JP2021004327A - Adhesive resin composition, sheet, lid material, member set for hermetic vessel and vessel - Google Patents

Adhesive resin composition, sheet, lid material, member set for hermetic vessel and vessel Download PDF

Info

Publication number
JP2021004327A
JP2021004327A JP2019119558A JP2019119558A JP2021004327A JP 2021004327 A JP2021004327 A JP 2021004327A JP 2019119558 A JP2019119558 A JP 2019119558A JP 2019119558 A JP2019119558 A JP 2019119558A JP 2021004327 A JP2021004327 A JP 2021004327A
Authority
JP
Japan
Prior art keywords
vinyl acetate
ethylene
resin composition
adhesive resin
mass
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP2019119558A
Other languages
Japanese (ja)
Other versions
JP7240067B2 (en
Inventor
智紀 山田
Tomonori Yamada
智紀 山田
太亮 赤木
Tasuke Akagi
太亮 赤木
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Artience Co Ltd
Original Assignee
Toyo Ink SC Holdings Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toyo Ink SC Holdings Co Ltd filed Critical Toyo Ink SC Holdings Co Ltd
Priority to JP2019119558A priority Critical patent/JP7240067B2/en
Publication of JP2021004327A publication Critical patent/JP2021004327A/en
Application granted granted Critical
Publication of JP7240067B2 publication Critical patent/JP7240067B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

To provide an adhesive resin composition having excellent vessel adhesion resistance without generating resin residue or cobwebbing even in a flange of the vessel, also even under normal temperature or under freezing, in particular, when an adherend is a polyester-based vessel, showing excellent easy opening property, and having excellent film forming property during coating, a sheet using the composition, a lid material, a member set for hermetic vessel and a vessel.SOLUTION: The above-described problem can be solved by an adhesive resin composition containing 10 to 25 mass% of (A) an ethylene-α olefin copolymer having density of 0.88 to 0.93 g/cm3, 20 to 45 mass% of (B) an ethylene-vinyl acetate copolymer having a vinyl acetate content of 5% or larger and smaller than 18%, 10 to 35 mass% of (C) an ethylene-vinyl acetate copolymer having a vinyl acetate content of 18% or larger and smaller than 30%, and 25 to 35 mass% of (D) a tackifier resin, an adhesive resin composition, a sheet with the adhesive resin composition, a lid member, a member set for hermetic vessels and vessels.SELECTED DRAWING: None

Description

本発明は、開封時に界面剥離することで易開封性を示し、耐容器付着性と成膜性に優れる接着性樹脂組成物、該接着性樹脂組成物を用いたシート、蓋材、密封容器用部材セット及び容器に関するものである。 The present invention is for an adhesive resin composition which exhibits easy-opening property by peeling off the interface at the time of opening and has excellent container adhesiveness and film-forming property, and for sheets, lid materials, and sealed containers using the adhesive resin composition. It relates to a member set and a container.

食品包装の分野では、これまで、カップラーメンやヨーグルト、ゼリー等の内容物をポリエチレン系樹脂で被覆された紙容器に充填し、該容器の開口部にシール性の優れたヒートシール層を有する蓋材を接着する包装形態が盛んに利用されてきた。 In the field of food packaging, contents such as cup ramen, yogurt, and jelly have been filled in a paper container coated with a polyethylene resin, and a lid having a heat-sealing layer with excellent sealing properties at the opening of the container. A packaging form in which materials are bonded has been widely used.

しかし近年では、強度、透明性、耐熱性等の物理的性質が優れているという理由から、ポリエステル系樹脂、特にポリエチレンテレフタレート(以下、PETという)系樹脂からなる容器の利用が増大している。 However, in recent years, the use of polyester-based resins, particularly polyethylene terephthalate (hereinafter referred to as PET) -based resins, has been increasing because of their excellent physical properties such as strength, transparency, and heat resistance.

従来、主にポリエチレン系樹脂で被覆された紙容器を対象とした易開封性接着剤として、例えば、8〜49質量%の少なくとも500,000の平均分子量を有する1−ブテンのホモポリマー又は共重合体、及び92〜51質量%の930kg/m3又はこれ以下の密度を有する変性又は非変性低密度ポリエチレンを含む組成物が提案されている(特許文献1参照)。 Conventionally, as an easy-to-open adhesive for paper containers mainly coated with a polyethylene resin, for example, a homopolymer or copolymer of 1-butene having an average molecular weight of at least 500,000 of 8 to 49% by mass has been used. Compositions containing coalesced and modified or non-modified low density polyethylene having a density of 92 to 51% by mass of 930 kg / m 3 or less have been proposed (see Patent Document 1).

また、メルトインデックスが0.1〜100である熱可塑性樹脂Aと、この熱可塑性樹脂Aに非相溶系又は部分相溶系の熱可塑性樹脂Bであって、メルトインデックスが前記熱可塑性樹脂Aと特定の関係にある熱可塑性樹脂Bとを特定の割合で含有する組成物が提案されている(特許文献2参照)。 Further, the thermoplastic resin A having a melt index of 0.1 to 100 and the thermoplastic resin B incompatible or partially compatible with the thermoplastic resin A, and the melt index is specified as the thermoplastic resin A. A composition containing the thermoplastic resin B having a relationship with the above in a specific ratio has been proposed (see Patent Document 2).

さらに他の例として、エチレン重合体及びエチレン・酢酸ビニル共重合体の少なくとも一方の樹脂Aと、前記樹脂Aに非相溶の樹脂Bと、粘着付与樹脂を含有し、引張破断強度が2MPa以上15MPa以下であり、引張伸び強度が50%以上500%以下である組成物が提案されている(特許文献3参照)。 As yet another example, it contains at least one resin A of an ethylene polymer and an ethylene-vinyl acetate copolymer, a resin B incompatible with the resin A, and a tackifier resin, and has a tensile strength at break of 2 MPa or more. A composition having a tensile elongation strength of 15 MPa or less and a tensile elongation strength of 50% or more and 500% or less has been proposed (see Patent Document 3).

特開平1−315443号公報Japanese Unexamined Patent Publication No. 1-315443 特開2000−302990号公報Japanese Unexamined Patent Publication No. 2000-302990 特開2016−148003号公報Japanese Unexamined Patent Publication No. 2016-148003

特許文献1〜3で提案されている組成物は、相溶性の異なる2種類の樹脂を用いることにより開封時に凝集破壊することが特徴である。これにより、内容物をしっかり密封することができる。しかし一方で、容器のフランジにおいて樹脂残りや糸曳きが発生するため、外観不良だけでなく、容器に口をつけて食べる際に誤飲する可能性がある。 The compositions proposed in Patent Documents 1 to 3 are characterized in that they are coagulated and broken at the time of opening by using two kinds of resins having different compatibility. As a result, the contents can be tightly sealed. However, on the other hand, since resin residue and stringing are generated on the flange of the container, not only the appearance is poor, but also there is a possibility of accidental ingestion when eating with the container in the mouth.

本発明が解決しようとする課題は、特に被着体がポリエステル系容器に対し、常温・冷凍下においても、容器のフランジにおいて樹脂残りや糸曳きが発生せず耐容器付着性に優れ、良好な易開封性を示し、且つ、塗工時の成膜性に優れる接着性樹脂組成物、該組成物を用いたシート、蓋材、密封容器用部材セット及び容器を提供することである。 The problem to be solved by the present invention is that the adherend is a polyester-based container, and even at room temperature and freezing, no resin residue or stringing occurs on the flange of the container, and the container has excellent adhesion resistance. It is an object of the present invention to provide an adhesive resin composition which is easy to open and has excellent film forming property at the time of coating, a sheet, a lid material, a member set for a sealed container, and a container using the composition.

本発明者は、上記の課題を解決するために鋭意検討を行った結果、密度が0.88〜0.93g/cmのエチレン−αオレフィン共重合体(A)、酢酸ビニル含有率が5%以上18%未満のエチレン−酢酸ビニル共重合体(B)、酢酸ビニル含有率が18%以上30%未満のエチレン−酢酸ビニル共重合体(C)、及び粘着付与樹脂(D)を特定範囲の比率で含有することで上記課題を解決することを見出した。
特酢酸ビニル含有率が5%以上18%未満のエチレン−酢酸ビニル共重合体(B)は、PETへの密着性を付与する密度が0.88〜0.93g/cmのエチレン−αオレフィン共重合体(A)と、冷凍下において接着強度を発現する酢酸ビニル含有率が18%以上30%未満のエチレン−酢酸ビニル共重合体(C)との相溶化剤として働き、成膜性を向上させる効果を有する。
上記により、特に被着体がポリエステル系容器に対し、常温・冷凍下において易開封性と耐容器付着性に優れ、また、塗工時の成膜性に優れた接着性樹脂組成物、及びその接着性樹脂組成物の被膜が積層されたシートを提供することが可能となる。
すなわち本発明は下記〔1〕〜〔11〕の発明に関する。
As a result of diligent studies to solve the above problems, the present inventor has an ethylene-α olefin copolymer (A) having a density of 0.88 to 0.93 g / cm 3 and a vinyl acetate content of 5. A specific range of ethylene-vinyl acetate copolymer (B) of% or more and less than 18%, ethylene-vinyl acetate copolymer (C) having a vinyl acetate content of 18% or more and less than 30%, and tackifier resin (D). It was found that the above-mentioned problem can be solved by containing the content in the ratio of.
The ethylene-vinyl acetate copolymer (B) having a special vinyl acetate content of 5% or more and less than 18% is an ethylene-α olefin having a density of 0.88 to 0.93 g / cm 3 that imparts adhesion to PET. It acts as a compatibilizer between the copolymer (A) and the ethylene-vinyl acetate copolymer (C) having a vinyl acetate content of 18% or more and less than 30%, which develops adhesive strength under freezing, and improves film forming properties. It has the effect of improving.
Based on the above, an adhesive resin composition in which the adherend is excellent in easy-opening property and container adhesion resistance at room temperature and freezing, and also excellent in film-forming property at the time of coating, particularly with respect to a polyester-based container, and an adhesive resin composition thereof. It is possible to provide a sheet in which a coating film of an adhesive resin composition is laminated.
That is, the present invention relates to the following inventions [1] to [11].

〔1〕 密度が0.88〜0.93g/cmのエチレン−αオレフィン共重合体(A)10〜25質量%、酢酸ビニル含有率が5%以上18%未満のエチレン−酢酸ビニル共重合体(B)20〜45質量%、酢酸ビニル含有率が18%以上30%未満のエチレン−酢酸ビニル共重合体(C)10〜35質量%、粘着付与樹脂(D)25〜35質量%を含有する、接着性樹脂組成物。 [1] Ethylene-α olefin copolymer (A) having a density of 0.88 to 0.93 g / cm 3 by 10 to 25% by mass, and an ethylene-vinyl acetate copolymer having a vinyl acetate content of 5% or more and less than 18%. 20 to 45% by mass of the coalescence (B), 10 to 35% by mass of the ethylene-vinyl acetate copolymer (C) having a vinyl acetate content of 18% or more and less than 30%, and 25 to 35% by mass of the tackifier resin (D). Adhesive resin composition to be contained.

〔2〕 前記エチレン−αオレフィン共重合体(A)の示差走査型熱量計により測定した融点が100〜120℃である、〔1〕に記載の接着性樹脂組成物。 [2] The adhesive resin composition according to [1], wherein the ethylene-α-olefin copolymer (A) has a melting point of 100 to 120 ° C. as measured by a differential scanning calorimeter.

〔3〕 前記酢酸ビニル含有率が5%以上18%未満のエチレン−酢酸ビニル共重合体(B)の示差走査型熱量計により測定した融点が80〜100℃である、〔1〕又は〔2〕に記載の接着性樹脂組成物。 [3] The melting point of the ethylene-vinyl acetate copolymer (B) having a vinyl acetate content of 5% or more and less than 18% as measured by a differential scanning calorimeter is 80 to 100 ° C. [1] or [2]. ] The adhesive resin composition according to.

〔4〕 前記酢酸ビニル含有率が18%以上30%未満のエチレン−酢酸ビニル共重合体(C)の示差走査型熱量計により測定した融点が60〜90℃である、〔1〕〜〔3〕いずれか1項に記載の接着性樹脂組成物。 [4] The melting point of the ethylene-vinyl acetate copolymer (C) having a vinyl acetate content of 18% or more and less than 30% is 60 to 90 ° C. as measured by a differential scanning calorimeter, [1] to [3]. ] The adhesive resin composition according to any one of the items.

〔5〕 前記粘着付与樹脂(D)が脂環族炭化水素樹脂を含む、〔1〕〜〔4〕いずれか1項に記載の接着性樹脂組成物。 [5] The adhesive resin composition according to any one of [1] to [4], wherein the tackifier resin (D) contains an alicyclic hydrocarbon resin.

〔6〕 接着性樹脂組成物のメルトフローレートが10〜25g/10分である、〔1〕〜〔5〕いずれか1項に記載の接着性樹脂組成物。 [6] The adhesive resin composition according to any one of [1] to [5], wherein the melt flow rate of the adhesive resin composition is 10 to 25 g / 10 minutes.

〔7〕 酢酸ビニル含有量が5%以上18%未満のエチレン−酢酸ビニル共重合体(B)及び酢酸ビニル含有量が18%以上30%未満のエチレン−酢酸ビニル共重合体(C)の合計に対する酢酸ビニル含有量が、8%以上9.5%未満である、〔1〕〜〔6〕いずれか1項に記載の接着性樹脂組成物。 [7] Total of ethylene-vinyl acetate copolymer (B) having a vinyl acetate content of 5% or more and less than 18% and ethylene-vinyl acetate copolymer (C) having a vinyl acetate content of 18% or more and less than 30%. The adhesive resin composition according to any one of [1] to [6], wherein the vinyl acetate content is 8% or more and less than 9.5%.

〔8〕 基材上に、〔1〕〜〔7〕いずれか1項に記載の接着性樹脂組成物の膜が積層されたシート。 [8] A sheet in which a film of the adhesive resin composition according to any one of [1] to [7] is laminated on a base material.

〔9〕 〔8〕に記載のシートにより形成された蓋材。 [9] A lid material formed of the sheet according to [8].

〔10〕 ポリエステル系樹脂製の容器本体又は内面がポリエステル系樹脂で覆われた容器本体と、〔9〕に記載の蓋材とからなる、開封可能な密封容器用部材セット。 [10] A set of members for a sealed container that can be opened, comprising a container body made of polyester resin or a container body whose inner surface is covered with polyester resin, and a lid material according to [9].

〔11〕 ポリエステル系樹脂製の容器本体又は内面がポリエステル系樹脂で覆われた容器本体の開口部が、〔9〕に記載の蓋材により密封された、開封可能な容器。 [11] An openable container in which the opening of the container body made of polyester resin or the container body whose inner surface is covered with polyester resin is sealed by the lid material according to [9].

本発明により、特に被着体がポリエステル系容器に対し、常温・冷凍下においても、容器のフランジにおいて樹脂残りや糸曳きが発生せず耐容器付着性に優れ、良好な易開封性を示し、且つ、塗工時の成膜性に優れる接着性樹脂組成物、該組成物を用いたシート、蓋材、密封容器用部材セット及び容器を提供することができる。 According to the present invention, especially when the adherend is a polyester-based container, resin residue and stringing do not occur on the flange of the container even at room temperature and freezing, and the container has excellent adhesion resistance and good easy-opening property. Moreover, it is possible to provide an adhesive resin composition having excellent film forming property at the time of coating, a sheet using the composition, a lid material, a member set for a sealed container, and a container.

本願発明の接着性樹脂組成物は、密度が0.88〜0.93g/cmのエチレン−αオレフィン共重合体(A)10〜25質量%、酢酸ビニル含有率が5%以上18%未満のエチレン−酢酸ビニル共重合体(B)20〜45質量%、酢酸ビニル含有率が18%以上30%未満のエチレン−酢酸ビニル共重合体(C)10〜35質量%、粘着付与樹脂(D)25〜35質量%を含有する。
以下に、本発明について、詳細に説明する。
The adhesive resin composition of the present invention has an ethylene-α olefin copolymer (A) having a density of 0.88 to 0.93 g / cm 3 in an amount of 10 to 25% by mass and a vinyl acetate content of 5% or more and less than 18%. Ethylene-vinyl acetate copolymer (B) 20-45% by mass, ethylene-vinyl acetate copolymer (C) 10-35% by mass with vinyl acetate content of 18% or more and less than 30%, tackifier resin (D) ) 25-35% by mass.
The present invention will be described in detail below.

<密度が0.88〜0.93g/cmのエチレン−αオレフィン共重合体(A)>
本発明の接着性組成物を構成する密度が0.88〜0.93g/cmのエチレン−αオレフィン共重合体(A)としては、エチレンとプロピレン、ブテン、ペンテン、ヘキセン及びそれ以上の炭素鎖の長いオレフィンの中からなる群より選ばれる少なくとも1種とを任意の比率で重合した共重合体を用いることができる。
耐ブロッキング性の観点からエチレン−αオレフィン共重合体(A)は、プロピレン又はブテンが好ましく、より好ましくはブテンである。オレフィンの炭素鎖は短いほど耐ブロッキング性は向上する。
なお、本願における密度とは、JIS.K7112にピクノメーター法による測定値である。
<Ethylene-α-olefin copolymer (A) having a density of 0.88 to 0.93 g / cm 3 >
The ethylene-α-olefin copolymer (A) having a density of 0.88 to 0.93 g / cm 3 constituting the adhesive composition of the present invention includes ethylene and propylene, butene, penten, hexene and higher carbons. A copolymer obtained by polymerizing at least one selected from the group consisting of long-chain olefins at an arbitrary ratio can be used.
From the viewpoint of blocking resistance, the ethylene-α-olefin copolymer (A) is preferably propylene or butene, and more preferably butene. The shorter the carbon chain of the olefin, the better the blocking resistance.
The density in the present application is defined as JIS. It is a measured value by the pycnometer method in K7112.

エチレン−αオレフィン共重合体(A)は、接着性樹脂組成物中、10〜25質量%であり、好ましくは10〜20質量%である。
エチレン−αオレフィン共重合体(A)が10質量%以上であることにより、冷凍下において開封強度を損なうことなく、ポリエステル系樹脂製容器に十分に接着する。また、25質量%以下であることにより、冷凍下及び常温下において開封強度を損なうことなく、ポリエステル系樹脂製容器に十分に接着する。
The ethylene-α-olefin copolymer (A) is 10 to 25% by mass, preferably 10 to 20% by mass in the adhesive resin composition.
When the ethylene-α-olefin copolymer (A) is 10% by mass or more, it sufficiently adheres to the polyester resin container under freezing without impairing the opening strength. Further, when the content is 25% by mass or less, the container is sufficiently adhered to the polyester resin container under freezing and at room temperature without impairing the opening strength.

また、エチレン−αオレフィン共重合体(A)としては、示差走査型熱量計により測定した融点(以下、DSC融点という)が80〜140℃であることが好ましく、より好ましくは90〜130℃であり、特に好ましくは100〜120℃の範囲内である。上記の範囲内であると、PETへの密着性を向上できる点で好ましい。 The ethylene-α-olefin copolymer (A) preferably has a melting point (hereinafter referred to as DSC melting point) measured by a differential scanning calorimeter of 80 to 140 ° C, more preferably 90 to 130 ° C. Yes, particularly preferably in the range of 100 to 120 ° C. When it is within the above range, it is preferable in that the adhesion to PET can be improved.

<酢酸ビニル含有量が5%以上18%未満のエチレン−酢酸ビニル共重合体(B)>
本発明における接着性組成物を構成する酢酸ビニル含有率が5%以上18%未満のエチレン−酢酸ビニル共重合体(B)としては、エチレンに対し酢酸ビニルを5%以上18%未満の比率で重合した共重合体を用いることができる。
<Ethylene-vinyl acetate copolymer (B) having a vinyl acetate content of 5% or more and less than 18%>
The ethylene-vinyl acetate copolymer (B) having a vinyl acetate content of 5% or more and less than 18% constituting the adhesive composition in the present invention contains vinyl acetate at a ratio of 5% or more and less than 18% with respect to ethylene. A polymerized copolymer can be used.

エチレン−酢酸ビニル共重合体(B)は、接着性樹脂組成物中20〜45質量%であり、好ましくは25〜40質量%の範囲内である。
エチレン−酢酸ビニル共重合体(B)が20質量%以上であることにより、冷凍下及び常温下において開封強度を損なうことなく、ポリエステル系樹脂製容器に十分に接着する。また、45質量%以下であることにより、塗加工適性と接着性とのバランスをとることができるだけでなく、常温・冷凍下においても、容器のフランジにおいて樹脂残りや糸曳きが発生しない。
The ethylene-vinyl acetate copolymer (B) is in the range of 20 to 45% by mass, preferably 25 to 40% by mass in the adhesive resin composition.
When the ethylene-vinyl acetate copolymer (B) is 20% by mass or more, it sufficiently adheres to the polyester resin container under freezing and at room temperature without impairing the opening strength. Further, when it is 45% by mass or less, not only the coating processability and the adhesiveness can be balanced, but also resin residue and stringing do not occur on the flange of the container even at room temperature and freezing.

エチレン−酢酸ビニル共重合体(B)としては、DSC融点が80℃以上100℃未満、好ましくは85℃以上95未満の範囲内が好ましい。上記の範囲内であると、エチレン−αオレフィン共重合体(A)とエチレン−酢酸ビニル共重合体(C)とを相溶させ、塗加工適性を向上させるとともに開封強度を損なうことなく十分に接着できる点で好ましい。 The ethylene-vinyl acetate copolymer (B) preferably has a DSC melting point of 80 ° C. or higher and lower than 100 ° C., preferably 85 ° C. or higher and lower than 95 ° C. When it is within the above range, the ethylene-α-olefin copolymer (A) and the ethylene-vinyl acetate copolymer (C) are compatible with each other to improve the coating processability and sufficiently without impairing the opening strength. It is preferable because it can be bonded.

<酢酸ビニル含有量が18%以上30%未満のエチレン−酢酸ビニル共重合体(C)>
本発明における接着性組成物を構成する酢酸ビニル含有率が18%以上30%未満のエチレン−酢酸ビニル共重合体(C)としては、エチレンに対し酢酸ビニルを18%以上30%未満の比率で重合した共重合体を用いることができる。
<Ethylene-vinyl acetate copolymer (C) having a vinyl acetate content of 18% or more and less than 30%>
The ethylene-vinyl acetate copolymer (C) having a vinyl acetate content of 18% or more and less than 30% constituting the adhesive composition in the present invention contains vinyl acetate at a ratio of 18% or more and less than 30% with respect to ethylene. A polymerized copolymer can be used.

エチレン−酢酸ビニル共重合体(C)は、接着性樹脂組成物中、10〜35質量%であり、好ましくは10〜30質量%であり、特に好ましくは10〜25質量%の範囲である。
エチレン−酢酸ビニル共重合体(B)が10質量%以上であることにより、冷凍下でノ開封強度を抑制することができる。また、35質量%以下であることにより、成膜性と冷凍下及び常温化での接着性とのバランスをとることができる。
The ethylene-vinyl acetate copolymer (C) is in the range of 10 to 35% by mass, preferably 10 to 30% by mass, and particularly preferably 10 to 25% by mass in the adhesive resin composition.
When the ethylene-vinyl acetate copolymer (B) is 10% by mass or more, the opening strength can be suppressed under freezing. Further, when it is 35% by mass or less, it is possible to balance the film forming property and the adhesiveness under freezing and at room temperature.

エチレン−酢酸ビニル共重合体(C)としては、DSC融点が60℃以上90℃未満、好ましくは、65℃以上85℃未満の範囲内が好ましい。上記の範囲内であると、冷凍下における接着性を向上できる点で好ましい。 The ethylene-vinyl acetate copolymer (C) preferably has a DSC melting point of 60 ° C. or higher and lower than 90 ° C., preferably 65 ° C. or higher and lower than 85 ° C. When it is within the above range, it is preferable in that the adhesiveness under freezing can be improved.

<粘着付与樹脂(D)>
本発明の接着性組成物を構成する粘着付与樹脂(D)としては、脂肪族炭化水素樹脂、脂環族炭化水素樹脂、芳香族系炭化水素樹脂、ポリテルペン系樹脂、ロジン類等、シーラント接着分野で使用されている公知の粘着付与樹脂を用いることができる。粘着付与樹脂(D)は、単独又は2種類以上が使用できる。
粘着付与樹脂(D)は、接着性組成物中、25〜35質量%の範囲である。粘着付与樹脂が25質量%以上であると、冷凍下及び常温下において開封強度を損なうことなく、ポリエステル系樹脂製容器に十分に接着する。また、35質量%以下であると、成膜性が良好となる。中でも、粘着付与樹脂(D)は、脂環族炭化水素樹脂及び芳香族炭化水素樹脂からなる群から選ばれる少なくとも1種を含むことが好ましく、より好ましくは脂環族炭化水素樹脂を含むものである。上記樹脂は、部分水添や完全水添されていてもよい。
<Adhesive-imparting resin (D)>
Examples of the tackifier resin (D) constituting the adhesive composition of the present invention include aliphatic hydrocarbon resins, alicyclic hydrocarbon resins, aromatic hydrocarbon resins, polyterpene resins, rosins and the like in the field of sealant adhesion. A known tackifier resin used in the above can be used. The tackifier resin (D) can be used alone or in combination of two or more.
The tackifier resin (D) is in the range of 25 to 35% by mass in the adhesive composition. When the tackifying resin is 25% by mass or more, it sufficiently adheres to the polyester resin container under freezing and at room temperature without impairing the opening strength. Further, when it is 35% by mass or less, the film forming property becomes good. Among them, the tackifier resin (D) preferably contains at least one selected from the group consisting of an alicyclic hydrocarbon resin and an aromatic hydrocarbon resin, and more preferably contains an alicyclic hydrocarbon resin. The resin may be partially hydrogenated or completely hydrogenated.

粘着付与樹脂(D)は、ヒートシール時の接着性、即ち開封強度(易開封性)の観点において、軟化点が120℃以下であることが好ましい。なお、本発明における軟化点とは、JIS K 6863に規定される方法により求められる温度である。すなわち、規定の環に充填し12時間以上静置させた樹脂を、熱媒体中に入れて規定の球を置き一定の割合で熱媒体の温度を上昇させたとき、樹脂の軟化により球が沈み環台の底板に触れたときの温度である。
また、粘着付与樹脂(D)のDSC融点は、65〜95℃であることが好ましく、より好ましくは65〜80℃である。
The tackifier resin (D) preferably has a softening point of 120 ° C. or lower from the viewpoint of adhesiveness at the time of heat sealing, that is, opening strength (easy opening property). The softening point in the present invention is a temperature determined by the method specified in JIS K 6863. That is, when a resin filled in a specified ring and allowed to stand for 12 hours or more is placed in a heat medium and a specified ball is placed and the temperature of the heat medium is raised at a constant rate, the ball sinks due to the softening of the resin. This is the temperature when the bottom plate of the annulus is touched.
The DSC melting point of the tackifier resin (D) is preferably 65 to 95 ° C, more preferably 65 to 80 ° C.

<接着性樹脂組成物>
密度が0.88〜0.93g/cmのエチレン−αオレフィン共重合体(A)、酢酸ビニル含有率が5%以上18%未満のエチレン−酢酸ビニル共重合体(B)、酢酸ビニル含有率が18%以上30%未満のエチレン−酢酸ビニル共重合体(C)及び粘着付与樹脂(D)を、(A)/(B)/(C)/(D)=10〜25/20〜45/10〜35/25〜35(質量%)の組成で含有するものであり、好ましくは、10〜20/25〜40/10〜30/25〜35(質量%)であり、より好ましくは、10〜20/25〜40/10〜25/25〜35(質量%)である。但し、(A)、(B)、(C)及び(D)の合計を100質量%とする。
<Adhesive resin composition>
Contains ethylene-α olefin copolymer (A) having a density of 0.88 to 0.93 g / cm 3 , ethylene-vinyl acetate copolymer (B) having a vinyl acetate content of 5% or more and less than 18%, and vinyl acetate. Ethylene-vinyl acetate copolymer (C) and tackifier resin (D) having a ratio of 18% or more and less than 30% can be used from (A) / (B) / (C) / (D) = 10 to 25/20. It is contained in a composition of 45/10 to 35/25 to 35 (mass%), preferably 10 to 20/25 to 40/10 to 30/25 to 35 (mass%), and more preferably. , 10 to 20/25 to 40/10 to 25/25 to 35 (mass%). However, the total of (A), (B), (C) and (D) is 100% by mass.

エチレン−αオレフィン共重合体(A)、エチレン−酢酸ビニル共重合体(B)、エチレン−酢酸ビニル共重合体(C)及び粘着付与樹脂(D)の合計量は、接着性樹脂組成物100質量%中、90質量%以上が好ましく、より好ましくは95質量%以上、さらに好ましくは98質量%以上である。 The total amount of the ethylene-α olefin copolymer (A), the ethylene-vinyl acetate copolymer (B), the ethylene-vinyl acetate copolymer (C) and the tackifier resin (D) is the adhesive resin composition 100. Of the mass%, 90% by mass or more is preferable, 95% by mass or more is more preferable, and 98% by mass or more is further preferable.

接着性樹脂組成物のMFRは、1〜50g/10分であることが好ましく、より好ましくは10〜25g/10分の範囲内である。上記の範囲内であると、塗工時の成膜性の点で好ましい。本願におけるMFRとは、JIS.K7210に準ずる190℃、21.168NにおけるMFR値である。 The MFR of the adhesive resin composition is preferably 1 to 50 g / 10 minutes, more preferably 10 to 25 g / 10 minutes. When it is within the above range, it is preferable in terms of film forming property at the time of coating. The MFR in the present application is defined as JIS. It is an MFR value at 190 ° C. and 21.168N according to K7210.

また、接着性樹脂組成物において、酢酸ビニル含有量が5%以上18%未満のエチレン−酢酸ビニル共重合体(B)及び酢酸ビニル含有量が18%以上30%未満のエチレン−酢酸ビニル共重合体(C)の合計に対する酢酸ビニル含有量は、好ましくは8%以上9.5%未満であり、より好ましくは8.5%以上9.0%未満である。上記範囲であると、成膜性、並びに、常温下及び冷凍下の易開封性のバランスに優れ、両物性を両立する観点から好ましい。 Further, in the adhesive resin composition, the ethylene-vinyl acetate copolymer (B) having a vinyl acetate content of 5% or more and less than 18% and the ethylene-vinyl acetate copolymer having a vinyl acetate content of 18% or more and less than 30% have a common weight. The vinyl acetate content with respect to the total of the coalescence (C) is preferably 8% or more and less than 9.5%, and more preferably 8.5% or more and less than 9.0%. The above range is preferable from the viewpoint of excellent balance between film forming property and easy opening property at room temperature and freezing, and both physical properties are compatible.

本発明の樹脂組成物には、本発明の目的に反しない範囲、すなわち、成膜性、冷凍下及び常温下での易開封性、並びにPET容器への耐容器付着性を損なわない範囲で、エチレン−αオレフィン共重合体(A)、エチレン−酢酸ビニル共重合体(B)、エチレン−酢酸ビニル共重合体(C)及び粘着付与樹脂(D)以外の樹脂を配合してもよい。 The resin composition of the present invention has a range not contrary to the object of the present invention, that is, a range that does not impair the film-forming property, the easy-opening property under freezing and at room temperature, and the adhesiveness to the PET container. A resin other than the ethylene-α olefin copolymer (A), the ethylene-vinyl acetate copolymer (B), the ethylene-vinyl acetate copolymer (C) and the tackifier resin (D) may be blended.

このような樹脂としては、具体的には、高密度ポリエチレン、ポリプロピレン等、公知のポリオレフィン樹脂及びその酸化物やマレイン酸変性物、エチレン−アクリル酸共重合体、エチレン−(メタ)アクリル酸共重合体等のエチレン−不飽和モノカルボン酸共重合体及びその金属塩、スチレン−ブタジエン共重合エラストマー及びその水素付加物等の各種エラストマー、あるいは、高密度ポリエチレンワックス、ポリプロピレンワックス、エチレン−酢酸ビニル共重合体ワックス、フィッシャートロプシュワックス、パラフィンワックス、酸化ワックス、マレイン酸変性ワックス、スチレンモノマーのグラフトされたポリエチレンワックス等、公知のワックスが挙げられる。また、これらの樹脂は、単独で用いられても、2種類以上が併用されてもよい。 Specific examples of such resins include known polyolefin resins such as high-density polyethylene and polypropylene, oxides thereof, maleic acid-modified products, ethylene-acrylic acid copolymers, and ethylene- (meth) acrylic acid copolymers. Various elastomers such as ethylene-unsaturated monocarboxylic acid copolymers and metal salts thereof, styrene-butadiene copolymer elastomers and hydrogen adducts thereof, or high-density polyethylene wax, polypropylene wax, ethylene-vinyl acetate copolymer weight. Known waxes such as coalesced wax, Fishertroph wax, paraffin wax, oxide wax, maleic acid-modified wax, and polyethylene wax grafted with styrene monomer can be mentioned. Further, these resins may be used alone or in combination of two or more.

本発明の接着性樹脂組成物には、本発明の目的を損なわない範囲で、熱劣化、熱分解、ブロッキング等を防止するため、及びフィルム加工、押出ラミネート加工等の加工適正を確保するために、さらに添加剤等が使用されてもよい。添加剤の例としては、例えばエルカ酸アミド等の有機滑剤、炭酸カルシウム等の無機滑剤、ヒンダードフェノール等の酸化防止剤、その他ブロッキング防止剤、帯電防止剤、充填剤、顔料、防曇剤などが挙げられる。これら添加剤は、エチレン−αオレフィン共重合体(A)、エチレン−酢酸ビニル共重合体(B)、エチレン−酢酸ビニル共重合体(C)及び粘着付与樹脂(D)の配合時に添加されてもよいし、予めエチレン−αオレフィン共重合体(A)、エチレン−酢酸ビニル共重合体(B)、エチレン−酢酸ビニル共重合体(C)又は粘着付与樹脂(D)のいずれかに練りこまれた後、他の成分と混練することにより配合されてもよい。 The adhesive resin composition of the present invention is used to prevent thermal deterioration, thermal decomposition, blocking, etc., and to ensure processing suitability such as film processing, extrusion laminating processing, etc., as long as the object of the present invention is not impaired. , Further additives and the like may be used. Examples of additives include organic lubricants such as erucic acid amide, inorganic lubricants such as calcium carbonate, antioxidants such as hindered phenol, other antiblocking agents, antistatic agents, fillers, pigments, antifogging agents and the like. Can be mentioned. These additives are added at the time of blending the ethylene-α olefin copolymer (A), the ethylene-vinyl acetate copolymer (B), the ethylene-vinyl acetate copolymer (C) and the tackifier resin (D). Alternatively, it may be kneaded in advance with any one of ethylene-α olefin copolymer (A), ethylene-vinyl acetate copolymer (B), ethylene-vinyl acetate copolymer (C) or tackifier resin (D). After being mixed, it may be blended by kneading with other ingredients.

エチレン−αオレフィン共重合体(A)、エチレン−酢酸ビニル共重合体(B)、エチレン−酢酸ビニル共重合体(C)、粘着付与樹脂(D)及び必要に応じ用いられる添加剤の配合は、例えば、これら各成分をヘンシェルミキサー、タンブラーミキサーなどの混合装置に投入し、ブレンド時間5〜20分間で混合した後、押出機に入れ、加熱混練した後押し出すことにより行われる。押出物は通常ペレット形状とされて、後の工程で利用される。押出機としては、例えば二軸押出機などが好ましいものとして挙げられるが、これに限られるものではない。また、押出は、通常140〜200℃で行われる。 The formulation of ethylene-α olefin copolymer (A), ethylene-vinyl acetate copolymer (B), ethylene-vinyl acetate copolymer (C), tackifier resin (D) and additives used as necessary For example, each of these components is put into a mixing device such as a Henschel mixer or a tumbler mixer, mixed for a blending time of 5 to 20 minutes, placed in an extruder, heat-kneaded, and then extruded. The extruded product is usually in pellet form and is used in a later process. Examples of the extruder include, but are not limited to, a twin-screw extruder. Further, extrusion is usually performed at 140 to 200 ° C.

<シート>
次に、基材上に、本発明の接着性樹脂組成物の被膜が積層されたシートについて説明する。本発明の接着性樹脂組成物の基材への積層方法としては、例えば、前記のごとくペレット化された樹脂組成物を用い、インフレーション法あるいはキャスト法などにより単層フィルム化し、このフィルムを基材と必要であれば別の接着剤層を介して積層する方法が挙げられる。あるいは、混練された樹脂組成物を直接基材に被覆してもよいし、更に他の方法がとられてもよい。
<Sheet>
Next, a sheet in which a coating film of the adhesive resin composition of the present invention is laminated on a base material will be described. As a method for laminating the adhesive resin composition of the present invention on a base material, for example, the resin composition pelletized as described above is used to form a single-layer film by an inflation method or a casting method, and this film is used as a base material. And if necessary, a method of laminating via another adhesive layer can be mentioned. Alternatively, the kneaded resin composition may be directly coated on the base material, or another method may be adopted.

積層面の接着性を改善するために、基材表面に火炎処理、オゾン処理、コロナ放電処理又はアンカーコート剤による処理が行われてもよい。ポリエチレン系樹脂を予めラミネートしてある基材に対しては、ダイレクトに押出しラミネートすることも可能である。また、ポリエチレンやポリプロピレン等との共押出しで多層フィルム化しておき、ドライラミネーション又はサンドラミネーションにより、基材となるポリエステルフィルム、ポリアミドフィルム、ポリプロピレンフィルム等の延伸又は未延伸フィルムと積層することにより、積層されたシートを得ることもできる。この場合にも、積層面の接着性を改善するために、必要であれば、基材表面に対し、火炎処理、オゾン処理、コロナ放電処理又はアンカーコート剤による処理などが行われてもよい。また、本発明の接着性樹脂組成物層の厚みは、好ましくは5μm以上、より好ましくは10μm以上である。
なお、本発明における「基材」とは、長尺及びカットされた短尺のフィルム、シートを包含するものとして用いられ、さらに「基材」は、単層のもの及び複数の層からなる積層物をも包含するものである。また、本発明の接着性樹脂組成物が積層されたシートは、後述するように蓋材として用いることができる他、シーラントフィルムとして接着性樹脂組成物の被膜を内面としてシールした製袋品にも好適に使用できる。
In order to improve the adhesiveness of the laminated surface, the surface of the base material may be treated with a flame treatment, an ozone treatment, a corona discharge treatment or an anchor coating agent. It is also possible to directly extrude and laminate a base material on which a polyethylene resin is laminated in advance. In addition, a multilayer film is formed by co-extrusion with polyethylene, polypropylene, etc., and then laminated by drying or sand lamination with a stretched or unstretched film such as a polyester film, a polyamide film, or a polypropylene film as a base material. You can also get the finished sheet. In this case as well, in order to improve the adhesiveness of the laminated surface, the surface of the base material may be treated with a flame treatment, an ozone treatment, a corona discharge treatment, an anchor coating agent, or the like, if necessary. The thickness of the adhesive resin composition layer of the present invention is preferably 5 μm or more, more preferably 10 μm or more.
The "base material" in the present invention is used to include long and cut short films and sheets, and the "base material" is a single layer or a laminate composed of a plurality of layers. Also includes. Further, the sheet on which the adhesive resin composition of the present invention is laminated can be used as a lid material as described later, and can also be used as a sealant film for a bag-making product in which a film of the adhesive resin composition is sealed as an inner surface. Can be suitably used.

<蓋材>
基材上に接着性樹脂組成物が積層された本発明のシートは、密封対象である容器本体の開口形状に合わせて裁断され蓋材として好適に用いられる。
本発明のシートを蓋材として用いる場合、基材としては種々の基材を用いることができる。使用される基材としては、紙、アルミニウム、ポリエステル、ポリエチレン、ポリプロピレン、ポリスチレン、アルミ蒸着ポリエステル、アルミ蒸着ポリプロピレン又はシリカ蒸着ポリエステルなどを挙げることができる。このような基材は、単層である必要はなく、二層以上の積層体であっても良い。
また、本発明のシートにより蓋材を形成する場合、基材として好ましくは、例えば5〜20μmのPETと5〜30μmのポリエチレンとの積層体であり、前記積層体のポリエチレン面に、本発明の接着性樹脂組成物から形成される厚さ5〜40μmの被膜を積層したものが好ましい。
<Lid material>
The sheet of the present invention in which the adhesive resin composition is laminated on the base material is cut according to the opening shape of the container body to be sealed and is suitably used as a lid material.
When the sheet of the present invention is used as a lid material, various base materials can be used as the base material. Examples of the base material used include paper, aluminum, polyester, polyethylene, polypropylene, polystyrene, aluminum vapor-deposited polyester, aluminum-deposited polypropylene, and silica-deposited polyester. Such a base material does not have to be a single layer, and may be a laminated body having two or more layers.
When the lid material is formed from the sheet of the present invention, the base material is preferably a laminate of, for example, 5 to 20 μm PET and 5 to 30 μm polyethylene, and the polyethylene surface of the laminate is covered with the present invention. A laminated film having a thickness of 5 to 40 μm formed from the adhesive resin composition is preferable.

<容器本体>
容器本体としては、ポリエステル系樹脂製の容器本体、内面がポリエステル系樹脂で覆われた容器本体の他、ポリエチレン系樹脂製の容器本体、内面がポリエチレン系樹脂で覆われた容器本体等が挙げられ、特に、ポリエステル系樹脂製の容器本体、内面がポリエステル系樹脂で覆われた容器本体が好ましい。
<Container body>
Examples of the container body include a container body made of polyester resin, a container body whose inner surface is covered with polyester resin, a container body made of polyethylene resin, and a container body whose inner surface is covered with polyethylene resin. In particular, a container body made of polyester resin and a container body whose inner surface is covered with polyester resin are preferable.

<開封可能な密封容器>
本発明の開封可能な密封容器は、容器本体の開口形状に合わせて裁断された蓋材によって、容器本体の開口部の封緘がなされたものである。即ち、蓋材の一方の面に配設された本発明の接着性樹脂組成物と、密封容器の開口部の接着面(フランジとも言われる)とを接触させ加熱することによって、両者を接着する。接着条件は、100〜180℃であることが好ましい。
容器本体がPET容器の場合、該容器本体と前記蓋材とを熱接着温度100〜180℃で熱接着を行うことが好ましく、常温での開封強度が7〜15Nの範囲であり、また剥離時に熱接着層が界面剥離することが好ましい。本発明の開封可能な密封には、例えばゼリー、プリン、ヨーグルトや冷菓、乾燥菓子又はカップ麺等を包装することができる。
<Openable sealed container>
The openable sealed container of the present invention is one in which the opening of the container body is sealed by a lid material cut according to the opening shape of the container body. That is, the adhesive resin composition of the present invention disposed on one surface of the lid material and the adhesive surface (also referred to as a flange) of the opening of the sealed container are brought into contact with each other and heated to bond the two. .. The bonding conditions are preferably 100 to 180 ° C.
When the container body is a PET container, it is preferable to heat-bond the container body and the lid material at a heat bonding temperature of 100 to 180 ° C., the opening strength at room temperature is in the range of 7 to 15 N, and at the time of peeling. It is preferable that the thermal adhesive layer is interfacially peeled off. For example, jelly, pudding, yogurt, frozen dessert, dried confectionery, cup noodles, etc. can be wrapped in the openable seal of the present invention.

以下に、本発明を実施例に基づいて説明するが、本発明はこれによって限定されるものではない。なお、実施例中、「部」及び「%」は、「質量部」及び「質量%」をそれぞれ表す。 Hereinafter, the present invention will be described based on examples, but the present invention is not limited thereto. In the examples, "parts" and "%" represent "parts by mass" and "% by mass", respectively.

<接着性樹脂組成物の製造方法>
[実施例1〜9及び比較例1〜8]
(接着性樹脂組成物(S−1)〜(S−17)の製造)
表1に記載の、密度が0.88〜0.93g/cmのエチレン−αオレフィン共重合体(A)、酢酸ビニル含有率が5%以上18%未満のエチレン−酢酸ビニル共重合体(B)、酢酸ビニル含有率が18%以上30%未満のエチレン−酢酸ビニル共重合体(C)、粘着付与樹脂(D)、ブロッキング防止剤及び酸化防止剤を、ヘンシェルミキサーで5分間プリブレンドした。ホッパーにプリブレンド物を投入し、スクリューフィーダーを用いて下記押出機に供給し、接着性樹脂組成物(S−1)〜(S−17)を製造した。表1中の数値の単位は、表記のないものは部を表す。

≪押出機条件≫
押出機:アイ・ケー・ジー社製同方向回転二軸押出機PMT32−40.5
バレル温度:180℃(供給口160℃)
スクリュー回転速度:200rpm
供給速度:10kg/hr
<Manufacturing method of adhesive resin composition>
[Examples 1 to 9 and Comparative Examples 1 to 8]
(Production of Adhesive Resin Compositions (S-1) to (S-17))
The ethylene-α olefin copolymer (A) having a density of 0.88 to 0.93 g / cm 3 and the ethylene-vinyl acetate copolymer having a vinyl acetate content of 5% or more and less than 18% (A) shown in Table 1 ( B), an ethylene-vinyl acetate copolymer (C) having a vinyl acetate content of 18% or more and less than 30%, a tackifier resin (D), an antioxidant and an antioxidant were pre-blended with a Henschel mixer for 5 minutes. .. The preblended product was put into a hopper and supplied to the following extruder using a screw feeder to produce adhesive resin compositions (S-1) to (S-17). Units of numerical values in Table 1 represent parts if not shown.

≪Extruder conditions≫
Extruder: IKG Co., Ltd. Same-direction rotating twin-screw extruder PMT32-40.5
Barrel temperature: 180 ° C (supply port 160 ° C)
Screw rotation speed: 200 rpm
Supply speed: 10 kg / hr

<接着性樹脂組成物の評価>
得られた接着性樹脂組成物について、MFR及び成膜性を評価した。また、下記に従って積層されたシート(蓋材)を作製し、該シートを用いて、冷凍下及び常温下の開封強度(易開封性)、耐容器付着性(糸曳き)を、以下の方法及び基準に基づいて評価した。結果を表1に示す。
<Evaluation of adhesive resin composition>
The MFR and film forming property of the obtained adhesive resin composition were evaluated. In addition, a sheet (lid material) laminated according to the following is prepared, and the sheet is used to determine the opening strength (easy opening property) and container adhesion (thread pulling) under freezing and at room temperature by the following methods and. Evaluated based on criteria. The results are shown in Table 1.

[MFR]
接着性樹脂組成物のMFRは、JIS.K7210に準拠し、メルトインデクサーL244(宝工業株式会社製)の内径9.55mm、長さ162mmのシリンダにサンプルを充填し、190℃で溶融した後、重さ2160g、直径9.48mmのプランジャーを使用して均等に荷重をかけ、シリンダの中央に設けた径2.1mmのオリフィスより単位時間あたりに押出される樹脂量(g/10分)から求めた。
[MFR]
The MFR of the adhesive resin composition is JIS. A plan with a weight of 2160 g and a diameter of 9.48 mm after filling a sample in a cylinder of melt indexer L244 (manufactured by Takara Kogyo Co., Ltd.) with an inner diameter of 9.55 mm and a length of 162 mm and melting it at 190 ° C. in accordance with K7210. A load was evenly applied using a jar, and the amount was determined from the amount of resin (g / 10 minutes) extruded per unit time from an orifice having a diameter of 2.1 mm provided in the center of the cylinder.

[成膜性]
接着性樹脂組成物の成膜性は、下記加工条件において200〜250℃のいずれかの温度での塗工の可否と、得られた塗工物から膜厚計を用いて無造作に10カ所の膜厚を測定した際の数値から、下記基準で評価した。
≪加工条件≫
押出しラミネーター:ムサシノキカイ製400M/MテストEXTラミネーターダイ直下樹脂温度:200〜250℃
加工速度:30m/分
Tダイ幅:400mm
冷却ロール表面温度:20℃
基材:PET12μm/PE25μm基材のPE面に塗工
○:塗工可能、かつ、膜厚が20±3μmである:良好
△:塗工可能、かつ、膜厚が20±6μmである:使用可能
×:膜割れ若しくは膜切れのいずれかが発生して塗工不可、又は、塗工可能だが膜厚が20±6μmを超える:不良
[Film film property]
The film-forming property of the adhesive resin composition is determined by whether or not it can be coated at any temperature of 200 to 250 ° C. under the following processing conditions, and from the obtained coated product, at 10 locations at random using a film thickness meter. From the numerical value when the film thickness was measured, it was evaluated according to the following criteria.
≪Processing conditions≫
Extruded laminator: Made by Musashinokikai 400M / M test EXT laminator Die direct resin temperature: 200-250 ℃
Processing speed: 30 m / min T die width: 400 mm
Cooling roll surface temperature: 20 ° C
Base material: PET 12 μm / PE 25 μm Coating on the PE surface of the base material ○: Can be applied and the film thickness is 20 ± 3 μm: Good Δ: Can be applied and the film thickness is 20 ± 6 μm: Use Possible ×: Either film cracking or film breakage occurs and coating is not possible, or coating is possible but the film thickness exceeds 20 ± 6 μm: Defective

[シート(蓋材)の作製方法]
得られた接着性樹脂組成物を、押出しラミネーターを用いて、PET12μm/PE25μmの基材のPE面に積層してシートを作製した。接着剤層の厚さは20μmであった。以下に加工条件を示す。
押出しラミネーター:ムサシノキカイ製400M/MテストEXTラミネーターダイ直下樹脂温度:200℃〜250℃(接着性樹脂組成物のMFR等により適宜調整した)。
加工速度:30m/分
Tダイ幅:400mm
冷却ロール表面温度:20℃
[Method of manufacturing sheet (lid material)]
The obtained adhesive resin composition was laminated on the PE surface of a base material of PET 12 μm / PE 25 μm using an extruded laminator to prepare a sheet. The thickness of the adhesive layer was 20 μm. The processing conditions are shown below.
Extruded laminator: 400M / M test EXT laminator manufactured by Musashinokikai Resin temperature directly under the die: 200 ° C to 250 ° C (adjusted appropriately by MFR or the like of the adhesive resin composition).
Processing speed: 30 m / min T die width: 400 mm
Cooling roll surface temperature: 20 ° C

[易開封性(常温)]
得られた積層シート(蓋材)を90mm×90mmのサイズに断裁後、ゲージ圧0.3MPa、150℃、1秒にて71ΦPET容器に、接着性樹脂組成物面を熱接着し、密封を行なった。温度23℃湿度65%の恒温恒湿室に24時間放置し、同恒温恒湿室にて90°角剥離、引張速度200mm/分の条件で剥離強度の測定を行った。最大値を開封強度とし、易開封性を下記基準で評価した。
〇:剥離強度が、7N以上15N未満:良好
△:剥離強度が、5N以上 7N未満、又は、15N以上17N未満:使用可能
×:剥離強度が、5N未満、又は、17N以上:不良
[Easy to open (normal temperature)]
The obtained laminated sheet (lid material) is cut into a size of 90 mm × 90 mm, and then the adhesive resin composition surface is heat-bonded to a 71Φ PET container at a gauge pressure of 0.3 MPa, 150 ° C., and 1 second to seal it. It was. It was left in a constant temperature and humidity chamber at a temperature of 23 ° C. and a humidity of 65% for 24 hours, and the peel strength was measured under the conditions of 90 ° square peeling and a tensile speed of 200 mm / min in the same constant temperature and humidity chamber. The maximum value was taken as the opening strength, and the ease of opening was evaluated according to the following criteria.
〇: Peeling strength is 7N or more and less than 15N: Good Δ: Peeling strength is 5N or more and less than 7N, or 15N or more and less than 17N: Usable ×: Peeling strength is less than 5N or 17N or more: Defective

[易開封性(冷凍)]
得られた積層シート(蓋材)を90mm×90mmのサイズに断裁後、ゲージ圧0.3MPa、150℃、1秒にて71ΦPET容器に、接着性樹脂組成物面を熱接着し、密封を行なった。温度−20℃の恒温槽に24時間放置し、同恒温槽にて90°角剥離、引張速度200mm/分の条件で剥離強度の測定を行った。最大値を開封強度とし、易開封性を下記基準で評価した。
〇:剥離強度が、7N以上15N未満:良好
△:剥離強度が、5N以上 7N未満、又は、15N以上17N未満:使用可能
×:剥離強度が、5N未満、又は、17N以上:不良
[Easy to open (frozen)]
The obtained laminated sheet (lid material) is cut into a size of 90 mm × 90 mm, and then the adhesive resin composition surface is heat-bonded to a 71Φ PET container at a gauge pressure of 0.3 MPa, 150 ° C., and 1 second to seal it. It was. It was left in a constant temperature bath at a temperature of −20 ° C. for 24 hours, and the peel strength was measured under the conditions of 90 ° square peeling and a tensile speed of 200 mm / min in the same constant temperature bath. The maximum value was taken as the opening strength, and the ease of opening was evaluated according to the following criteria.
〇: Peeling strength is 7N or more and less than 15N: Good Δ: Peeling strength is 5N or more and less than 7N, or 15N or more and less than 17N: Usable ×: Peeling strength is less than 5N or 17N or more: Defective

[常温下及び冷凍下での耐容器付着性]
上記常温下及び冷凍下における開封強度測定時のPET容器フランジ部の接着性樹脂組成物の有無を目視で確認し、下記基準で評価した。
〇: 常温下及び冷凍下いずれにおいても、フランジ部に接着性樹脂組成物の付着がないもの:良好
△:常温下又は冷凍下いずれかにおいて、フランジ部に接着性樹脂組成物の付着が僅かにみられたもの:使用可能
×:常温下又は冷凍下いずれかにおいて、フランジ部に接着性樹脂組成物の付着がみられたもの:不良
[Container adhesion resistance at room temperature and freezing]
The presence or absence of the adhesive resin composition on the flange of the PET container at the time of measuring the opening strength at room temperature and freezing was visually confirmed and evaluated according to the following criteria.
〇: No adhesion of the adhesive resin composition to the flange at both normal temperature and freezing: Good Δ: Slight adhesion of the adhesive resin composition to the flange at either normal temperature or freezing Specified: Usable ×: Adhesive resin composition adhered to the flange at either normal temperature or freezing: Defective

表1で用いた原料略称を以下に示す。
A1:ルミタック22−7(東ソー社製、エチレン−ブテン共重合体、密度0.900g/cm3、DSC融点113℃、MFR2g/10分)
A2:ルミタック43−1(東ソー社製、エチレン−ブテン共重合体、密度0.910g/cm3、DSC融点113℃、MFR20g/10分)
The raw material abbreviations used in Table 1 are shown below.
A1: Lumitac 22-7 (manufactured by Tosoh Corporation, ethylene-butene copolymer, density 0.900 g / cm 3 , DSC melting point 113 ° C., MFR 2 g / 10 minutes)
A2: Lumitac 43-1 (manufactured by Tosoh Corporation, ethylene-butene copolymer, density 0.910 g / cm 3 , DSC melting point 113 ° C., MFR 20 g / 10 minutes)

B1:ウルトラセン540(東ソー社製、エチレン−酢酸ビニル共重合体(酢酸ビニル含有率10%)、密度0.929g/cm3、DSC融点94℃、MFR3g/10分)
B2:ウルトラセン626(東ソー社製、エチレン−酢酸ビニル共重合体(酢酸ビニル含有率15%)、密度0.936g/cm3、DSC融点88℃、MFR3g/10分)
B1: Ultrasen 540 (manufactured by Tosoh Corporation, ethylene-vinyl acetate copolymer (vinyl acetate content 10%), density 0.929 g / cm 3 , DSC melting point 94 ° C., MFR 3 g / 10 minutes)
B2: Ultrasen 626 (manufactured by Tosoh Corporation, ethylene-vinyl acetate copolymer (vinyl acetate content 15%), density 0.936 g / cm 3 , DSC melting point 88 ° C., MFR 3 g / 10 minutes)

C1:ウルトラセン627(東ソー社製、エチレン−酢酸ビニル共重合体(酢酸ビニル含有率20%)、密度0.941g/cm3、DSC融点83℃、MFR1g/10分)
C2:ウルトラセン751(東ソー社製、エチレン−酢酸ビニル共重合体(酢酸ビニル含有率28%)、密度0.952g/cm3、DSC融点70℃、MFR6g/10分)
C3:ウルトラセン634(東ソー社製、エチレン−酢酸ビニル共重合体(酢酸ビニル含有率26%)、密度0.949g/cm3、DSC融点74℃、MFR4g/10分)
C1: Ultrasen 627 (manufactured by Tosoh Corporation, ethylene-vinyl acetate copolymer (vinyl acetate content 20%), density 0.941 g / cm 3 , DSC melting point 83 ° C., MFR 1 g / 10 minutes)
C2: Ultrasen 751 (manufactured by Tosoh Corporation, ethylene-vinyl acetate copolymer (vinyl acetate content 28%), density 0.952 g / cm 3 , DSC melting point 70 ° C., MFR 6 g / 10 minutes)
C3: Ultrasen 634 (manufactured by Tosoh Corporation, ethylene-vinyl acetate copolymer (vinyl acetate content 26%), density 0.949 g / cm 3 , DSC melting point 74 ° C., MFR 4 g / 10 minutes)

D1:アルコンM−115(荒川化学工業社製、部分水添脂環族炭化水素樹脂、軟化点115℃)
D2:アルコンP−115(荒川化学工業社製、完全水添脂環族炭化水素樹脂、軟化点115℃)
D1: Archon M-115 (manufactured by Arakawa Chemical Industries, Ltd., partially hydrogenated alicyclic hydrocarbon resin, softening point 115 ° C)
D2: Archon P-115 (manufactured by Arakawa Chemical Industries, Ltd., completely hydrogenated alicyclic hydrocarbon resin, softening point 115 ° C)

ブロッキング防止剤:インクロスリップC(クローダ社製、エルカ酸アミド、DSC融点80℃) Anti-blocking agent: Incross Lip C (manufactured by Croda, erucic acid amide, DSC melting point 80 ° C)

酸化防止剤:IRGANOX 1010(BASF社製、ヒンダードフェノール系酸化防止剤) Antioxidant: IRGANOX 1010 (BASF, hindered phenolic antioxidant)

VA cont.:酢酸ビニル含有率(%) VA cont. : Vinyl acetate content (%)

実施例1〜9の接着剤組成物は、成膜性に優れ、且つ、常温下及び冷凍下においてPET容器に対して良好な易開封性と耐容器付着性を示した。よって、特定の樹脂(A)〜(D)を特定比率で含む本願発明の接着性樹脂組成物は、ポリエステル系樹脂、特にポリエチレンテレフタレート(PET)系樹脂からなる容器向け蓋材用として最適である。
The adhesive compositions of Examples 1 to 9 were excellent in film forming property, and showed good easy-opening property and container adhesion resistance to PET containers at room temperature and freezing. Therefore, the adhesive resin composition of the present invention containing the specific resins (A) to (D) in a specific ratio is most suitable for a lid material for containers made of a polyester resin, particularly a polyethylene terephthalate (PET) resin. ..

Claims (11)

密度が0.88〜0.93g/cmのエチレン−αオレフィン共重合体(A)10〜25質量%、酢酸ビニル含有率が5%以上18%未満のエチレン−酢酸ビニル共重合体(B)20〜45質量%、酢酸ビニル含有率が18%以上30%未満のエチレン−酢酸ビニル共重合体(C)10〜35質量%、粘着付与樹脂(D)25〜35質量%を含有する、接着性樹脂組成物。 Ethylene-α olefin copolymer (A) having a density of 0.88 to 0.93 g / cm 3 by 10 to 25% by mass, and an ethylene-vinyl acetate copolymer (B) having a vinyl acetate content of 5% or more and less than 18%. ) 20 to 45% by mass, 10 to 35% by mass of the ethylene-vinyl acetate copolymer (C) having a vinyl acetate content of 18% or more and less than 30%, and 25 to 35% by mass of the tackifier resin (D). Adhesive resin composition. 前記エチレン−αオレフィン共重合体(A)の示差走査型熱量計により測定した融点が100〜120℃である、請求項1に記載の接着性樹脂組成物。 The adhesive resin composition according to claim 1, wherein the ethylene-α-olefin copolymer (A) has a melting point of 100 to 120 ° C. as measured by a differential scanning calorimeter. 前記酢酸ビニル含有率が5%以上18%未満のエチレン−酢酸ビニル共重合体(B)の示差走査型熱量計により測定した融点が80〜100℃である、請求項1又は2に記載の接着性樹脂組成物。 The adhesion according to claim 1 or 2, wherein the ethylene-vinyl acetate copolymer (B) having a vinyl acetate content of 5% or more and less than 18% has a melting point of 80 to 100 ° C. as measured by a differential scanning calorimeter. Sex resin composition. 前記酢酸ビニル含有率が18%以上30%未満のエチレン−酢酸ビニル共重合体(C)の示差走査型熱量計により測定した融点が60〜90℃である、請求項1〜3いずれか1項に記載の接着性樹脂組成物。 Any one of claims 1 to 3, wherein the ethylene-vinyl acetate copolymer (C) having a vinyl acetate content of 18% or more and less than 30% has a melting point of 60 to 90 ° C. as measured by a differential scanning calorimeter. The adhesive resin composition according to. 前記粘着付与樹脂(D)が脂環族炭化水素樹脂を含む、請求項1〜4いずれか1項に記載の接着性樹脂組成物。 The adhesive resin composition according to any one of claims 1 to 4, wherein the tackifier resin (D) contains an alicyclic hydrocarbon resin. 接着性樹脂組成物のメルトフローレートが10〜25g/10分である、請求項1〜5いずれか1項に記載の接着性樹脂組成物。 The adhesive resin composition according to any one of claims 1 to 5, wherein the melt flow rate of the adhesive resin composition is 10 to 25 g / 10 minutes. 酢酸ビニル含有量が5%以上18%未満のエチレン−酢酸ビニル共重合体(B)及び酢酸ビニル含有量が18%以上30%未満のエチレン−酢酸ビニル共重合体(C)の合計に対する酢酸ビニル含有量が、8%以上9.5%未満である、請求項1〜6いずれか1項に記載の接着性樹脂組成物。 Vinyl acetate with respect to the total of ethylene-vinyl acetate copolymer (B) having a vinyl acetate content of 5% or more and less than 18% and ethylene-vinyl acetate copolymer (C) having a vinyl acetate content of 18% or more and less than 30%. The adhesive resin composition according to any one of claims 1 to 6, wherein the content is 8% or more and less than 9.5%. 基材上に、請求項1〜7いずれか1項に記載の接着性樹脂組成物の膜が積層されたシート。 A sheet in which a film of the adhesive resin composition according to any one of claims 1 to 7 is laminated on a base material. 請求項8に記載のシートにより形成された蓋材。 A lid material formed of the sheet according to claim 8. ポリエステル系樹脂製の容器本体又は内面がポリエステル系樹脂で覆われた容器本体と、請求項9に記載の蓋材とからなる、開封可能な密封容器用部材セット。 An openable sealed container member set comprising a container body made of polyester resin or a container body whose inner surface is covered with polyester resin, and the lid material according to claim 9. ポリエステル系樹脂製の容器本体又は内面がポリエステル系樹脂で覆われた容器本体の開口部が、請求項9に記載の蓋材により密封された、開封可能な容器。 An openable container in which the opening of the container body made of polyester resin or the container body whose inner surface is covered with polyester resin is sealed by the lid material according to claim 9.
JP2019119558A 2019-06-27 2019-06-27 Adhesive resin composition, sheet, lid material, member set for sealed container and container Active JP7240067B2 (en)