JP2012181449A - Pseudo adhesive label - Google Patents

Pseudo adhesive label Download PDF

Info

Publication number
JP2012181449A
JP2012181449A JP2011045520A JP2011045520A JP2012181449A JP 2012181449 A JP2012181449 A JP 2012181449A JP 2011045520 A JP2011045520 A JP 2011045520A JP 2011045520 A JP2011045520 A JP 2011045520A JP 2012181449 A JP2012181449 A JP 2012181449A
Authority
JP
Japan
Prior art keywords
pseudo
line
cut
base material
label
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP2011045520A
Other languages
Japanese (ja)
Other versions
JP5730618B2 (en
Inventor
Daisuke Tomita
大介 冨田
Masaru Matsushima
大 松島
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Lintec Corp
Original Assignee
Lintec Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Lintec Corp filed Critical Lintec Corp
Priority to JP2011045520A priority Critical patent/JP5730618B2/en
Publication of JP2012181449A publication Critical patent/JP2012181449A/en
Application granted granted Critical
Publication of JP5730618B2 publication Critical patent/JP5730618B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

PROBLEM TO BE SOLVED: To provide a pseudo adhesive label which hardly causes tear on a surface substrate at positions other than a separation line when the surface substrate is peeled off from a pseudo adhesive layer and has excellent workability.SOLUTION: A pseudo adhesive label 10 is formed by laminating a surface substrate, a pseudo adhesive layer to be pseudo-bonded to the surface substrate, and a pressure-sensitive adhesive layer in this order. The surface substrate can be peeled off from the pseudo adhesive layer by being divided into label parts 18, 19 along a separation line 20. The separation line 20 is formed by arranging first to third cutting lines 21 to 23 composed of multiple cuts arranged at intervals so that the separation line 20 has a double linear shape. In order to close the interval between the adjacent first cutting lines 21 from both sides, the cuts of the second and third cutting lines 22, 23 are arranged in the vicinity of the interval.

Description

本発明は、物品の搬送や管理等に使用される配送伝票、各種の保険やチケットの申し込み等に使用される記録票等に適用される擬似接着ラベルに関する。   The present invention relates to a pseudo-adhesive label applied to a delivery slip used for transportation and management of articles, a record slip used for application for various insurances and tickets, and the like.

例えば、郵便、宅配便、通信販売などにおいて、商品の受注、発送、顧客の受け取り等からなる流通過程を管理するために、配送伝票等が用いられる。広く用いられる配送伝票の1つとして、感圧紙が複数枚重ね合わされた伝票がある。このような配送伝票では、商品名、送り先等の情報を記入する際、一番下の伝票まで情報を書き込むために、強い圧力を加えなければならず、ボールペン、タイプライター、ドットプリンター等が必要とされる。しかし、ボールペン、タイプライターを用いての書き込みは、煩雑な手作業であり、また誤字、脱字、写し間違いなどによって、誤配送の原因となる。また、ドットプリンターを用いる場合、印字に時間がかかるという欠点がある。さらに、感圧紙が複数枚重ね合わされた配送伝票は、その一部が流通過程で破れたり、剥がれ落ちたりすることもある。   For example, a delivery slip or the like is used in order to manage a distribution process including ordering of goods, shipping, receipt of a customer, etc. in mail, parcel delivery, mail order sales, and the like. As one of widely used delivery slips, there is a slip in which a plurality of pressure sensitive papers are overlapped. In such a delivery slip, when filling in information such as product name and destination, it is necessary to apply a strong pressure to write the information down to the bottom slip, and a ballpoint pen, typewriter, dot printer, etc. are required. It is said. However, writing with a ballpoint pen or a typewriter is a cumbersome manual operation, and causes erroneous delivery due to typographical errors, omissions, or copying errors. In addition, when using a dot printer, there is a drawback that printing takes time. Furthermore, a part of a delivery slip in which a plurality of pressure sensitive papers are stacked may be broken or peeled off during the distribution process.

上記問題点を解決するために、例えば、表面基材、擬似接着層、粘着剤層、及び剥離シートがこの順に積層されてなり、表面基材と擬似接着層との間が剥離可能なように擬似接着された擬似接着ラベルが配送伝票に使用される。擬似接着ラベルは、剥離シートが剥離された後、粘着剤層が配送物に貼付されて、配送伝票として使用される(例えば、特許文献1参照)。   In order to solve the above problems, for example, a surface base material, a pseudo-adhesive layer, a pressure-sensitive adhesive layer, and a release sheet are laminated in this order so that the surface base material and the pseudo-adhesive layer can be peeled off. The pseudo-adhesive label that is pseudo-adhered is used for the delivery slip. The pseudo-adhesive label is used as a delivery slip after the release sheet is peeled off, and an adhesive layer is affixed to the delivery (see, for example, Patent Document 1).

このような擬似接着ラベルの配送伝票には、通常、種々の印刷が施された表面基材の表面にミシン目の切れ目や、連続的な一条の切れ目によって形成された分離線が入れられており、1枚の表面基材が2つのラベル部として分離して剥離可能となっている。そして、例えば、一方のラベル部が配達票として使用されると共に、他方のラベル部が、受領票として使用され、捺印・サイン後に剥がされて持ち帰られ、伝票整理等に使用される。   Such pseudo-adhesive label delivery slips usually have perforations and various lines formed on the surface of the surface substrate on which various types of printing have been applied. One surface base material can be separated and separated as two label portions. For example, one label portion is used as a delivery slip, the other label portion is used as a receipt slip, peeled off after stamping / signing, and taken home, and used for slip arrangement.

擬似接着ラベルを用いれば、郵便、宅配便、通信販売などにおいて商品の受注から顧客の受け取りまで1枚のシートで流通過程を管理することが可能であり、さらに流通過程における伝票の破れや紛失等も防止することができる。また、レーザープリンター、熱転写等による情報の書き込みが可能であるため、記入が迅速に行えると共に、誤字・脱字等も低減させることができる。   By using pseudo-adhesive labels, it is possible to manage the distribution process with a single sheet from the order of goods to the receipt of customers in mail, courier, mail order, etc. Furthermore, slips and loss of slips in the distribution process, etc. Can also be prevented. In addition, since information can be written by laser printer, thermal transfer, etc., it is possible to fill in quickly and to reduce typographical errors and omissions.

特公昭55−15035号公報Japanese Patent Publication No.55-15035

しかし、擬似接着ラベルにおいて分離線がミシン目の場合には、ミシン目で一方のラベル部を切り離すことができずに表面基材が破れるおそれがある。特に、表面基材は紙の流れ方向やフィルムの延伸方向に沿って破れやすいため、ミシン目が流れ方向や延伸方向に対して垂直に形成されている場合には、表面基材がより破れやすくなる。   However, when the separation line is perforated in the pseudo-adhesive label, one surface of the label cannot be separated by the perforation, and the surface base material may be broken. In particular, since the surface substrate is easily broken along the paper flow direction and the film stretching direction, the surface substrate is more easily broken when the perforation is formed perpendicular to the flow direction and the stretching direction. Become.

一方、分離線が一条の切れ目によって構成される場合には、表面基材の破れは発生しにくいが、擬似接着ラベルを剥離シートから剥離した際、ラベルが分離線で折れ曲がりやすく、作業性が悪いという問題がある。また、一条の切れ目の場合には、剥離シートから剥離された擬似接着ラベルが切れ目によって分断されないように、切れ目は、擬似接着層や粘着剤層には切り込まず、表面基材のみを切り込んで形成する必要がある。しかし、このような切れ目は、切込の制御が難しく、所望の深さに切込を入れることが難しいという加工上の問題がある。   On the other hand, when the separation line is constituted by a single cut, the surface base material is not easily torn, but when the pseudo-adhesive label is peeled from the release sheet, the label is easily bent at the separation line and the workability is poor. There is a problem. In the case of a single cut, the cut is not cut into the pseudo-adhesive layer or the pressure-sensitive adhesive layer so that the pseudo-adhesive label peeled off from the release sheet is not divided by the cut, but only the surface base material is cut. Need to form. However, such a cut has a processing problem that it is difficult to control the cut and it is difficult to make a cut at a desired depth.

そこで、本発明は、表面基材を分離線で分離して剥離する際に、分離線以外の箇所で表面基材に破れが発生することなく、更に擬似接着ラベルが分離線で折れ曲がることなく作業性の良い擬似接着ラベルを提供することを目的とする。   Therefore, when separating the surface substrate with a separation line and peeling it, the present invention does not cause the surface substrate to be broken at a place other than the separation line, and further, the pseudo-adhesive label does not bend at the separation line. An object of the present invention is to provide a pseudo adhesive label having good properties.

本発明は上記課題を解決するためになされたものであり、本発明に係る擬似接着ラベルは、表面基材と、表面基材に擬似接着される擬似接着層と、粘着剤層とがこの順に積層された積層構造を備え、粘着剤層が被着物に貼着された状態で、表面基材を擬似接着層から剥離可能な擬似接着ラベルであって、表面基材は、少なくとも2以上のラベル部に分離して擬似接着層から剥離可能とする分離線を備え、分離線は、複数の切れ目が間隔をおいて形成された断裁線が、少なくとも2本近接して並べられて複線状となり、上記少なくとも2本の断裁線のうちの1本の断裁線の間隔を塞ぐように、その間隔の近傍に他の1本の断裁線の切れ目が配置されることを特徴とする。   The present invention has been made to solve the above problems, and the pseudo-adhesive label according to the present invention comprises a surface base material, a pseudo-adhesion layer pseudo-adhered to the surface base material, and an adhesive layer in this order. A pseudo-adhesive label having a laminated structure and having a pressure-sensitive adhesive layer attached to an adherend and capable of peeling the surface substrate from the pseudo-adhesive layer, wherein the surface substrate has at least two or more labels It is provided with a separation line that can be separated into a part and can be peeled off from the pseudo-adhesive layer, and the separation line has a plurality of cut lines formed at intervals, and is arranged in a double line shape by arranging at least two adjacent lines, Another cut line break is arranged in the vicinity of the interval so as to close the interval between one of the at least two cut lines.

分離線が、断裁線が少なくとも3本近接して並べられて複線状となる場合、上記1本の断裁線の間隔を両側から塞ぐように、他の2本の断裁線の切れ目が配置されることが好ましい。   In the case where the separation line is formed in a double-line shape by arranging at least three cutting lines close to each other, the cut line of the other two cutting lines is arranged so as to close the interval of the one cutting line from both sides. It is preferable.

上記1本の断裁線の各切れ目は、直線状であることが好ましい。また、断裁線のうち上記他の1本又は2本の断裁線の各切れ目は、直線状、あるいは両端が上記1本の断裁線に近づくように傾斜した線状であることが好ましい。   Each cut line of the one cutting line is preferably linear. Moreover, it is preferable that each cut | interruption of said other 1 or 2 cutting line is a linear form or the linear form which inclined so that both ends may approach said 1 cutting line among cutting lines.

本発明では、表面基材を分離線で分離して剥離する際に、分離線以外の箇所で表面基材に破れが発生することなく、更にラベルが分離線で折れ曲がることがなく作業性の良い擬似接着ラベルを提供することができる。   In the present invention, when the surface substrate is separated and separated by the separation line, the surface substrate is not torn at a place other than the separation line, and the label is not bent by the separation line, and the workability is good. A pseudo-adhesive label can be provided.

本発明の第1実施形態に係る擬似接着ラベルを模式的に示す断面図である。It is sectional drawing which shows typically the pseudo | simulation adhesive label which concerns on 1st Embodiment of this invention. 本発明の第1実施形態に係る擬似接着ラベルを模式的に示す平面図である。It is a top view showing typically the pseudoadhesive label concerning a 1st embodiment of the present invention. 本発明の第1実施形態に係る擬似接着ラベルの分離線の部分拡大図である。It is the elements on larger scale of the separation line of the pseudo-adhesive label which concerns on 1st Embodiment of this invention. 本発明の第2実施形態に係る擬似接着ラベルの分離線の部分拡大図である。It is the elements on larger scale of the separation line of the pseudo-adhesive label which concerns on 2nd Embodiment of this invention. 本発明の第3実施形態に係る擬似接着ラベルの分離線の部分拡大図である。It is the elements on larger scale of the separation line of the pseudo-adhesive label which concerns on 3rd Embodiment of this invention. 本発明の第3実施形態に係る擬似接着ラベルの分離線の変形例を示す部分拡大図である。It is the elements on larger scale showing the modification of the separation line of the pseudoadhesive label concerning a 3rd embodiment of the present invention.

以下、図面を参照しつつ本発明の実施形態について説明する。
本発明の第1実施形態に係る擬似接着ラベルを図1〜3を用いて説明する。図1は、本発明の第1実施形態に係る擬似接着ラベルを模式的に示す断面図である。
Hereinafter, embodiments of the present invention will be described with reference to the drawings.
The pseudo-adhesive label according to the first embodiment of the present invention will be described with reference to FIGS. FIG. 1 is a cross-sectional view schematically showing a pseudo-adhesive label according to the first embodiment of the present invention.

図1に示すように、本発明の第1実施形態に係る擬似接着ラベル10は、表面基材11、表面基材11に擬似接着される擬似接着層12、擬似接着層12に接着された粘着剤層13がこの順に積層された積層構造を備え、更に、剥離基材14が粘着剤層13に貼着されている。擬似接着ラベル10は、剥離基材14が粘着剤層13から剥離され、露出した粘着剤層13によって、被着物(図示せず)に貼着されて使用される。   As shown in FIG. 1, a pseudo-adhesive label 10 according to the first embodiment of the present invention includes a surface base material 11, a pseudo-adhesion layer 12 that is pseudo-adhered to the surface base material 11, and an adhesive that is adhered to the pseudo-adhesion layer 12. The adhesive layer 13 has a laminated structure in which the layers are laminated in this order, and the release substrate 14 is attached to the pressure-sensitive adhesive layer 13. The pseudo-adhesive label 10 is used after the release substrate 14 is peeled off from the pressure-sensitive adhesive layer 13 and is adhered to an adherend (not shown) by the exposed pressure-sensitive adhesive layer 13.

擬似接着層12は、表面基材11に剥離可能に擬似接着されており、ラベル10が被着物に貼着された状態で、表面基材11が擬似接着層12から剥離される。擬似接着ラベル10には、表面基材11の表面から多数の切れ目31〜33が切り込まれており、後述するように、切れ目31〜33によって分離線20(図2参照)が構成される。切れ目31〜33は、図1に示すように、表面基材11の表面から切り込まれて、表面基材11、擬似接着層12、及び粘着剤層13を貫通するものである。ただし、切れ目31〜33は、表面基材11の裏面まで貫通していれば、擬似接着層12及び粘着剤層13は切り込まれていなくても良い。   The pseudo-adhesion layer 12 is pseudo-adhered to the surface base material 11 so as to be peeled off, and the surface base material 11 is peeled from the pseudo-adhesion layer 12 in a state where the label 10 is attached to the adherend. In the pseudo-adhesive label 10, a large number of cuts 31 to 33 are cut from the surface of the surface base material 11, and a separation line 20 (see FIG. 2) is formed by the cuts 31 to 33 as described later. As shown in FIG. 1, the cuts 31 to 33 are cut from the surface of the surface base material 11 and penetrate the surface base material 11, the pseudo adhesive layer 12, and the pressure-sensitive adhesive layer 13. However, if the cut lines 31 to 33 penetrate to the back surface of the surface base material 11, the pseudo adhesive layer 12 and the pressure-sensitive adhesive layer 13 do not need to be cut.

表面基材11としては、例えば上質紙、熱転写用紙、クラフト紙、グラシン紙、感熱紙、合成紙、又はプラスティックフィルムが使用される。表面基材11の厚みは、例えば15〜120μm、好ましくは20〜110μmであり、更に好ましくは30〜100μmである。表面基材11の表面は、例えば文字等の情報が表示されるための面に使用される。   As the surface base material 11, for example, high-quality paper, thermal transfer paper, craft paper, glassine paper, thermal paper, synthetic paper, or plastic film is used. The thickness of the surface base material 11 is 15-120 micrometers, for example, Preferably it is 20-110 micrometers, More preferably, it is 30-100 micrometers. The surface of the surface substrate 11 is used as a surface for displaying information such as characters.

擬似接着層12は、表面基材11に剥離可能に擬似接着されるものであれば、特に限定されないが、熱可塑性樹脂層であることが好ましい。熱可塑性樹脂層は、例えば、加熱溶融された熱可塑性樹脂が表面基材11の裏面に押出積層されることにより形成される。熱可塑性樹脂層を形成するための熱可塑性樹脂としては、例えば、ポリエチレン、ポリプロピレン、ポリメチルペンテン等が単独で又は2種類以上混合されて使用される。熱可塑性樹脂層の厚さは、特に限定されないが、例えば3〜70μm、好ましくは5〜50μmである。   The pseudo adhesive layer 12 is not particularly limited as long as it is pseudo-adhered to the surface substrate 11 so as to be peeled off, but is preferably a thermoplastic resin layer. The thermoplastic resin layer is formed, for example, by extrusion laminating a heat-melted thermoplastic resin on the back surface of the surface base material 11. As the thermoplastic resin for forming the thermoplastic resin layer, for example, polyethylene, polypropylene, polymethylpentene and the like are used alone or in admixture of two or more. Although the thickness of a thermoplastic resin layer is not specifically limited, For example, it is 3-70 micrometers, Preferably it is 5-50 micrometers.

表面基材11の裏面には、擬似接着層12から表面基材11を容易に剥離できるように、離型剤層が被膜されていても良い。離型剤層は、特に限定されないが、スチレン−アクリル共重合体、ポリスチレン、スチレン−ブタジエン共重合体、エチレン酢酸ビニル共重合体、アクリル酸エステル、アクリル酸エステル共重合体、エチレン・アクリル酸共重合体などからなる離型剤によって形成される。なお、表面基材11は、離型剤層が設けられる場合には、擬似接着層12と離型剤層との界面で剥離される。また、表面基材11は、その裏面にさらに上記熱可塑性樹脂で形成された熱可塑性樹脂層と、離型剤層とがこの順に設けられたものであっても良い。   A release agent layer may be coated on the back surface of the surface base material 11 so that the surface base material 11 can be easily peeled off from the pseudo adhesive layer 12. The release agent layer is not particularly limited, but styrene-acrylic copolymer, polystyrene, styrene-butadiene copolymer, ethylene vinyl acetate copolymer, acrylic acid ester, acrylic acid ester copolymer, ethylene / acrylic acid copolymer. It is formed by a mold release agent made of a polymer or the like. In addition, the surface base material 11 peels in the interface of the pseudo adhesion layer 12 and a mold release agent layer, when a mold release agent layer is provided. Moreover, the surface base material 11 may be further provided with a thermoplastic resin layer formed of the thermoplastic resin and a release agent layer in this order on the back surface.

粘着剤層13は、擬似接着層12の裏面側に設けられ、擬似接着ラベル10を被着物に粘着させるための層であって、アクリル系粘着剤、天然ゴム系粘着剤、合成ゴム系粘着剤、シリコーン系粘着剤等の従来公知の粘着剤から形成される。粘着剤層13の厚さは、特に限定されないが、例えば5〜50μm、好ましくは10〜40μmである。剥離基材14は、粘着剤層13に貼着されるための表面がシリコーン系剥離剤等によって離型処理された剥離シート等である。   The pressure-sensitive adhesive layer 13 is provided on the back side of the pseudo-adhesive layer 12 and is a layer for adhering the pseudo-adhesive label 10 to an adherend, and is an acrylic pressure-sensitive adhesive, natural rubber-based pressure-sensitive adhesive, and synthetic rubber-based pressure-sensitive adhesive. It is formed from a conventionally known adhesive such as a silicone-based adhesive. Although the thickness of the adhesive layer 13 is not specifically limited, For example, 5-50 micrometers, Preferably it is 10-40 micrometers. The release substrate 14 is a release sheet or the like whose surface to be attached to the pressure-sensitive adhesive layer 13 is subjected to a release treatment with a silicone release agent or the like.

粘着剤層13は、例えば、剥離基材14に粘着剤が塗布されて形成される。そして、その剥離基材14の上に形成された粘着剤層13に、表面基材11に積層された擬似接着層12が貼り合わされることにより、擬似接着ラベル10が得られる。但し、粘着剤層13は、表面基材11に積層されている擬似接着層12の上に直接塗布して形成され、その上に剥離基材14が貼り合わされて擬似接着ラベル10が形成されても良い。   The pressure-sensitive adhesive layer 13 is formed, for example, by applying a pressure-sensitive adhesive to the peeling substrate 14. And the pseudoadhesion label 10 is obtained by bonding the pseudoadhesion layer 12 laminated | stacked on the surface base material 11 to the adhesive layer 13 formed on the peeling base material 14 together. However, the pressure-sensitive adhesive layer 13 is formed by directly coating the pseudo-adhesive layer 12 laminated on the surface base material 11, and the pseudo-adhesive label 10 is formed by pasting the release base material 14 thereon. Also good.

図2は第1実施形態に係る擬似接着ラベル10を模式的に示す平面図であり、図3は図2の分離線20の部分拡大図である。擬似接着ラベル10は、打ち抜き加工が施されることにより、表面基材11、擬似接着層12、及び粘着剤層13が打ち抜き切断された後、カス上げによって不要部分が剥離基材14から取り除かれ、下辺10A及び上辺10Bを長辺とし、左右の側辺10C、10Dを短辺とする略矩形のラベルに形成される。擬似接着ラベル10は、打ち抜き加工と共に略中央部にミシン目加工が施され、表面基材11の略中央部に分離線20が形成される。打ち抜き加工及びミシン目加工は、例えば、ダイカッタが用いられて行われるが、レーザー照射等によって行われても良い。   FIG. 2 is a plan view schematically showing the pseudo-adhesive label 10 according to the first embodiment, and FIG. 3 is a partially enlarged view of the separation line 20 of FIG. The pseudo-adhesive label 10 is punched, whereby the surface base material 11, the pseudo-adhesive layer 12, and the pressure-sensitive adhesive layer 13 are punched and cut, and then unnecessary portions are removed from the release base material 14 by scraping. The lower side 10A and the upper side 10B are long sides and the left and right side sides 10C and 10D are short sides. The pseudo-adhesive label 10 is perforated at a substantially central portion together with the punching process, and a separation line 20 is formed at a substantially central portion of the surface base material 11. The punching and perforation are performed using, for example, a die cutter, but may be performed by laser irradiation or the like.

図2に示すように、分離線20は、表面基材11の下辺10Aから上辺10Bまで直線的に縦方向に延在する。表面基材11は、分離線20によって右左の矩形シート(これらをラベル部18、19という)に分離して擬似接着層12から剥離可能である。   As shown in FIG. 2, the separation line 20 extends linearly in the vertical direction from the lower side 10 </ b> A to the upper side 10 </ b> B of the surface base material 11. The surface base material 11 can be separated from the pseudo-adhesive layer 12 by separating it into right and left rectangular sheets (referred to as label portions 18 and 19) by a separation line 20.

分離線20は、第1〜第3の断裁線21、22、23が、近接して横方向に並べられて形成され複線状となる。図3に示すように、第1の断裁線21は、縦方向(すなわち、分離線20に沿う方向)に平行な直線状の切れ目31が、縦方向に間隔34をおいて複数並べられて形成されたものであり、縦方向に平行なミシン目状の直線となる。同様に、第2及び第3の断裁線22、23はそれぞれ、縦方向に平行な直線状の切れ目32、33それぞれが、縦方向に間隔35、36をおいて複数並べられて形成されたものであり、縦方向に平行なミシン目状の直線となる。第2及び第3の断裁線22、23は、第1の断裁線21を両側から挟み込むように配置される。   The separation line 20 has a double-line shape in which the first to third cutting lines 21, 22, and 23 are formed adjacently and arranged in the horizontal direction. As shown in FIG. 3, the first cutting line 21 is formed by arranging a plurality of linear cuts 31 parallel to the vertical direction (that is, the direction along the separation line 20) at intervals 34 in the vertical direction. It becomes a perforated straight line parallel to the vertical direction. Similarly, the second and third cutting lines 22 and 23 are each formed by arranging a plurality of straight cuts 32 and 33 parallel to the vertical direction at intervals 35 and 36 in the vertical direction. It becomes a perforated straight line parallel to the vertical direction. The 2nd and 3rd cutting lines 22 and 23 are arranged so that the 1st cutting line 21 may be inserted from both sides.

第1の断裁線21の切れ目31は、下辺10Aから上辺10Bまで間隔34をおいて連続的に設けられる。そして、第1の断裁線21の最下端及び最上端に配置された切れ目31、31は、表面基材11の外縁である下辺10A及び上辺10Bに接続される。   The cut line 31 of the first cutting line 21 is continuously provided at an interval 34 from the lower side 10A to the upper side 10B. And the cut | disconnections 31 and 31 arrange | positioned at the lowermost end and the uppermost end of the 1st cutting line 21 are connected to the lower edge | side 10A and the upper edge | side 10B which are the outer edges of the surface base material 11. FIG.

第2及び第3の断裁線22、23それぞれにおいて、切れ目32、33は、間隔34に対応する数設けられる。各切れ目32、33は、第1の断裁線21の間隔34それぞれの近傍において間隔34を中心に対称的に、各間隔34を両側から塞ぐように配置される。つまり、各切れ目32、33は、その長さL2、L3が間隔34の長さD1よりも長くなる。そして、各切れ目32、33は、隣接する2本の切れ目31、31の上側の切れ目31の下端部、及び下側の切れ目31の上端部に、縦方向においてオーバーラップするように配置される。   In each of the second and third cutting lines 22 and 23, the cut lines 32 and 33 are provided in a number corresponding to the interval 34. Each of the cut lines 32 and 33 is disposed in the vicinity of each of the intervals 34 of the first cutting line 21 so as to be symmetrical with respect to the interval 34 so as to close the intervals 34 from both sides. That is, the lengths L2 and L3 of the cut lines 32 and 33 are longer than the length D1 of the interval 34. And each cut | interruption 32 and 33 is arrange | positioned so that it may overlap in the vertical direction at the lower end part of the upper cut 31 of the adjacent two cuts 31 and 31, and the upper end part of the lower cut 31. FIG.

本実施形態では、切れ目32、33の長さL2、L3が、間隔34の長さD1より長く、切れ目32、33が間隔34を確実に塞ぐため、後述するように、切れ目31の端部を起点とする表面基材11の横方向への破れが確実に防止される。なお、長さL2、L3は、例えば、0.2〜5mm、好ましくは0.3〜3mmである。   In the present embodiment, the lengths L2 and L3 of the cuts 32 and 33 are longer than the length D1 of the interval 34, and the cuts 32 and 33 reliably block the interval 34. Breaking in the lateral direction of the surface base material 11 as a starting point is reliably prevented. In addition, length L2, L3 is 0.2-5 mm, for example, Preferably it is 0.3-3 mm.

第1の断裁線21の各切れ目31の長さL1は、間隔34の長さD1や、切れ目32、33の長さL2、L3よりも長くなることが好ましい。長さL1が長さD1、L2、L3より短くなると、第1の断裁線21に沿って表面基材11が分離されにくくなり、破れが生じやすくなる。   The length L1 of each cut 31 of the first cutting line 21 is preferably longer than the length D1 of the interval 34 and the lengths L2 and L3 of the cuts 32 and 33. When the length L1 is shorter than the lengths D1, L2, and L3, the surface base material 11 becomes difficult to be separated along the first cutting line 21, and breakage is likely to occur.

本実施形態では、切れ目31の長さL1は、例えば0.3〜15mm、好ましくは0.4〜10mmであるとともに、長さL1に対する長さD1の比D1/L1は、例えば1/10〜2/3、好ましくは1/5〜1/2である。また、間隔34の長さD1は、例えば、0.1〜1.5mm、好ましくは0.2〜1.0mmである。長さL1が上記範囲より長くなり、あるいは、比D1/L1がこれら範囲未満となると、擬似接着ラベル10は、剥離基材14が取り除かれた後、分離線20で折れ曲がりやすくなる。また、長さL1が上記範囲より短くなり、あるいは、D1/L1がこれら範囲より大きくなると、ラベル部を剥離する際、第1の断裁線21に沿って表面基材11が分離されにくくなり、破れが生じやすくなる。   In the present embodiment, the length L1 of the cut 31 is, for example, 0.3 to 15 mm, preferably 0.4 to 10 mm, and the ratio D1 / L1 of the length D1 to the length L1 is, for example, 1/10 to 10/10. 2/3, preferably 1/5 to 1/2. Moreover, the length D1 of the space | interval 34 is 0.1-1.5 mm, for example, Preferably it is 0.2-1.0 mm. When the length L1 is longer than the above range or the ratio D1 / L1 is less than these ranges, the pseudo-adhesive label 10 is easily bent at the separation line 20 after the release substrate 14 is removed. Further, when the length L1 is shorter than the above range, or when D1 / L1 is larger than these ranges, the surface base material 11 is hardly separated along the first cutting line 21 when peeling the label portion, It is easy to break.

さらに、切れ目32、33の上端又は下端と、切れ目31との離間距離E1は、例えば0.1〜2mm、好ましくは0.2〜1.5mmである。離間距離E1が長すぎると、後述するように、一旦表面基材の破断が第2ないし第3の断裁線22、23に進んだ後、第1の断裁線21に戻りにくくなる。一方、離間距離E1が短すぎると、上記したような擬似接着ラベルの折れ曲がりが発生しやすくなる。   Furthermore, the separation distance E1 between the upper end or lower end of the cut lines 32 and 33 and the cut line 31 is, for example, 0.1 to 2 mm, preferably 0.2 to 1.5 mm. If the separation distance E1 is too long, it will be difficult to return to the first cutting line 21 after the surface base material breakage once proceeds to the second to third cutting lines 22 and 23, as will be described later. On the other hand, when the separation distance E1 is too short, the above-described pseudo adhesive label is likely to be bent.

次に、疑似接着ラベル10における表面基材11の剥離方法について説明する。表面基材11のラベル部18の切り離しは、例えば、下辺10Aと分離線20が交差するラベル部18の角部18Aを剥離開始部として摘まんで、表面基材11を剥離方向Aに引き剥がすことにより行われる。このとき、ラベル部18は、ラベル部19側を残すように、分離線20に沿って表面基材11を断裁しつつ擬似接着層12から剥離される。   Next, the peeling method of the surface base material 11 in the pseudo adhesive label 10 is demonstrated. The label part 18 of the surface base material 11 is separated by, for example, picking the corner part 18A of the label part 18 where the lower side 10A intersects the separation line 20 as a peeling start part and peeling the surface base material 11 in the peeling direction A. Is done. At this time, the label portion 18 is peeled from the pseudo adhesive layer 12 while cutting the surface base material 11 along the separation line 20 so as to leave the label portion 19 side.

第1の裁断線21における最下端の切れ目31は、下辺10Aに接続され、したがって剥離方向Aにラベル部18が引き剥がされると、ラベル部18の剥離が、第1の裁断線21の切れ目31に沿って開始される。ここで、剥離方向Aは分離線20に対して斜め方向であるため、ラベル部18の破断は、切れ目31の上端から縦方向に進み、間隔34を介して、次の切れ目31に進むこともあるが、切れ目31の上端から横方向へ進むこともある。   The lowermost cut line 31 in the first cutting line 21 is connected to the lower side 10A. Therefore, when the label part 18 is peeled off in the peeling direction A, the peeling of the label part 18 causes the cut 31 of the first cutting line 21. Will start along. Here, since the peeling direction A is an oblique direction with respect to the separation line 20, the break of the label portion 18 proceeds in the vertical direction from the upper end of the cut line 31, and may proceed to the next cut line 31 via the interval 34. There is a case where it proceeds in the horizontal direction from the upper end of the cut 31.

本実施形態では、この切れ目31の上端から横方向へ進む破断は、ラベル部18側から間隔34を塞ぐように配置された、第2の裁断線22の切れ目32により止められる。すなわち、切れ目31の上端から横方向に破断しても、その破断は、切れ目31の上端に隣接する切れ目32に進み、ラベル部18の剥離は、その切れ目32に沿って再び縦方向に進むこととなる。そして、ラベル部18の剥離は、その切れ目32の上端まで進むと、その上端から隣接する次の切れ目31に戻ることとなる。このように本実施形態では、切れ目31の上端から表面基材11の破断が一旦横方向に進んでも、ラベル部18の剥離は、第1の破断線21の切れ目31を順次進むこととなり、ラベル部18が横方向に大きく破れることが防止される。勿論、分離線20と上辺10Bが交差する位置にあるラベル部18の角部18Bからラベル部18が剥がされる場合も同様の作用により破れが防止される。   In the present embodiment, the break that proceeds in the lateral direction from the upper end of the cut line 31 is stopped by the cut line 32 of the second cutting line 22 arranged so as to close the interval 34 from the label part 18 side. That is, even when the cut 31 is broken laterally from the upper end, the breakage proceeds to the cut 32 adjacent to the upper end of the cut 31, and the peeling of the label portion 18 proceeds again along the cut 32 in the vertical direction. It becomes. Then, when the peeling of the label portion 18 proceeds to the upper end of the cut 32, the label portion 18 returns from the upper end to the next adjacent cut 31. As described above, in the present embodiment, even if the breaking of the surface base material 11 once proceeds in the horizontal direction from the upper end of the cut line 31, the separation of the label portion 18 proceeds in the cut line 31 of the first break line 21 in sequence. The portion 18 is prevented from being greatly broken in the lateral direction. Of course, when the label portion 18 is peeled off from the corner portion 18B of the label portion 18 at the position where the separation line 20 and the upper side 10B intersect, tearing is prevented by the same action.

なお、以上の説明では、2つのラベル部のうち、ラベル部18が先に剥離されるときの動作について説明したが、ラベル部19が、その角部19A、19Bを剥離開始部として、先に剥離される際にも同様の作用により第3の破断線23の切れ目33によってラベル部19の破れが防止される。さらに、一方のラベル部が剥がされた後、残ったラベル部は、擬似接着層12から適宜剥離される。   In the above description, of the two label portions, the operation when the label portion 18 is peeled first has been described. However, the label portion 19 has the corner portions 19A and 19B as peeling start portions, Even when peeled off, the label portion 19 is prevented from being broken by the cut 33 of the third break line 23 by the same action. Further, after the one label portion is peeled off, the remaining label portion is appropriately peeled off from the pseudo adhesive layer 12.

以上のように、本実施形態では、ミシン目状の破断線21〜23が複線状に設けられたため、分離線20に沿ってラベル部18、19が分離して剥離される際、表面基材11に破れが発生しにくくなる。また、各破断線21〜23は、ミシン目状であるため、剥離基材11から剥離した擬似接着ラベルは、分離線20において折り曲がりにくく、擬似接着ラベルを被着体に貼着する際の作業性が良好となる。   As described above, in this embodiment, since the perforated break lines 21 to 23 are provided in a double line shape, when the label portions 18 and 19 are separated and peeled along the separation line 20, the surface base material 11 is hard to break. Moreover, since each broken line 21-23 is perforated, the pseudo-adhesive label peeled off from the peeling base material 11 is hard to bend | fold at the separation line 20, and when sticking a pseudo-adhesive label to a to-be-adhered body. Workability is improved.

また、ラベル部18、19は分離線20に沿って容易に縦方向に切れるため、分離線20が流れ方向やフィルムの延伸方向に対して垂直に形成されている場合であっても表面基材11が破れにくくなる。   Further, since the label portions 18 and 19 are easily cut in the longitudinal direction along the separation line 20, even if the separation line 20 is formed perpendicular to the flow direction or the film stretching direction, the surface base material 11 becomes difficult to tear.

なお、本実施形態では、表面基材11等にマーク等が付されて、例えば、角部18Aがラベル部18の剥離開始部であることが示されていても良い。   In the present embodiment, a mark or the like may be attached to the surface base material 11 or the like, for example, to indicate that the corner portion 18A is a peeling start portion of the label portion 18.

さらに、マーク等が付されて、剥離開始部の位置が予め定められている場合には、第1の断裁線21における最上端及び最下端の切れ目31のいずれか一方は、表面基材11の外縁(すなわち、上辺10B又は下辺10A)に接続しなくても良い。例えば、角部18Aや角部19Aが剥離開始部と予め定められている場合には、角部18Bや角部19Bから剥離を開始しやすくする必要はないので、第1の断裁線21の最上端における切れ目31は、上辺10Bに接続しなくても良い。   Further, when a mark or the like is added and the position of the peeling start portion is determined in advance, one of the uppermost end and the lowermost cut 31 in the first cutting line 21 is formed on the surface base material 11. It is not necessary to connect to the outer edge (that is, the upper side 10B or the lower side 10A). For example, when the corner 18A or the corner 19A is predetermined as the peeling start portion, it is not necessary to easily start the peeling from the corner 18B or the corner 19B. The cut line 31 at the upper end may not be connected to the upper side 10B.

図4は、本発明の第2の実施形態に係る分離線を示す。第2の実施形態は、第2及び第3の断裁線における切れ目の形状を除いて、第1の実施形態と同様である。以下、第2の実施形態について、第1の実施形態との相違点を説明する。なお、以下の説明では、第1の実施形態と同一の構成を有する部材については、同一の符号を付す。   FIG. 4 shows a separation line according to the second embodiment of the present invention. The second embodiment is the same as the first embodiment except for the shape of the cut line in the second and third cutting lines. Hereinafter, the difference between the second embodiment and the first embodiment will be described. In the following description, members having the same configuration as those of the first embodiment are denoted by the same reference numerals.

第2の実施形態では、第2及び第3の断裁線42、43における切れ目52、53は、両端が第1の断裁線21に近づくように傾斜した線状となっている。具体的には、切れ目52、53は、縦方向(分離線20に沿う方向)に対して傾斜する2本の同じ長さの直線部が連接して成る「く」の字状の切れ目である。各切れ目52、53は、縦方向における長さL5、L6が、第1の断裁線31の間隔34の長さD1より長くなっており、両側から間隔34を塞ぐように配置される。なお、本実施形態において、切れ目52、53の長さL5、L6、及び、切れ目52、53の上端又は下端と切れ目31との離間距離E2は、第1の実施形態における長さL2、L3及び離間距離E1と同様であるので、その説明は省略する。   In the second embodiment, the cut lines 52 and 53 in the second and third cutting lines 42 and 43 are linearly inclined so that both ends approach the first cutting line 21. Specifically, the cuts 52 and 53 are “<” shaped cuts formed by connecting two straight portions having the same length that are inclined with respect to the vertical direction (the direction along the separation line 20). . The cut lines 52 and 53 have lengths L5 and L6 in the vertical direction longer than the length D1 of the interval 34 of the first cutting line 31, and are arranged so as to close the interval 34 from both sides. In the present embodiment, the lengths L5 and L6 of the cuts 52 and 53, and the separation distance E2 between the upper end or the lower end of the cuts 52 and 53 and the cut 31 are the lengths L2 and L3 in the first embodiment. Since it is the same as the separation distance E1, its description is omitted.

切れ目52は、その両端が、横方向において同じ位置に配置される。したがって、第2の断裁線42における全ての切れ目52の両端を結んだ仮想線α1は、縦方向に延在する直線状となる。第3の断裁線43においても同様に、切れ目53の両端を結んだ仮想線α2は、縦方向に延在する直線状となる。すなわち、第2及び第3の断裁線42、43はそれぞれ、複数の切れ目52、53が間隔55、56をおいて、縦方向に直線的に並べられたものである。   Both ends of the cut 52 are arranged at the same position in the lateral direction. Therefore, the imaginary line α1 connecting both ends of all the cut lines 52 in the second cutting line 42 is a straight line extending in the vertical direction. Similarly, in the third cutting line 43, the virtual line α2 connecting both ends of the cut 53 is a straight line extending in the vertical direction. That is, each of the second and third cutting lines 42 and 43 is formed by linearly arranging a plurality of cut lines 52 and 53 at intervals 55 and 56 in the vertical direction.

本実施形態では、切れ目52、53は、両端が第1の断裁線21に近づくように傾斜しているため、表面基材11の破断が一旦、第1の断裁線21の切れ目31から切れ目52、53に進んでも、その破断は、切れ目52、53から、切れ目31に戻りやすくなり、表面基材11の破れがより防止されやすくなる。   In the present embodiment, since the cut lines 52 and 53 are inclined so that both ends approach the first cutting line 21, the surface base material 11 is once broken from the cutting line 31 to the cutting line 52 of the first cutting line 21. , 53, the breakage easily returns from the cuts 52, 53 to the cut 31, and the surface base material 11 is more easily prevented from being broken.

なお、第2の実施形態では、切れ目52、53は、両端が第1の断裁線21に近づくように傾斜しているものであれば、他の形状であっても良く、例えば曲線状であっても良い。勿論、第2及び第3の断裁線の切れ目は、表面基材11の横方向への破断を防止できるものであれば上記したものに限定されず、他の形状であっても良い。   In the second embodiment, the cut lines 52 and 53 may have other shapes as long as both ends are inclined so as to approach the first cutting line 21. For example, the cut lines 52 and 53 are curved. May be. Of course, the cut lines of the second and third cutting lines are not limited to those described above as long as they can prevent the surface base material 11 from being broken in the lateral direction, and may have other shapes.

図5は、第3の実施形態における分離線を示す拡大平面図である。以下、本実施形態について第1の実施形態との相違点を説明する。第3の実施形態では、第3の破断線が省略されており、分離線60は、2本の破断線(第1及び第2の断裁線21、22)によって複線状に形成される。そのため、第1の破断線21の間隔34は、一方のラベル部18側から切れ目32によって塞がれるが、他方のラベル部19側からは切れ目によって塞がれない。   FIG. 5 is an enlarged plan view showing a separation line in the third embodiment. Hereinafter, differences of the present embodiment from the first embodiment will be described. In the third embodiment, the third break line is omitted, and the separation line 60 is formed in a double-line shape by two break lines (first and second cutting lines 21 and 22). Therefore, the interval 34 of the first breaking line 21 is closed by the cut 32 from the one label portion 18 side, but is not closed by the cut from the other label portion 19 side.

したがって、2つのラベル部のうち、切れ目によって間隔34が塞がれていないラベル部19側から先に剥離されると、横方向の破断が切れ目によって防止されにくくなるので、表面基材11に破れが生じやすくなる。そのため、本実施形態では、擬似接着ラベルは、2つのラベル部のうち、ラベル部18が先に剥離されるように設計されることが好ましい。例えば、擬似接着ラベルが配送伝票に使用される場合、ラベル部18が受領票とされ、ラベル部19が配達票とされることが好ましい。また、ラベル部18を先に剥離すべきであることが、表面基材等に表示されても良い。   Accordingly, if the gap 34 is peeled off first from the side of the label portion 19 where the gap 34 is not blocked by the cut, the lateral break is difficult to be prevented by the cut, and the surface base material 11 is broken. Is likely to occur. Therefore, in this embodiment, it is preferable that the pseudo-adhesive label is designed so that the label portion 18 of the two label portions is peeled first. For example, when a pseudo-adhesive label is used for a delivery slip, it is preferable that the label portion 18 is a receipt slip and the label portion 19 is a delivery slip. Moreover, it may be displayed on the surface base material that the label part 18 should be peeled first.

なお、第3の実施形態のように、第3の断裁線が省略される場合も、第2の断裁線の切れ目の形状は、直線状に限定されず、図6に示すように、第2の実施形態と同様に、「く」の字状の切れ目52であっても良いし、他の形状のものであっても良い。   Even when the third cutting line is omitted as in the third embodiment, the shape of the cut line of the second cutting line is not limited to a straight line, and as shown in FIG. Similarly to the embodiment, the “<”-shaped cut 52 may be used, or another shape may be used.

なお、上記各実施形態において、ラベル部21、22は略矩形であったが、その形状は矩形に限定されず、例えば三角形等他の多角形でも良いし、円形等であっても良い。また、擬似接着ラベル10の構造や材質は、上記実施形態に限定されない。例えば、表面基材11、擬似接着層12、粘着剤層13以外の層を備えたものであっても構わない。また、各断裁線の間隔や切れ目の長さは、均等でも非均等であっても構わないし、各断裁線は、直線に限定されず曲線であっても構わない。   In each of the above-described embodiments, the label portions 21 and 22 are substantially rectangular. However, the shape is not limited to a rectangle, and may be other polygons such as a triangle or a circle. Further, the structure and material of the pseudo-adhesive label 10 are not limited to the above embodiment. For example, you may provide layers other than the surface base material 11, the pseudo adhesion layer 12, and the adhesive layer 13. Further, the interval between cut lines and the length of cut lines may be equal or non-uniform, and each cut line is not limited to a straight line but may be a curved line.

次に、本発明について、以下実施例を用いて説明するが、本発明は以下の実施例の構成に限定されない。   Next, the present invention will be described below using examples, but the present invention is not limited to the configurations of the following examples.

[実施例1]
表面基材としてタック原紙(ユポ・コーポレーション社製、商品名:ユポタック原紙 60SGS)を使用し、擬似接着層を形成するための熱可塑性樹脂として、ポリプロピレン(サンアロマー社製、商品名:サンアロマーPHA03A)を使用した。熱可塑性樹脂を押出温度290℃で厚さ20μmとなるようにTダイにて押し出し塗工し、表面基材の裏面に擬似接着層を積層した擬似接着シートを得た。次に、シリコーン系剥離紙の離型剤面に、アクリル系粘着剤を厚さ25μmになるように塗工して粘着剤層を形成し、先に形成した擬似接着シートの擬似接着層に貼り合わせた。その後、打ち抜き加工とともにミシン目加工により第1〜第3の破断線を形成し、カス上げを行って図2に示す擬似接着ラベルを得た。
[Example 1]
Tack base paper (manufactured by Yupo Corporation, trade name: Yupotac base paper 60SGS) is used as the surface base material, and polypropylene (manufactured by Sun Allomer, trade name: Sun Allomer PHA03A) is used as the thermoplastic resin for forming the pseudo-adhesive layer. used. The thermoplastic resin was extrusion coated with a T-die so that the thickness was 20 μm at an extrusion temperature of 290 ° C., and a pseudo adhesive sheet was obtained in which a pseudo adhesive layer was laminated on the back surface of the surface base material. Next, an acrylic pressure-sensitive adhesive is applied to the release agent surface of the silicone release paper to a thickness of 25 μm to form a pressure-sensitive adhesive layer, which is then applied to the pseudo-adhesive layer of the previously formed pseudo-adhesive sheet. Combined. Then, the 1st-3rd broken line was formed by perforation processing with punching, and the residue was raised, and the pseudo-adhesive label shown in FIG. 2 was obtained.

擬似接着ラベルは、横150mm、縦100mmのものであって、横方向における中央に第1〜第3の断裁線を設けたものであった。第1の破断線における切れ目の長さL1は2mm、間隔の長さD1は0.5mm、第2及び第3の破断線における切れ目の長さL2、L3は1mm、第1の破断線の切れ目と、第2及び第3の破断線の切れ目の端部との離間距離E1は0.3mmであった。なお、各切れ目は、表面基材、擬似接着層及び粘着剤層を貫通するように形成したものであった。   The pseudo-adhesive label had a width of 150 mm and a length of 100 mm, and was provided with first to third cutting lines in the center in the horizontal direction. The cut line length L1 in the first break line is 2 mm, the interval length D1 is 0.5 mm, the cut line lengths L2 and L3 in the second and third break lines are 1 mm, and the cut line in the first break line is 1 mm. And the separation distance E1 between the end portions of the second and third break lines was 0.3 mm. In addition, each cut | interruption was formed so that a surface base material, a pseudo adhesion layer, and an adhesive layer might be penetrated.

[比較例1]
第2及び第3の断裁線を設けずに、第1の断裁線を上辺から下辺まで延在する一条の縦の切れ目とし、その切れ目を表面基材のみが貫通するように切り込んだものとした点を除いて実施例1と同様であった。
[Comparative Example 1]
Without providing the second and third cutting lines, the first cutting line was a single vertical cut extending from the upper side to the lower side, and the cut was made so that only the surface base material penetrated. It was the same as Example 1 except the point.

[比較例2]
分離線において、第2及び第3の断裁線を設けなかったことを除いて実施例1と同様に実施した。
[Comparative Example 2]
The separation line was carried out in the same manner as in Example 1 except that the second and third cutting lines were not provided.

[評価方法]
(1)擬似側剥離試験
実施例、比較例の擬似接着ラベルを、剥離基材を引き剥がして除去した後、被着物である台紙に貼着した。この状態で、図2に示す角部18Aからラベル部18を剥離方向Aに剥離角度180°で剥離する試験を10回行い、表面基材を破かずに分離線に沿って剥がすことができるかを評価した。表面基材の破れが発生した回数を、剥離不良率(破れが発生した回数/試験回数×100)で表し、剥離不良率20%未満を良好、剥離不良率20%以上を不可と評価した。
[Evaluation methods]
(1) Pseudo-side peeling test The pseudo-adhesive labels of Examples and Comparative Examples were removed by peeling off the peeling base material, and then attached to a backing sheet as an adherend. In this state, can the test be performed 10 times to peel the label portion 18 from the corner portion 18A shown in FIG. 2 in the peeling direction A at a peeling angle of 180 ° and peeled along the separation line without breaking the surface substrate? Evaluated. The number of occurrences of tearing of the surface base material was expressed as a peel failure rate (number of tears generated / number of tests × 100).

(2)作業性確認試験
実施例及び比較例の擬似接着ラベルを、剥離基材を引き剥がして除去し、被着物である台紙に貼着する際の作業性を確認した。作業性が良好なものを良好(○)、作業可能なものを可(△)、作業し難いものを不可(×)として評価した。
(2) Workability confirmation test The pseudo-adhesive labels of the examples and comparative examples were removed by peeling off the release substrate, and workability was confirmed when sticking to a backing paper as an adherend. Good workability was evaluated as good (◯), workable was acceptable (Δ), and difficult to work was evaluated as unacceptable (x).

表1に、実施例及び比較例で得られた擬似接着ラベルの評価試験の結果を示す。

Figure 2012181449
Table 1 shows the results of the evaluation test of the pseudo-adhesive labels obtained in the examples and comparative examples.
Figure 2012181449

表面基材に一条の縦の切込を入れた比較例1では、擬似側剥離試験では問題なかったが、作業性確認試験では剥離基材を除去すると、擬似接着ラベルが自重により切込部分で折れ曲がり作業し難かった。また、断裁線を通常のミシン目形状とした比較例2は、作業性確認試験では表面基材が折れ曲がることなく問題なかったが、擬似側剥離試験では表面基材の破れが発生した。   In Comparative Example 1 in which a single vertical cut was made on the surface base material, there was no problem in the pseudo side peel test. However, in the workability confirmation test, when the peel base material was removed, the pseudo adhesive label was cut by its own weight. It was difficult to bend. Further, in Comparative Example 2 in which the cutting line had a normal perforation shape, there was no problem in that the surface base material was not bent in the workability confirmation test, but the surface base material was broken in the pseudo side peel test.

これに対し、実施例1では、表面基材に破れが発生することなく擬似接着層からラベル部を剥離することができ、更に、剥離基材を除去した後にラベルが折り曲がることなく作業性が良好だった。このように、分離線を複線状としたことにより、表面基材を分離線で分離して剥離する際に表面基材に破れが発生することなく、更にラベルの折れ曲がりも発生しない作業性の良い擬似接着ラベルを得ることができた。   On the other hand, in Example 1, the label part can be peeled from the pseudo-adhesive layer without tearing the surface base material, and the workability is improved without the label being bent after the peeling base material is removed. It was good. Thus, by making the separation line into a double-line shape, when the surface base material is separated and separated by the separation line, the surface base material is not torn, and further, the label is not bent and the workability is good. A pseudo-adhesive label could be obtained.

10 擬似接着ラベル
11 表面基材
12 疑似接着層
13 粘着剤層
20 分離線
21〜23 第1〜第3の断裁線
31〜33 切れ目
DESCRIPTION OF SYMBOLS 10 Pseudo-adhesion label 11 Surface base material 12 Pseudo-adhesion layer 13 Adhesive layer 20 Separation line 21-23 1st-3rd cutting line 31-33 Break

Claims (4)

表面基材と、前記表面基材に擬似接着される擬似接着層と、粘着剤層とがこの順に積層された積層構造を備え、前記粘着剤層が被着物に貼着された状態で、前記表面基材を前記擬似接着層から剥離可能な擬似接着ラベルであって、
前記表面基材は、少なくとも2以上のラベル部に分離して前記擬似接着層から剥離可能とする分離線を備え、
前記分離線は、複数の切れ目が間隔をおいて形成された断裁線が、少なくとも2本近接して並べられて複線状となり、
前記少なくとも2本の断裁線のうちの1本の断裁線の間隔を塞ぐように、その間隔の近傍に他の1本の断裁線の切れ目が配置されることを特徴とする擬似接着ラベル。
A surface base material, a pseudo-adhesive layer that is pseudo-adhered to the surface base material, and a pressure-sensitive adhesive layer are provided in this order, and the pressure-sensitive adhesive layer is attached to an adherend, A pseudo-adhesive label capable of peeling the surface substrate from the pseudo-adhesive layer,
The surface base material is provided with a separation line that can be separated into at least two or more label portions and can be peeled off from the pseudo-adhesive layer,
The separating line is a double-lined shape in which at least two cutting lines in which a plurality of cuts are formed at intervals are arranged close to each other,
The pseudo-adhesive label, wherein a cut line of another cutting line is arranged in the vicinity of the interval so as to close the interval of one cutting line of the at least two cutting lines.
前記分離線は、前記断裁線が、少なくとも3本近接して並べられて複線状となり、
前記1本の断裁線の前記間隔を両側から塞ぐように、他の2本の断裁線の切れ目が配置されることを特徴とする請求項1に記載される擬似接着ラベル。
The separating line is a double-lined shape in which at least three cutting lines are arranged close to each other,
2. The pseudo adhesive label according to claim 1, wherein the cut line of the other two cutting lines is disposed so as to close the interval of the one cutting line from both sides.
前記1本の断裁線の各切れ目は、直線状であることを特徴とする請求項1又は2に記載される擬似接着ラベル。   The pseudo adhesive label according to claim 1 or 2, wherein each cut line of the one cutting line is linear. 前記断裁線のうちの前記他の1本又は2本の断裁線の各切れ目は、直線状、あるいは両端が前記1本の断裁線に近づくように傾斜した線状であることを特徴とする請求項1ないし3のいずれか1項に記載される擬似接着ラベル。   Each of the cuts of the other one or two of the cutting lines is linear or inclined so that both ends approach the one cutting line. Item 4. A pseudo-adhesive label according to any one of items 1 to 3.
JP2011045520A 2011-03-02 2011-03-02 Pseudo adhesive label Active JP5730618B2 (en)