにより、オーブン20の中に搬送される。所定の積層構成に積層された積層体は、まだ一体化されていないため、連続長さを有する積層体を、積層角度をずらすことなく持ち運ぶことは困難であり、したがって、コンベア上で強化繊維基材を積層した後、連続的にオーブンに搬送するのが好ましい。かかる手段を採用することにより、積層角度をずらすことなく、加熱工程及び加圧接着工程に移送することができる。   (C) In a conveyance process, the laminated body obtained at the lamination process of (B) is conveyed to the heating process of (D). In FIG. 5, the reinforcing fiber base laminate 2 having a predetermined laminated configuration arranged on the conveyor 10 is conveyed into the oven 20 by operating the conveyor 10 in the traveling direction intermittently. . Since the laminated bodies laminated in a predetermined laminated structure are not yet integrated, it is difficult to carry a laminated body having a continuous length without shifting the lamination angle. After laminating the materials, it is preferable to continuously convey the materials to an oven. By adopting such means, it is possible to transfer to the heating step and the pressure bonding step without shifting the stacking angle.

また、(E)の加圧接着工程での接着一体化の前に、コンベア上での移動により、積層角度がずれる懸念のある場合は、端部などをミシンなどにより仮縫いするなどして、仮止めすることも好ましい様態の一つである。仮縫いした場合には、後の加圧接着工程にて、積層体の全面にわたり所定の箇所を接着した後、仮縫いした端部を切り落として除去することにより、本発明の強化繊維基材積層体を得ることができる。   If there is a concern that the stacking angle may shift due to movement on the conveyor before the adhesive integration in the pressure bonding process of (E), temporarily sew the end part with a sewing machine, etc. Stopping is also one of the preferred modes. In the case of temporary stitching, after adhering a predetermined portion over the entire surface of the laminate in the subsequent pressure bonding step, the end portion of the temporary stitching is cut off and removed, whereby the reinforcing fiber base laminate of the present invention is removed. Obtainable.

(D)の加熱工程においては、(B)の積層工程にて得られた積層体を、後述する所定の温度において、加熱する。加熱装置としては、強化繊維基材に非接触で加熱することができるため熱風オーブンが好ましい。   In the heating step (D), the laminated body obtained in the laminating step (B) is heated at a predetermined temperature to be described later. As the heating device, a hot air oven is preferable because it can heat the reinforcing fiber base without contact.

図4に記載されているようなオーブン20を用いて、後の加圧接着工程(E)において、接着する範囲を選択的に加熱してもよい。このようなオーブン20を用いて、接着する範囲を選択的に加熱することにより、加熱効率が向上するだけでなく、加熱条件をコントロールしやすく、さらに加熱設備の小型化、コンベア10に併設することが容易などのメリットがあるため、好ましい。また、後述する加圧接着治具21に発熱機能を設ければ、オーブン20を用いなくてもよい。発熱機能のある加圧接着治具21で積層体を直接加熱することにより効率よく加熱することができる。加熱は積層体の加圧接着箇所全体において、均一に加熱されることが好ましい。特に、加圧接着する箇所の厚み方向に均一な温度に加熱する事が好ましい。厚み方向に均一な温度でないと、強化繊維基材1の表面に付着している樹脂8の加熱が均一にならず、厚み方向の接合力にばらつきが生じるため好ましくないのである。ここで均一とは、±5℃以内を意味する。より好ましくは±3℃以内である。測定方法は特に限定するものではないが、積層体の代表的な加熱箇所において、積層体の表層及び積層層間に熱電対を配置し、加熱処理を行い、積層体の過熱状況をモニターすることによって測定することができる。   In the subsequent pressure bonding step (E), the range to be bonded may be selectively heated using an oven 20 as described in FIG. By using such an oven 20 to selectively heat the area to be bonded, not only the heating efficiency is improved, it is easy to control the heating conditions, the heating equipment is downsized, and the conveyor 10 is attached. Is preferable because it has advantages such as ease. Moreover, if the heat generating function is provided in the pressure bonding jig 21 described later, the oven 20 may not be used. By directly heating the laminate with the pressure bonding jig 21 having a heat generating function, it can be efficiently heated. It is preferable that the heating is uniformly performed in the entire pressure bonding portion of the laminate. In particular, it is preferable to heat to a uniform temperature in the thickness direction of the part to be pressure bonded. If the temperature is not uniform in the thickness direction, the heating of the resin 8 adhering to the surface of the reinforcing fiber base 1 is not uniform, and the bonding force in the thickness direction varies, which is not preferable. Here, uniform means within ± 5 ° C. More preferably, it is within ± 3 ° C. The measuring method is not particularly limited, but by placing a thermocouple between the surface layer and the interlayer of the laminate at a representative heating location of the laminate, performing a heat treatment, and monitoring the overheating state of the laminate. Can be measured.

また加熱する際の所定の温度は、強化繊維基材1の表面に付着している樹脂のガラス転移温度Tgよりも高い温度であることが好ましい。加熱温度を該樹脂のガラス転移温度よりも高くすることにより、樹脂8が軟化するため、(F)の加圧接着工程において、より低圧でより確実に接着することができるため好ましい。より好ましくは、ガラス転移温度Tg+5〜20℃である。   Moreover, it is preferable that the predetermined temperature at the time of heating is higher than the glass transition temperature Tg of the resin adhering to the surface of the reinforcing fiber substrate 1. By making the heating temperature higher than the glass transition temperature of the resin, the resin 8 is softened. Therefore, in the pressure bonding step (F), it is possible to bond more reliably at a lower pressure, which is preferable. More preferably, it is glass transition temperature Tg + 5-20 degreeC.

加圧接着工程(E)においては、加圧治具の一定面積当たりに有する加圧部の面積割合が高い領域を1〜10%有する加圧治具を用いて加圧し、強化繊維基材の表面に付着している前記熱可塑性樹脂を含有する樹脂8により、加圧部の強化繊維基材同士を厚み方向に接着させる必要がある。加圧部の面積割合が高い領域として、基材の剥離しやすい箇所に相当するところが好ましく、例えば強化繊維基材の端部領域や基材と基材との継ぎ合わせ部7や後のプリフォーム工程における形状カット箇所に相当する箇所などを挙げることができる。   In the pressure bonding step (E), pressurization is performed using a pressure jig having 1 to 10% of a region having a high area ratio of the pressure part per fixed area of the pressure jig, It is necessary to adhere the reinforcing fiber bases of the pressurizing part in the thickness direction with the resin 8 containing the thermoplastic resin adhering to the surface. As the area where the area ratio of the pressurizing part is high, the part corresponding to the part where the base material is easily peeled is preferable. The part etc. which correspond to the shape cut part in a process can be mentioned.

ここでは、図5を用いて、基材の端部領域を加圧する加圧治具部の面積割合が高い加圧治具の圧着工程の一例を示す。すなわち、図5は、図4で示したオーブン20内に設置されている加圧接着治具21および強化繊維基材積層体2、コンベア10の一断面を示す。   Here, FIG. 5 is used to show an example of a pressure bonding process of a pressure jig having a high area ratio of the pressure jig part that pressurizes the end region of the base material. That is, FIG. 5 shows a cross section of the pressure bonding jig 21, the reinforcing fiber base laminate 2, and the conveyor 10 installed in the oven 20 shown in FIG. 4.

コンベア10上の強化繊維基材積層体2は、コンベア10を稼働させることにより、オーブン内に設置されている加圧接着治具21に搬送される。加圧接着治具21は、接着治具上22と接着治具下23から構成され、加圧接着治具上22は、例えば凸形状の独立した加圧部を有している。加圧部の面積は、強化繊維基材積層体の端部からの幅W(1〜5cm)である端部領域を加圧する加圧治具の一定面積当たりの加圧部の面積割合が、前記端部領域以外を加圧する加圧治具の一定面積あたりの加圧部の面積割合に対して、1.5〜5倍以上であることが好ましい。加圧部24の断面形状は強化繊維基材を傷つけないものが好ましく、球状もしくは角を面取りした矩形状のものが好ましい。加圧部の面積は、あまり大きくし過ぎると層間の自由度が小さくなり皺を防止するような層間のすべりが生じにくくなり、また圧着部の面積を小さくし過ぎると所望の接合力を得るために加圧部を増やす必要があることから、1〜100mmが好ましく、1〜50mmであればより好ましい。 また、加圧接着治具21は金属製で発熱機能を有することが好ましい。発熱方法は特に限定するものではないが、加圧接着治具21内に電熱ヒーターもしくは温水もしくは温油ラインを併設するなどの方法が挙げられる。加圧接着治具21を金属製にすることにより、上記発熱方法もしくはオーブン20による昇温効率を向上することができるため好ましい。
また加圧部24は、メンテナンス、加圧条件の変更などの調整をするなどの観点から取り外し可能とすることが好ましい。
The reinforcing fiber base laminate 2 on the conveyor 10 is transported to the pressure bonding jig 21 installed in the oven by operating the conveyor 10. The pressure bonding jig 21 includes an upper bonding jig 22 and a lower bonding jig 23, and the pressure bonding jig upper 22 has, for example, a convex independent pressure portion. The area of the pressing part is the area ratio of the pressing part per fixed area of the pressing jig that pressurizes the end region that is the width W (1 to 5 cm) from the end of the reinforcing fiber base laminate. It is preferable that it is 1.5-5 times or more with respect to the area ratio of the pressurization part per fixed area of the pressurization jig which pressurizes other than the said edge part area | region. The cross-sectional shape of the pressure unit 24 is preferably one that does not damage the reinforcing fiber substrate, and is preferably spherical or a rectangular shape with chamfered corners. If the area of the pressurizing part is too large, the degree of freedom between the layers will be reduced and it will be difficult for slippage between layers to prevent wrinkles. If the area of the crimping part is too small, the desired bonding strength will be obtained. 1 to 100 mm 2 is preferable, and 1 to 50 mm 2 is more preferable. The pressure bonding jig 21 is preferably made of metal and has a heat generating function. The heating method is not particularly limited, and examples thereof include a method in which an electric heater, hot water, or hot oil line is provided in the pressure bonding jig 21. It is preferable to make the pressure bonding jig 21 made of metal since the heating method or the temperature rising efficiency by the oven 20 can be improved.
Moreover, it is preferable that the pressurization part 24 can be removed from a viewpoint, such as adjusting maintenance, a change of pressurization conditions, etc.

(F)冷却工程においては、(D)加熱工程、(E)加圧接着工程にて加熱された各強化繊維基材を接着している接着樹脂を冷却することにより、接着を完了させる。図5においては、オーブン20と巻き取り用のロール25の間に、強化繊維基材積層体を室温にて冷却する冷却用スペース26を設けることにより、室温にて冷却して、接着を完了させた後、巻き取り用のロール25にて巻き取る工程となっている。巻き取り用のロール25は強化繊維基材積層体を巻き取れるものであれば特に限定されるものではなく、適切な径を有する紙管などを用いることができるが、直径が50〜150cmであれば好ましい。また、必要に応じて強化繊維基材積層体を巻き取る前に、積層体の端部を、ミシンなどを用いて縫うことにより、巻き取り時の変形により、強化繊維基材積層体がばらけることを抑制することができる。この場合、必要に応じて縫った端部を取り除くことにより、強化繊維基材積層体は所定の賦形性能を発現させることができる。   (F) In the cooling step, (D) heating step and (E) the adhesive resin bonding the reinforcing fiber substrates heated in the pressure bonding step is cooled to complete the bonding. In FIG. 5, by providing a cooling space 26 for cooling the reinforcing fiber base laminate at room temperature between the oven 20 and the winding roll 25, cooling is performed at room temperature to complete the bonding. After that, it is a step of winding with a roll 25 for winding. The roll 25 for winding is not particularly limited as long as it can wind up the reinforcing fiber base laminate, and a paper tube having an appropriate diameter can be used, but if the diameter is 50 to 150 cm. It is preferable. In addition, before winding up the reinforcing fiber base laminate as necessary, the reinforcing fiber base laminate is separated by deformation during winding by sewing the end of the laminate using a sewing machine or the like. This can be suppressed. In this case, the reinforcing fiber base laminate can exhibit a predetermined shaping performance by removing the sewn end as necessary.

また、接着が完了した積層体を巻き取らずに、一定幅のスリット状やプリフォームで使用するカット形状などに裁断し、ストック棚などに保管してもよい。これら(A)〜(F)の各工程を、コンベア10を用いて、連続で行うことにより、連続長さを有する強化繊維基材積層体を製造することができるため好ましい。   Further, without winding up the laminated body that has been bonded, it may be cut into a slit shape having a certain width or a cut shape used in a preform and stored in a stock shelf or the like. These steps (A) to (F) are preferably performed continuously by using the conveyor 10 because a reinforced fiber base material laminate having a continuous length can be produced.

以下、実施例を用いて本発明をさらに詳細に説明する。なお、本発明が実施例に記載の発明に限定されるものではない。また、各パラメータの値は、下記する方法により求めたものである。   Hereinafter, the present invention will be described in more detail with reference to examples. In addition, this invention is not limited to the invention as described in an Example. In addition, the value of each parameter is obtained by the following method.

(1)積層層間の接合力
本文中に記載した方法により求めた。
(1) Bonding force between laminated layers Determined by the method described in the text.

(2)高接合領域の積層層間における割合
長さ方向に端部から少なくとも10mm以上の距離を有し、幅方向にもっとも多くの試験片を切り出せる箇所において、強化繊維基材積層体2から幅方向にわたり、幅50mm、長さ150mmの試験片を等間隔に切り出し、本文中に記載した測定方法に基づき、幅方向の接合力の分布を求めた。試験片の数を10個以上作成できない幅であった場合は、試験片の数が10個となる大きさの試験片(長さは幅の3倍とする)を作成した。その後、強化繊維基材積層体2の面積を、これらの試験片を用いて上記測定方法に基づき測定した接合力が500〜1000N/mの試験片(高接合領域5)の数、およびその試験片に含まれる接合部4の分布する密度(すなわち、単位面積あたりに対する接合部の面積または数)を求めた。最後に、高接合領域の積層層間における割合を接合力が500〜1000N/mの試験片(高接合領域5)の数を、試験片の総数で除して求めた。
(2) Ratio between the laminated layers of the high-bonding region The width from the reinforcing fiber base laminate 2 is a portion having a distance of at least 10 mm from the end in the length direction and the largest number of test pieces in the width direction. A test piece having a width of 50 mm and a length of 150 mm was cut out at equal intervals in the direction, and the distribution of bonding force in the width direction was determined based on the measurement method described in the text. When the width was such that ten or more test pieces could not be produced, a test piece having a size that would result in ten test pieces (the length was three times the width) was produced. Then, the number of test pieces (high bonding region 5) having a bonding force of 500 to 1000 N / m 2 measured based on the measurement method using these test pieces and the area of the reinforcing fiber substrate laminate 2, The density of the joints 4 included in the test piece (that is, the area or number of joints per unit area) was determined. Finally, the ratio between the laminated layers in the high bonding area was determined by dividing the number of test pieces (high bonding area 5) having a bonding force of 500 to 1000 N / m 2 by the total number of test pieces.

(3)樹脂のガラス転移温度
本文中に記載した方法により求めた。
(3) Glass transition temperature of resin Obtained by the method described in the text.

(4)樹脂の付着量
樹脂の付着量を以下のように測定した。まず、強化繊維基材積層体2から強化繊維基材を少なくとも1ply取り出し、該基材を125×125mmに裁断する。切り出したサンプル基材の重量を電子天秤で0.1g単位まで測定し、基材総目付W(g/m)=W0(g)/(0.125×0.125(m))を求めた。
(4) Amount of resin adhesion The amount of resin adhesion was measured as follows. First, at least 1 ply of the reinforcing fiber base material is taken out from the reinforcing fiber base material laminate 2, and the base material is cut into 125 × 125 mm. The weight of the cut-out sample base material is measured to the 0.1 g unit with an electronic balance, and the base material total weight W (g / m 2 ) = W 0 (g) / (0.125 × 0.125 (m 2 )) is obtained. Asked.

次に該サンプル基材を、塩化メチレンを入れた容器に入れ、塩化メチレンに浸漬し、基材に付着している接着樹脂を溶解、除去した。接着樹脂を溶解・除去した後、基材を乾燥機の中で110℃±5℃にて1時間乾燥し、デシケータ内で室温まで冷却した。冷却した基材を電子天秤にて、重量W1(g)を0.1g単位まで測定し、基材目付F(g/m)=W1(g)/(0.125×0.125(m))として求めた。最後に樹脂の付着量を、樹脂の付着量(g/m)=基材総目付W(g/m)−基材目付F(g/m)として求めた。 Next, the sample substrate was placed in a container containing methylene chloride and immersed in methylene chloride to dissolve and remove the adhesive resin adhering to the substrate. After dissolving and removing the adhesive resin, the substrate was dried in a dryer at 110 ° C. ± 5 ° C. for 1 hour and cooled to room temperature in a desiccator. The cooled substrate was measured with an electronic balance, and the weight W1 (g) was measured to a unit of 0.1 g, and the substrate weight per unit area F (g / m 2 ) = W1 (g) / (0.125 × 0.125 (m 2 )). Finally, the resin adhesion amount was determined as resin adhesion amount (g / m 2 ) = base material total weight W (g / m 2 ) −base material weight F (g / m 2 ).

(5)プリフォームの強化繊維体積率Vpf
試料サイズは300×300mmとし、各実施例に記載のようにプリフォームを作製して、下記のようにプリフォームの強化繊維体積率Vpfを求めた。
(5) Preform reinforcing fiber volume fraction Vpf
The sample size was 300 × 300 mm, a preform was prepared as described in each example, and the reinforcing fiber volume fraction Vpf of the preform was determined as follows.

強化繊維の密度ρ(g/cm)は、基材に使用している強化繊維糸条の密度であり、JIS R 7603(1999)のA法に準拠して測定したものである。 The density ρ (g / cm 3 ) of the reinforcing fiber is the density of the reinforcing fiber yarn used for the base material, and is measured in accordance with the method A of JIS R 7603 (1999).

プリフォームの厚みt(mm)は、プリフォームを賦形型に配置し、バッグフィルムで密閉して、密閉空間を真空吸引し、プリフォームに大気圧をかけた状態にて、ハイトゲージおよびマイクロメーターを用いて、プリフォームの中心および4隅の厚み計5カ所を0.01mm単位まで測定した。プリフォームの中心の厚みは、上記のプリフォームに大気圧をかけた状態にて、バッグフィルムの上から、プリフォームの中心位置の高さを測定し、予め測定しておいた賦形型の高さおよびバッグフィルムの厚みを差し引くことにより測定した。プリフォームの4隅の厚みは、上記のプリフォームに大気圧をかけた状態にて、マイクロメーターにて、賦形型、プリフォーム、バッグフィルムを合わせた厚みを測定し、予め測定しておいた賦形型の厚みおよびバッグフィルムの厚みを差し引くことにより、測定した。   The thickness t (mm) of the preform is determined by placing the preform in a shaping mold, sealing it with a bag film, vacuuming the sealed space, and applying atmospheric pressure to the preform. Was used to measure 5 thickness gauges at the center and 4 corners of the preform up to 0.01 mm. The thickness of the center of the preform is measured by measuring the height of the center position of the preform from the top of the bag film with atmospheric pressure applied to the above preform. Measured by subtracting height and bag film thickness. The thickness of the four corners of the preform is measured in advance by measuring the combined thickness of the shaping mold, the preform, and the bag film with a micrometer in a state where atmospheric pressure is applied to the preform. It was measured by subtracting the thickness of the shaped mold and the thickness of the bag film.

プリフォームの強化繊維体積率Vpfは、上記方法により測定した基材目付F(g/m)、基材の積層枚数p(枚)、強化繊維の密度ρ(g/cm)、プリフォームの厚みt(mm)を用いて、プリフォームの厚みを測定した5個所のVpfをVpf=F×p/ρ/t/10(%)として求め、5カ所の平均値をプリフォームの強化繊維体積率Vpfとして求めた。 Reinforcing fiber volume fraction Vpf of the preform is the base material weight F (g / m 2 ), the number of laminated base materials p (sheet), the density of reinforcing fibers ρ (g / cm 3 ) Using the thickness t (mm) of the preform, the Vpf at which the thickness of the preform was measured was determined as Vpf = F × p / ρ / t / 10 (%), and the average value at the five locations was determined as the reinforcing fiber of the preform. It calculated | required as volume ratio Vpf.

(6)FRPの強化繊維体積率Vf
実施例に記載のようにFRPを作製して、下記のようにFRPの強化繊維体積率Vfを求めた。基材目付Fおよび強化繊維の密度ρは上記と同様である。
(6) Reinforced fiber volume fraction Vf of FRP
FRP was produced as described in the Examples, and the reinforcing fiber volume fraction Vf of FRP was determined as follows. The base weight F and the density ρ of the reinforcing fibers are the same as described above.

FRPの厚みt(mm)は、FRPを成形型から脱型した後、マイクロメーターを用いて、エポキシ樹脂の注入口および真空吸引工の周辺および注入口と真空吸引口間の中央の3カ所の厚みを0.01mm単位まで測定した。   After removing the FRP from the mold, the thickness t (mm) of the FRP was measured at three locations around the epoxy resin injection port and the vacuum suction work center and between the injection port and the vacuum suction port using a micrometer. The thickness was measured up to 0.01 mm.

FRPの強化繊維体積率Vfは、上記方法により測定した基材目付F(g/m)、基材の積層枚数p(枚)、強化繊維の密度ρ(g/cm)、FRPの厚みt(mm)を用いて、Vf=F×p/ρ/t/10 (%)として求めた。 The reinforcing fiber volume fraction Vf of the FRP is the base material weight F (g / m 2 ), the number of laminated base materials p (sheets), the density ρ (g / cm 3 ) of the reinforcing fibers, and the thickness of the FRP measured by the above method. Using t (mm), Vf = F × p / ρ / t / 10 (%).

(実施例1)
以下に、強化繊維基材積層体2を使ってプリフォームを作成する場合の実施例を説明する。
Example 1
Below, the Example in the case of producing a preform using the reinforcing fiber base laminate 2 will be described.

まず、引張り強さが5800MPa、引張弾性率が290GPaのフィラメント数が24000本の炭素繊維を用いて、炭素繊維目付200g/mの基材を製織した。次にこの基材の上面に平均径が120μmでガラス転移温度が70℃の熱可塑性樹脂を含む粒子を接着樹脂として、27g/mを均一に散布し、200℃に加熱することによって基材の表面に付着させ強化繊維基材1を作製した。 First, a base material having a carbon fiber basis weight of 200 g / m 2 was woven using carbon fibers having a tensile strength of 5800 MPa and a tensile modulus of 290 GPa and a filament number of 24,000. Next, 27 g / m 2 is uniformly sprayed on the upper surface of the base material, containing thermoplastic resin having an average diameter of 120 μm and a glass transition temperature of 70 ° C. as an adhesive resin, and heated to 200 ° C. A reinforcing fiber substrate 1 was prepared by adhering to the surface.

この強化繊維基材1を45°方向、0°方向、−45°方向、90°方向の繊維方向の角度を有する、幅1m、長さ1mの強化繊維基材1に裁断して、45°方向、0°方向、−45°方向、90°方向、90°方向、−45°方向、0°方向、45°方向に順次積層し、積層体を準備した。この積層体をアルミ合金製の平板の上に配置して、雰囲気温度が85℃のオーブンの中に入れて加熱した。また高接合領域5として基材の端部から5cmの領域を端部領域に設定した。   The reinforcing fiber substrate 1 is cut into a reinforcing fiber substrate 1 having a width of 1 m and a length of 1 m having a fiber direction angle of 45 ° direction, 0 ° direction, −45 ° direction and 90 ° direction. Direction, 0 ° direction, −45 ° direction, 90 ° direction, 90 ° direction, −45 ° direction, 0 ° direction, and 45 ° direction were sequentially laminated to prepare a laminate. This laminate was placed on a flat plate made of aluminum alloy and heated in an oven having an ambient temperature of 85 ° C. Moreover, the area | region 5 cm from the edge part of the base material was set to the edge part area | region as the high joining area | region 5. FIG.

積層体を十分に加熱した後、図5に示すように1つの加圧部24の断面積が1mmでありかつ、高接合領域5を加圧する加圧部24のピッチは幅方向・長さ方向とも5mmで、低接合領域6を加圧する加圧部24のピッチは幅方向・長さ方向とも20mmである加圧接着治具21を積層体の上に配置して、さらに加圧接着治具21の上に1本の加圧部24にかかる圧力が0.1MPaになるように10分間積層体を加圧し、強化繊維基材1の表面の接着樹脂により強化繊維基材1同士を、厚み方向にわたり部分的に接合した。その後積層体をオーブンから取り出し室温にて放置・冷却して、強化繊維基材の積層体を得た。ここで該積層体の高接合領域5(端部領域)から幅5cm、長さ15cmの試験片を切り出し、接合力を測定したところ、550N/mであった。 After sufficiently heating the laminate, as shown in FIG. 5, the cross-sectional area of one pressing portion 24 is 1 mm 2 , and the pitch of the pressing portions 24 that pressurize the high bonding area 5 is the width direction / length. A pressure bonding jig 21 having a pressure of 5 mm in both directions and a pressure of the pressure members 24 for pressing the low bonding area 6 in the width direction and the length direction of 20 mm is arranged on the laminate, and further pressure bonding treatment is performed. Pressurize the laminate for 10 minutes so that the pressure applied to one pressing part 24 on the tool 21 is 0.1 MPa, and bond the reinforcing fiber bases 1 to each other with the adhesive resin on the surface of the reinforcing fiber base 1. It joined partially over the thickness direction. Thereafter, the laminate was taken out of the oven and left to cool at room temperature to obtain a laminate of reinforcing fiber substrates. Here, a test piece having a width of 5 cm and a length of 15 cm was cut out from the high bonding region 5 (end region) of the laminate, and the bonding force was measured. As a result, it was 550 N / m 2 .

次に、該積層体から幅方向に150mm、長さ方向に1000mmとなるような積層体を切り出し、該積層体をC型の賦形型(幅100mm×長さ800mm×高さ60mm、コーナーR5mm、長手方向の断面:C型)の上に配置し、バギングフィルムにて賦形型とバギングフィルムによって形成されている空間を真空ポンプにて真空吸引して、積層体を賦形型に加圧して賦形した。   Next, a laminate having a width of 150 mm and a length of 1000 mm is cut out from the laminate, and the laminate is cut into a C-shaped shaping die (width 100 mm × length 800 mm × height 60 mm, corner R5 mm). , Longitudinal section: C type), vacuuming the space formed by the bagging film with the shaping mold and the bagging film with a vacuum pump, and pressurizing the laminate to the shaping mold And shaped.

積層体を賦形型に加圧した状態でオーブン内に入れ、温度80℃にて2時間の加熱をすることにより、積層体の強化繊維基材間を接合させた後、オーブンから取り出し、室温にて冷却しC型プリフォームを作製したところ、皺のないプリフォームが得られた。プリフォームの強化繊維体積率Vpfを測定したところ、Vpfは53%であった。   The laminated body is put into an oven in a state where it is pressed into a shaping mold, and heated at a temperature of 80 ° C. for 2 hours to join the reinforcing fiber bases of the laminated body, and then removed from the oven at room temperature. When a C-shaped preform was produced by cooling at a temperature, a wrinkle-free preform was obtained. When the reinforcing fiber volume fraction Vpf of the preform was measured, the Vpf was 53%.

(実施例2)
実施例1で作製したプリフォームを成形型に配置して、エポキシ樹脂を注入し、真空バッグ成形を行った。
エポキシ樹脂の注入は、エポキシ樹脂がプリフォーム全体に含浸するまで行い、真空吸引口からエポキシ樹脂が排出された後、注入口を閉じて、エポキシ樹脂の注入を中止した。注入口に真空吸引ラインを繋いで、元の真空吸引口と共に、真空吸引を行い、余分に注入しているエポキシ樹脂の排出を行った。
(Example 2)
The preform produced in Example 1 was placed in a mold, an epoxy resin was injected, and vacuum bag molding was performed.
The injection of the epoxy resin was performed until the entire epoxy resin was impregnated with the epoxy resin. After the epoxy resin was discharged from the vacuum suction port, the injection port was closed and the injection of the epoxy resin was stopped. A vacuum suction line was connected to the inlet, and vacuum suction was performed together with the original vacuum suction port, and the epoxy resin that had been injected in excess was discharged.

元の真空吸引口と注入口を新たに真空吸引ラインに繋いで準備した真空吸引口からのエポキシ樹脂の排出は、エポキシ樹脂が含浸されたプリフォームの厚みを測定し、成形後の強化繊維体積率Vfが55%に相当する厚みになるまで行った。エポキシ樹脂が含浸されたプリフォームの厚みの測定は、注入口と真空吸引口の周辺および注入口と真空吸引口間の中央の3カ所を測定した。   The discharge of the epoxy resin from the vacuum suction port prepared by connecting the original vacuum suction port and the injection port to the new vacuum suction line is performed by measuring the thickness of the preform impregnated with the epoxy resin, and the reinforcing fiber volume after molding. The process was performed until the rate Vf reached a thickness corresponding to 55%. The thickness of the preform impregnated with the epoxy resin was measured at three locations around the injection port and the vacuum suction port and at the center between the injection port and the vacuum suction port.

エポキシ樹脂を排出した後、プリフォームに含浸したエポキシ樹脂を、温度130℃、2時間にて一次硬化させ、引き続き温度180℃、2時間にて二次硬化させて、真空バッグ成形を行った。
得られたFRPの強化繊維体積率Vfを測定したところ、Vfは56%であった。また該FRPの表面外観を観察した結果、顕著な皺や繊維の蛇行などは認められず、良好な表面品位を有していた。
After discharging the epoxy resin, the epoxy resin impregnated in the preform was primarily cured at a temperature of 130 ° C. for 2 hours, and then secondarily cured at a temperature of 180 ° C. for 2 hours to form a vacuum bag.
When the reinforcing fiber volume fraction Vf of the obtained FRP was measured, Vf was 56%. Further, as a result of observing the surface appearance of the FRP, no remarkable wrinkles or fiber meandering was observed, and the surface quality was excellent.

(比較例1)
端部領域を加圧する加圧部のピッチが20mmである接合治具で加圧する以外は実施例1と同様にして、強化繊維基材の積層体を得た。ここで該積層体の端部領域から幅5cm、長さ15cmの試験片を切り出し、接合力を測定したところ、300N/mであった
該積層体から幅方向に150mm、長さ方向に1000mmとなるように切り出し、C型の賦形型の上に配置したところ、基材の端部が剥がれてしまい、作業性が悪かった。
(Comparative Example 1)
A laminated body of reinforced fiber base materials was obtained in the same manner as in Example 1 except that the pressure was applied with a joining jig in which the pitch of the pressure parts for pressing the end region was 20 mm. Here, a test piece having a width of 5 cm and a length of 15 cm was cut out from the end region of the laminated body, and the bonding force was measured. As a result, it was 300 N / m 2 From the laminated body, 150 mm in the width direction and 1000 mm in the length direction. When it was cut out and placed on a C-shaped shaping mold, the end of the substrate was peeled off, and workability was poor.

(比較例2)
端部領域を加圧する条件を、加熱温度を95℃、加圧時間を15分とした以外は実施例1と同様にして、強化繊維基材の積層体を得た。ここで該積層体の端部領域から幅5cm、長さ15cmの試験片を切り出し、接合力を測定したところ、1200N/mであった
該積層体から幅方向に150mm、長さ方向に1000mmとなるように切り出し、C型のプリフォームを作製したところ、皺のあるC型のプリフォームとなった。
(Comparative Example 2)
A laminated body of reinforcing fiber substrates was obtained in the same manner as in Example 1 except that the heating conditions were 95 ° C. and the pressing time was 15 minutes. Here, a test piece having a width of 5 cm and a length of 15 cm was cut out from the end region of the laminated body, and the bonding force was measured. As a result, it was 1200 N / m 2 From the laminated body, 150 mm in the width direction and 1000 mm in the length direction. When a C-shaped preform was produced, a C-shaped preform with wrinkles was obtained.

(実施例3)
実施例1の強化繊維基材1を用いて、強化繊維基材積層体(8ply[45/0/−45/90]s、幅500mm×長さ5000mm)を作成する。
(Example 3)
A reinforcing fiber substrate laminate (8ply [45/0 / −45 / 90] s, width 500 mm × length 5000 mm) is prepared using the reinforcing fiber substrate 1 of Example 1.

(A)裁断工程において、45°方向、90°方向、−45°方向の基材を自動裁断機で裁断し、(B)の積層工程において、裁断した基材1を、ロボットアームを用いてコンベア10の所定の位置に搬送、配置した。0°基材は原料のロール9から直接配置、積層し、上記積層体(8ply[45/0/−45/90]s、幅500mm×長さ5000mm)を作成した。   (A) In the cutting step, the base material in the 45 ° direction, 90 ° direction, and −45 ° direction is cut with an automatic cutting machine. In the (B) lamination step, the cut base material 1 is cut using a robot arm. It was conveyed and arranged at a predetermined position on the conveyor 10. The 0 ° base material was directly arranged and laminated from the raw material roll 9 to prepare the above laminate (8ply [45/0 / −45 / 90] s, width 500 mm × length 5000 mm).

(C)搬送工程において、該積層体をコンベアで加熱工程へ搬送した。(D)の加熱工程では、オーブンを使用せずに温水による発熱機能を有する加圧接着治具21を70±5℃に加熱し、該積層体を直接加熱した。積層体を上下の接着治具で直接加熱することにより効率よく積層体を加熱することができた。   (C) In the transport process, the laminate was transported to the heating process by a conveyor. In the heating step (D), the pressure bonding jig 21 having a function of generating heat with hot water was heated to 70 ± 5 ° C. without using an oven, and the laminate was directly heated. The laminate was efficiently heated by directly heating the laminate with the upper and lower bonding jigs.

(E)加圧接着工程において、図7に示すように幅方向の中心部50mmを高接合領域とし、該領域に相当する加圧部24の断面積を400mm、断面形状を20mm角の矩形状にし、ピッチを幅方向・長さ方向ともに30mmとした。また低接合領域に相当する加圧部24は断面積を4mm、形状を2mm角の矩形状にし、ピッチを幅方向10mm、長さ方向40mmとした。 (E) In the pressure bonding step, as shown in FIG. 7, the central portion 50 mm in the width direction is set as a high bonding region, the cross-sectional area of the pressure portion 24 corresponding to the region is 400 mm 2 , and the cross-sectional shape is a 20 mm square rectangle. The shape was set, and the pitch was set to 30 mm in both the width direction and the length direction. Further, the pressurizing unit 24 corresponding to the low bonding region has a cross-sectional area of 4 mm 2 , a 2 mm square shape, and a pitch of 10 mm in the width direction and 40 mm in the length direction.

一本の加圧部24の圧力が0.05MPaになるように積層体を5分間加圧し、強化繊維基材1の表面の接着樹脂により強化繊維基材1同士を、厚み方向にわたり部分的に接合した。
その後該積層体を室温にて放置・冷却し、強化繊維基材の積層体2を得た。ここで該積層体の高接合領域5の割合を求めるために、該積層体から幅50mm、長さ150mmの試験片を10個切り出し、接合力を測定したところ、中心部に相当する高接合領域の接合力は900N/mで、その他9個の接合力は500N/m未満であった(高接合領域の積層層間における割合は10%)。
The laminated body is pressurized for 5 minutes so that the pressure of one pressing part 24 is 0.05 MPa, and the reinforcing fiber bases 1 are partially bonded across the thickness direction by the adhesive resin on the surface of the reinforcing fiber base 1. Joined.
Thereafter, the laminate was allowed to stand at room temperature and cooled to obtain a laminate 2 of reinforcing fiber substrate. Here, in order to obtain the ratio of the high bonding area 5 of the laminate, ten test pieces having a width of 50 mm and a length of 150 mm were cut out from the laminate and the bonding force was measured. As a result, the high bonding area corresponding to the center portion was obtained. The bonding force of 900 was N / m 2 , and the other nine bonding forces were less than 500 N / m 2 (the ratio of the high bonding region between the laminated layers was 10%).

次に該積層体2から幅500mm、長さ600mmとなる積層体を8枚切り出し、該積層体8枚をC型の賦形型(幅300mm×長さ700mm×高さ150mm、コーナーR10mm、長手方向の断面:C型、長手方向の曲率半径2000mm)の上に積層し、ラバーシートで賦形型とラバーシートで形成される空間を真空ポンプにて真空吸引して、積層体を賦形型に加圧して賦形した。   Next, eight laminates having a width of 500 mm and a length of 600 mm are cut out from the laminate 2, and the eight laminates are formed into a C-shaped shaping die (width 300 mm × length 700 mm × height 150 mm, corner R10 mm, longitudinal Cross section in the direction: C type, longitudinal radius of curvature 2000 mm), and the space formed by the rubber sheet and the rubber sheet is vacuumed by a vacuum pump to form the laminate. Pressurized to form.

次に、該積層体を賦形型に加圧した状態でオーブン内に入れ、温度90℃にて積層体を3時間加熱することにより積層体間を接合させた後、オーブンから取り出し、室温にて冷却しC型プリフォームを作製したところ、皺や繊維の配向のずれのない高品質なプリフォームが得られた。   Next, the laminate is put in an oven in a state where it is pressed into a shaping mold, and the laminate is heated at a temperature of 90 ° C. for 3 hours to join the laminates, then taken out of the oven and brought to room temperature. As a result, a C-type preform was produced, and a high-quality preform with no deviation in wrinkles and fiber orientation was obtained.

本発明の強化繊維基材積層体の一例を示す斜視図である。It is a perspective view which shows an example of the reinforced fiber base material laminated body of this invention. 本発明の強化繊維基材積層体における高接合領域の一例を示す斜視図である。It is a perspective view which shows an example of the high joining area | region in the reinforced fiber base material laminated body of this invention. 本発明の強化繊維基材積層体の一例を示す断面図である。It is sectional drawing which shows an example of the reinforced fiber base material laminated body of this invention. 本発明の強化繊維基材積層体の製造方法を示す概略図である。It is the schematic which shows the manufacturing method of the reinforced fiber base-material laminated body of this invention. 本発明の製造方法における加圧接着工程を示す概略断面図である。It is a schematic sectional drawing which shows the pressure bonding process in the manufacturing method of this invention. 本発明における接合力測定法を説明する概略断面図である。It is a schematic sectional drawing explaining the joining force measuring method in this invention. 本発明の製造方法における加圧接着工程を示す概略断面図である。It is a schematic sectional drawing which shows the pressure bonding process in the manufacturing method of this invention. 本発明の強化繊維基材積層体の高接合領域と低接合領域を見分ける方法の説明に用いられる図である。It is a figure used for description of the method of distinguishing the high joining area | region and low joining area | region of the reinforced fiber base material laminated body of this invention.

符号の説明Explanation of symbols

1 強化繊維基材
2 強化繊維基材積層体
3 層間
4 接合部
5 高接合領域
6 低接合領域
7 継ぎ合わせ部
8 樹脂
9 ロボットアーム
10 コンベア
11 ハンド装置
12 ロール
13 45°の強化繊維基材の裁断用自動裁断機
14 45°の強化繊維基材
15 90°の強化繊維基材の裁断用自動裁断機
16 90°の強化繊維基材
17 −45°の強化繊維基材の裁断用自動裁断機
18 −45°の強化繊維基材
19 スライダー
20 オーブン
21 加圧接着治具
22 接着治具上
23 接着治具下
24 加圧部
25 巻き取り用のロール
26 冷却用スペース
27 SUS板
28 両面テープ
29 試験体
30 台座
31 取り付け治具
32 長手方向
33 幅方向
34 試験片
DESCRIPTION OF SYMBOLS 1 Reinforcement fiber base material 2 Reinforcement fiber base material laminated body 3 Interlayer 4 Joint part 5 High joint area 6 Low joint area 7 Joint part 8 Resin 9 Robot arm 10 Conveyor 11 Hand apparatus 12 Roll 13 45 degree reinforcement fiber base material Automatic cutting machine 14 for cutting 14 45 ° reinforcing fiber substrate 15 Automatic cutting machine for cutting 90 ° reinforcing fiber substrate 16 90 ° reinforcing fiber substrate 17 Automatic cutting machine for cutting 45 ° reinforcing fiber substrate 18-45 ° Reinforcing Fiber Base 19 Slider 20 Oven 21 Pressure Bonding Jig 22 Bonding Jig Top 23 Bonding Jig Bottom 24 Pressure Unit 25 Winding Roll 26 Cooling Space 27 SUS Plate 28 Double-Sided Tape 29 Specimen 30 Base 31 Mounting jig 32 Longitudinal direction 33 Width direction 34 Test piece

Claims (9)

強化繊維基材を複数枚積層してなる平面状の強化繊維基材積層体であって、該強化繊維基材の積層層間の全面にわたって接合部が分布しており、該接合部は、ガラス転移温度Tgが0℃〜95℃である熱可塑性樹脂を含有する樹脂が2g/m〜40g/m付着しており、かつ、前記積層層間を形成する前記強化繊維基材両方に融着することにより形成されているとともに、前記積層層間が、接合力が500〜1000N/mである高接合領域と、前記高接合領域より接合部の分布する密度が低い低接合領域から形成されることを特徴とする強化繊維基材積層体。 A planar reinforcing fiber substrate laminate formed by laminating a plurality of reinforcing fiber substrates, wherein joints are distributed over the entire surface between the laminated layers of the reinforcing fiber substrates, and the joints are formed by glass transition. temperature Tg has a resin containing a thermoplastic resin is adhered 2g / m 2 ~40g / m 2 is 0 ° C. to 95 ° C., and fused to the both reinforcing fiber substrates forming the laminated layers In addition, the stacked layers are formed from a high bonding region having a bonding force of 500 to 1000 N / m 2 and a low bonding region in which the density of bonding portions is lower than that of the high bonding region. Reinforced fiber base laminate characterized by the above. 前記高接合領域の積層層間における割合が1〜10%である請求項1に記載の強化繊維基材積層体。 The reinforcing fiber substrate laminate according to claim 1, wherein a ratio of the high bonding region between the laminated layers is 1 to 10%. 前記高接合領域が強化繊維基材積層体の端部からの幅1〜5cmの領域である請求項1または2に記載の強化繊維基材積層体。 The reinforcing fiber base laminate according to claim 1 or 2, wherein the high bonding region is a region having a width of 1 to 5 cm from an end of the reinforcing fiber base laminate. 前記高接合領域の層間の接合力が低接合領域の層間の接合力に対して、1.5〜5倍である請求項1〜3のいずれかに記載の強化繊維基材積層体。 The reinforcing fiber substrate laminate according to any one of claims 1 to 3, wherein a bonding force between the layers in the high bonding region is 1.5 to 5 times as large as a bonding force between the layers in the low bonding region. 請求項1〜4のいずれかに記載の強化繊維基材積層体を賦形して得た強化繊維体積率Vpfが40%〜62%であるプリフォーム。 A preform having a reinforcing fiber volume fraction Vpf of 40% to 62% obtained by shaping the reinforcing fiber substrate laminate according to any one of claims 1 to 4. 強化繊維基材層間の全面にわたり、前記熱可塑性樹脂を含有する樹脂によって接着されている請求項5に記載のプリフォーム。 The preform according to claim 5, wherein the preform is bonded to the entire surface between the reinforcing fiber base layers with a resin containing the thermoplastic resin. 請求項5または6に記載のプリフォームに、マトリックス樹脂を注入、含浸、硬化して得られる強化繊維体積率Vfが35%〜72%の範囲内である繊維強化プラスチック成形品。 A fiber-reinforced plastic molded article having a reinforcing fiber volume fraction Vf in the range of 35% to 72% obtained by injecting, impregnating, and curing a matrix resin into the preform according to claim 5 or 6. 強化繊維基材の少なくとも片側の表面に、ガラス転移温度Tgが0℃〜95℃である熱可塑性樹脂を含有する樹脂が、2g/m〜40g/mの範囲内で付着されている強化繊維基材を用い、少なくとも次の工程(A)から(F)を経て強化繊維基材積層体を製造することを特徴とする強化繊維基材積層体の製造方法。
(A)強化繊維基材を所定の形状に裁断する裁断工程。
(B)前記所定の形状に裁断された強化繊維基材を、所定の積層構成に基づいて、順次、平面上に搬送・配置する積層工程。
(C)(B)で得られた積層体を加熱工程へ間欠的に搬送する搬送工程。
(D)搬送された積層体を加熱する加熱工程。
(E)該積層体を、加圧治具の一定面積当たりに有する加圧部の面積割合が、高い領域を1〜10%有する加圧治具を用いて加圧し、強化繊維基材の表面に付着している前記熱可塑性樹脂を含有する樹脂により、加圧部の強化繊維基材同士を厚み方向に接着する加圧接着工程。
(F)該積層体を冷却する冷却工程。
Strengthening reinforcement on at least one surface of the fibrous substrate, a resin containing a thermoplastic resin having a glass transition temperature Tg of 0 ° C. to 95 ° C. is being deposited within the 2g / m 2 ~40g / m 2 A method for producing a reinforced fiber substrate laminate, comprising using a fiber substrate and producing a reinforced fiber substrate laminate through at least the following steps (A) to (F).
(A) A cutting step of cutting the reinforcing fiber base into a predetermined shape.
(B) A laminating process in which the reinforcing fiber base material cut into the predetermined shape is sequentially transported and arranged on a plane based on a predetermined laminating configuration.
(C) The conveyance process which conveys the laminated body obtained by (B) intermittently to a heating process.
(D) The heating process which heats the conveyed laminated body.
(E) The surface of the reinforcing fiber substrate is pressed using a pressing jig having a region where the area ratio of the pressing part having a high area per fixed area of the pressing jig is 1 to 10%. A pressure bonding step in which the reinforcing fiber bases of the pressure portion are bonded in the thickness direction with the resin containing the thermoplastic resin adhering to the surface.
(F) A cooling step for cooling the laminate.
強化繊維基材積層体の端部からの幅1〜5cmである端部領域を加圧する加圧治具の一定面積当たりの加圧部の面積割合が、前記端部領域以外を加圧する加圧治具の一定面積当たりの加圧部の面積割合に対して、1.5〜5倍である請求項8に記載の強化繊維基材積層体の製造方法。 Pressurization in which the area ratio of the pressurizing unit per fixed area of the pressurizing jig pressurizing the end region having a width of 1 to 5 cm from the end of the reinforcing fiber base laminate presses other than the end region The method for producing a reinforced fiber base laminate according to claim 8, wherein the ratio is 1.5 to 5 times the area ratio of the pressing portion per fixed area of the jig.
JP2007056815A 2006-03-15 2007-03-07 Reinforced fiber substrate laminate and method for producing the same Active JP5029072B2 (en)