CN1597348A - Manufacturing method of artistic building or artificial snow garden - Google Patents

Manufacturing method of artistic building or artificial snow garden Download PDF

Info

Publication number
CN1597348A
CN1597348A CN 200410070786 CN200410070786A CN1597348A CN 1597348 A CN1597348 A CN 1597348A CN 200410070786 CN200410070786 CN 200410070786 CN 200410070786 A CN200410070786 A CN 200410070786A CN 1597348 A CN1597348 A CN 1597348A
Authority
CN
China
Prior art keywords
cured
model
mold
glass fibre
fibre cloth
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN 200410070786
Other languages
Chinese (zh)
Inventor
李翠华
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN 200410070786 priority Critical patent/CN1597348A/en
Publication of CN1597348A publication Critical patent/CN1597348A/en
Pending legal-status Critical Current

Abstract

The patent relates to method of making snow scenery as artist building designs or snow gardens which is formed by: preparing materials and casting in a short time and with low cost. They have various designs in size, color, shape and material, can be located anywhere, and are valuable as artist buildings and artificial snow gardens for enjoy and commercial development.

Description

The process for making of art architecture or artificial snow garden
Technical field
The present invention relates to the making construction method of art architecture or artificial snow garden, belong to water mould, engraving, Counterfeit Item field.
Existing snow garden is the scenery under the cold temperature, so goods are on sense organ, works with great care not as Counterfeit Item, and color is soft and moist pure, is not subjected to the restriction of temperature, imitated vestige.
The process for making that the purpose of this invention is to provide art architecture or artificial snow garden, goods obviously are better than the scenery of the Nature, and the imitative snow garden duration is short, and cost is low; Not being subjected to the restriction in environment, temperature, space, kind, specification, color, classification, traditional handicraft, material, environmental protection, market, is to have room construction material and the art architecture of viewing and admiring, develop value.
1) simulation:
(1) system wooden mold: timber is sawed, cuts, carves, bondd, the model that joggle becomes to adhere to specification;
(2) system plaster cast: gypsum is added 801 glue, mix well, water and be filled in, after solidifying it is engraved as the model that adheres to specification than in big 0.5~10 centimeter sylphon of model by the mixing of 100: 40~70 ratio;
(3) system mud model: the model that foundry loam or rubber cement kneading model are become to adhere to specification;
(4) engraving: work with great care according to layout;
(5) polishing: the corase grind machine, finish grind by hand, to the light cleaning;
(6) bonding: add talcum powder with 502 glue and add saw wood ash=100: 10~30: 10~30;
(7) play putty: add diluent with transparent resin and add curing agent=100: 10~30: 10~30;
(8) polishing: with the sand polishing, from thick number to thin number, to the light cleaning;
(9) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on the model, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
2) the three-dimensional soft or hard mould of system:
(1) fixed model: the position that model is narrow down, wide position stands on the tabula rasa up, adds talcum powder with 502 glue, by 100: 10~30 fixed ratio;
(2) system soft mold: add with silicon rubber and to solidify Ji, mix well, water and be filled on the model, up catch up with the mixing silicon rubber that grey cutter will down drop down from the model, till solidifying by 100: 5~20 ratio mixing;
(3) drying: dried in the shade slow curing 2~24 hours 1~2 hour;
(4) system gypsum mold: add curing agent with 801 glue, mix by 100: 50~80 ratio and mix well, be put on half of soft mold, extremely above till over half 0,5~10 centimeters of soft mold;
(5) drying: dried in the shade 5~10 minutes;
(6) remove mould: the plaster mold over half 0,5~10 centimeters above soft mold removed;
(7) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on half soft mold that does not water gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(8) system hard mold 1: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush was being gone up on the soft mold of cured half, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth is brushed above-mentioned hybrid resin on thick glass fibre cloth again;
(9) drying: dried in the shade 10~30 minutes;
(10) remove mould: the gypsum mold of second half of the hard mold that will make is all removed, and cleans up;
(11) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on half the soft mold of having removed gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(12) system hard mold 2: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush is on the soft mold of half of removing gypsum mold, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth is brushed above-mentioned hybrid resin on thick glass fibre cloth again;
(13) drying: dried in the shade 10~30 minutes;
(14) die sinking: hard mold is opened respectively, taken out soft mold, soft mold is cut a mouth, take out the model of the inside;
(15) cut edge: the burr around the hard mold are cut off,
(16) polishing: corase grind machine, correct grinding are by hand, and be extremely smooth straight and even;
(17) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on the inwall of soft or hard mould, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
3) system plane soft or hard mould:
(1) system sylphon: vary in size according to model, make the sylphon of different size;
(2) system soft mold; Silicon rubber is added curing agent, mix well in 100: 5~20 ratio mixing, brush was being gone up on that cured half model;
(3) drying: dried in the shade slow curing 2~24 hours 1~2 hour;
(4) system hard mold: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush do not water gypsum mold half soft mold on, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed at fine glass fibre cloth, layer overlay thick glass fibre cloth waters above-mentioned hybrid resin and is filled on the thick glass fibre cloth till flood over half 0,5~10 centimeters of thick glass fibre cloth;
(5) drying: dried in the shade 10~30 minutes;
(6) die sinking tool: open box, remove tabula rasa, take out the model of the inside;
(7) upward cured; The floor is cured or mould is cured or table leather board spray is cured, brush or be sprayed on the soft or hard mould inner wall, to dry in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
4) system plane soft mold:
(1) system box: vary in size according to model, make different size, than model big 0.5 centimeter~10 centimeters sylphon;
(2) fixed model: model is placed on the tabula rasa, model bottom packing paper plate or fiberboard or plank or laminate, thickness determines what according to goods, goods fill up slab more, and goods fill up rich plate less, after fixing with 502 glue, again the sylphon of making is enclosed within on the model, fixes with 502 glue;
(3) system soft mold: silicon rubber is added curing agent, mix by 100: 5~20 ratio and mix well, water sylphon, till flooding 0.5~10 centimeter on model;
(4) drying: dried in the shade slow curing 2~24 hours 1~2 hour;
(5) die sinking tool: open box, remove tabula rasa, take out the model of the inside;
(6) go up cured: the floor is cured or mould is cured or it is cured to spray the spray of table leather board, brush or be sprayed on the soft mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
5) system gypsum plane hard mold:
(1) system sylphon: vary in size according to model, make a different size, than big 0.5~10 centimeter sylphon of model:
(2) fixed model: model is placed on the tabula rasa, after fixing with 502 glue, again the sylphon of making is put on the model, fix with 502 glue again
(3) system gypsum hard mold: resin is added the ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush is not watering on that half model of gypsum mold, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth, again above-mentioned hybrid resin is brushed on thick glass fibre cloth, after drying in the shade 10~30 minutes, add talcum powder with 801 glue, ratio mixing in 100: 40~70 is mixed well, waters to be filled on the thick glass fibre cloth, and be last to flooding 0.5~10 centimeter of thick glass fibre cloth;
(4) drying: dried in the shade 5~10 minutes;
(5) die sinking: open sylphon, remove tabula rasa, take out the model of the inside;
(6) go up cured: the floor is cured or mould is cured or the table leather board sprays cured brush or be sprayed on the inwall of gypsum plane hard mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times.
6) the three-dimensional hard mold of system gypsum:
(1) system sylphon; Vary in size according to goods, make different size,, fix with 502 glue than 2 big 0.5~10 centimeter sylphons of model:
(2) fixed model: external model is placed on the tabula rasa, fixes, again sylphon is enclosed within on the model, fix with 502 glue with 502 glue;
(3) system gypsum mold: add land plaster with 801 glue, mix well, water sylphon, till flooding over half 0.5~10 centimeter of model by the mixing of 100: 40~70 ratio;
(4) drying: dried in the shade 5~10 minutes;
(5) remove mould: the gypsum mold that will make 0.5~10 centimeter gypsum mold over half has been carved, and cleans up;
(6) go up cured: the floor is cured or mould is cured or it is cured to spray the spray of table leather board, brush or be sprayed on half the model that does not water gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(7) system gypsum hard mold 1: resin is added the ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush was being gone up on the model of cured half, spread on two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth, again above-mentioned hybrid resin is brushed on thick glass fibre cloth, after drying in the shade 10~30 minutes, again 801 glue are added land plaster, mix in 100: 40~70 ratio and mix well, water and be filled on the thick glass fibre cloth of brushing above-mentioned hybrid resin, till flooding 0,5~10 centimeters on model;
(8) drying: dried in the shade 5~10 minutes;
(9) remove mould: second half the gypsum mold that will make the hard mold made good use of is all removed, and cleans up;
(10) go up cured: the floor is cured or mould is cured or it is cured to spray the spray of table leather board, brush or be sprayed on half the model of having removed gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(11) system hard mold 2: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush was being gone up on that cured half model, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth, above-mentioned hybrid resin is brushed on the thick winding cloth of glass again, after drying in the shade 10~30 minutes, again 801 glue are added land plaster, mix in 100: 40~70 ratio and mix well, water and be filled on the thick glass fibre cloth of brushing above-mentioned hybrid resin, till flooding 0,5~10 centimeters of thick glass fibre cloth;
(12) die sinking tool: the gypsum hard mold is opened respectively, taken out the model of the inside;
(13) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on the inwall of gypsum hard mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
7) make hollow hard mold:
(1) system box: vary in size according to external model, make different size, than 2 big 0.5~10 centimeter sylphons of model;
(2) fixing external model: model is placed on the tabula rasa, with 502 glue fixing after, sylphon is enclosed within on the model;
(3) system gypsum mold: 801 glue are added land plaster, mix by 100: 40~70 ratio and mix well, water sylphon, to flooding over half 0.5~10 centimeter of model, till solidifying;
(4) remove mould: the gypsum mold over half 0,5~10 centimeters above gypsum mold removed, cleaned up;
(5) go up cured: the cured mould in floor is cured or the spray of table leather board is cured, brush or be sprayed on second half the external model of having made gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(6) system outer mold 1: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush is on second half model of the gypsum mold of having made, spread two layers of fine glass fibre cloth, again with above-mentioned hybrid resin, brush is on fine glass fibre cloth, layer overlay thick glass fibre cloth, again with above-mentioned hybrid resin, water and be filled on the thick glass fibre cloth, till flooding 0.5~10 centimeter of thick glass fibre cloth;
(7) drying: dried in the shade 10~30 minutes;
(8) remove mould: the gypsum mold of second half of the outer mold 1 that will make is all removed, and cleans up;
(9) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on half the model of having removed gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(10) system outer mold 2: resin is added ketone slurry add and buy liquid and add talcum powder, mixing is mixed well, brush is on the model of half of removing gypsum mold, spread on two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth waters above-mentioned hybrid resin and is filled on the thick glass fibre cloth, till flooding 0.5~10 centimeter of thick glass fibre cloth;
(11) drying: dried in the shade 10~30 minutes;
(12) die sinking tool: hard mold is opened respectively, taken out the model of the inside;
(13) polishing: with the machine polishing, to smooth straight and even;
(14) system box:, make different size, than 2 big 0.5~10 centimeter sylphons of inner model according to inner model size shape difference;
(15) fixing inner mold: inner mold 1 is placed on the tabula rasa, with 502 glue fixing after, again sylphon is enclosed within on the inner model, fix with 502 glue;
(16) system inner mold 1: resin is added ketone slurry add and buy liquid and add talcum powder, the ratio by 100: 10~30: 10~30: 10~30 is mixed and is mixed well, and waters sylphon, till flooding inner model;
(17) drying: dried in the shade 15~20 minutes;
(18) system inner mold 2: inner mold 2 is placed on the tabula rasa, is used for resin and adds ketone slurry and add and buy liquid and add talcum powder, the ratio by 100: 10~30: 10~30: 10~30 is mixed and is mixed well, and waters sylphon, till flooding inner model;
(19) engraving: unnecessary hybrid resin has been carved, cleaned up;
(20) die sinking tool: hard mold is opened respectively, taken out inner model;
(21) polishing: the corase grind machine, finish grind by hand, till the light cleaning;
(22) go up cured: with the mould brush or the floor is cured or the spray of table leather board is cured, brush or be sprayed on the inner mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
8) the imitative ice and snow material of system: transparent resin is added diluent add curing agent and add=100: 10~30: 10~30 or talcum powder add transparent resin and add diluent and add curing agent and add required color=100: 1~10: 10~50: 10~50: 1~10.
9) imitative material of system and goods:
(1) mould: soft mold is put in the hard mold;
(2) goods: transparent resin is added diluent add curing agent, by 100: 10~30: 10~30: 10~30; 10~30: 10~30 ratio is mixed and is mixed well, and with syringe or other vessel, injects or waters and be filled in soft mold or soft or hard mould or hard mold or the gypsum mold, buckle the pressing mold tool, with the limit that a plurality of clips are clamped mould, above-mentioned hybrid resin can't be leached, dry in the shade to solidifying; Or talcum powder is added transparent resin add diluent and add curing agent and add required color by 100: 1~10: 10~50: 10~50: 1~10, be sprinkling upon and dry in the shade on the floor to solidifying;
(3) die sinking tool: open mould, take out early-products;
(4) engraving: early-products is engraved as the goods that adhere to specification;
(5) cool off: goods are placed in the cold water soaked 30 minutes~1 hour;
(6) polishing: the corase grind machine, finish grind by hand, to the light cleaning;
(7) gluing: with above-mentioned mixed transparent resin goods are described repeatedly, till satisfied;
(8) drying: dried in the shade 10~30 minutes;
(9) japanning: with blowing varnish goods are sprayed repeatedly, dried in the shade 15~20 minutes, this step needs 2~3 times repeatedly.
11), combination shaping:
(1) main body is shaped: the surface plate of making by above-mentioned same process method, post and the beam of carving dragon picture phoenix on the main body frame that all is combined to methods such as perforating, bondings, allow body reach designing requirement;
(2) engraving: adhesive has been carved, cleaned up;
(3) polishing: carry out with fine sandpaper, from thick number to thin number, to the light cleaning;
(4) ice making snow: add curing agent with transparent resin and add diluent, mix well by 100: 10~30: 10~30 mixing, dial or drench on the article in the garden, till icing sensation arranged, be sprinkling upon the snow of making by above-mentioned process on the hybrid resin that solidifies or the ground again, till having ice and snow to exist;
(5) drying: dried in the shade 30 minutes~1 hour;
(6) drying: with being sprayed on the duplicate from spraying paint, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
With art architecture or artificial snow garden that above-mentioned process for making is finished, workmanship is exquisite, lines are graceful, happy, is that the utmost point has material and the goods of viewing and admiring, collect, develop value.
The specific embodiment:
Introduce the step of making art architecture or artificial snow garden of process provided by the present invention below.
Art architecture or artificial snow garden profile: long * wide * high=0.98 meter * 0.68 meter * 0.78 meter
Basic pattern be one by ice and snow topped all move, plant, the art architecture or the artificial snow garden in personage, mountain, water, foot bridge, house.
1) simulation:
(1) system wooden mold: timber is sawed, cuts, carves, bondd, the model that joggle becomes to adhere to specification;
(2) system plaster cast: gypsum is added 801 glue, mix well, water and be filled in, after solidifying it is engraved as the model that adheres to specification than in big 0.5~10 centimeter sylphon of model by the mixing of 100: 40~70 ratio;
(3) system mud model: the model that foundry loam or rubber cement kneading model are become to adhere to specification;
(4) engraving: work with great care according to layout;
(5) polishing: the corase grind machine, finish grind by hand, to the light cleaning;
(6) bonding: add talcum powder with 502 glue and add saw wood ash=100: 10~30: 10~30;
(7) play putty: add diluent with transparent resin and add curing agent=100: 10~30: 10~30;
(8) polishing: with the sand polishing, from thick number to thin number, to the light cleaning;
(9) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on the model, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
2) the three-dimensional soft or hard mould of system:
(1) fixed model: the position that model is narrow down, wide position stands on the tabula rasa up, adds talcum powder with 502 glue, by 100: 10~30 fixed ratio;
(2) system soft mold: add with silicon rubber and to solidify Ji, mix well, water and be filled on the model, up catch up with the mixing silicon rubber that grey cutter will down drop down from the model, till solidifying by 100: 5~20 ratio mixing;
(3) drying: dried in the shade slow curing 2~24 hours 1~2 hour;
(4) system gypsum mold: add curing agent with 801 glue, mix by 100: 50~80 ratio and mix well, be put on half of soft mold, extremely above till over half 0,5~10 centimeters of soft mold;
(5) drying: dried in the shade 5~10 minutes;
(6) remove mould: the plaster mold over half 0,5~10 centimeters above soft mold removed;
(7) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on half soft mold that does not water gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(8) system hard mold 1: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush was being gone up on the soft mold of cured half, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth is brushed above-mentioned hybrid resin on thick glass fibre cloth again;
(9) drying: dried in the shade 10~30 minutes;
(10) remove mould: the gypsum mold of second half of the hard mold that will make is all removed, and cleans up;
(11) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on half the soft mold of having removed gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(12) system hard mold 2: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush is on the soft mold of half of removing gypsum mold, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth is brushed above-mentioned hybrid resin on thick glass fibre cloth again;
(13) drying: dried in the shade 10~30 minutes;
(14) die sinking: hard mold is opened respectively, taken out soft mold, soft mold is cut a mouth, take out the model of the inside;
(15) cut edge: the burr around the hard mold are cut off,
(16) polishing: corase grind machine, correct grinding are by hand, and be extremely smooth straight and even;
(17) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on the inwall of soft or hard mould, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
3) system plane soft or hard mould:
(1) system sylphon: vary in size according to model, make the sylphon of different size;
(2) system soft mold: silicon rubber is added curing agent, mix well in 100: 5~20 ratio mixing, brush was being gone up on that cured half model;
(3) drying: dried in the shade slow curing 2~24 hours 1~2 hour;
(4) system hard mold: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush do not water gypsum mold half soft mold on, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed at fine glass fibre cloth, layer overlay thick glass fibre cloth waters above-mentioned hybrid resin and is filled on the thick glass fibre cloth till flood over half 0,5~10 centimeters of thick glass fibre cloth;
(5) drying: dried in the shade 10~30 minutes;
(6) go up cured: analyse ground cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on the soft or hard mould inner wall, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
4) system plane soft mold:
(1) system box: vary in size according to model, make different size, than model big 0.5 centimeter~10 centimeters sylphon;
(2) fixed model: model is placed on the tabula rasa, model bottom packing paper plate or fiberboard or plank or laminate, thickness determines what according to goods, goods fill up slab more, and goods fill up rich plate less, after fixing with 502 glue, again the sylphon of making is enclosed within on the model, fixes with 502 glue;
(3) system soft mold: silicon rubber is added curing agent, mix by 100: 5~20 ratio and mix well, water sylphon, till flooding 0.5~10 centimeter on model;
(4) drying: dried in the shade slow curing 2~24 hours 1~2 hour;
(5) die sinking tool: open box, remove tabula rasa, take out the model of the inside;
(6) go up cured: the floor is cured or mould is cured or it is cured to spray the spray of table leather board, brush or be sprayed on the soft mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
5) system gypsum plane hard mold:
(1) system sylphon: vary in size according to model, make a different size, than big 0.5~10 centimeter sylphon of model:
(2) fixed model: model is placed on the tabula rasa, after fixing with 502 glue, again the sylphon of making is put on the model, fix with 502 glue again
(3) system gypsum hard mold: resin is added the ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush is not watering on that half model of gypsum mold, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth, again above-mentioned hybrid resin is brushed on thick glass fibre cloth, after drying in the shade 10~30 minutes, add talcum powder with 801 glue, ratio mixing in 100: 40~70 is mixed well, waters to be filled on the thick glass fibre cloth, and be last to flooding 0.5~10 centimeter of thick glass fibre cloth;
(4) drying: dried in the shade 5~10 minutes;
(5) die sinking: open sylphon, remove tabula rasa, take out the model of the inside;
(6) go up cured: the floor is cured or mould is cured or the table leather board sprays cured brush or be sprayed on the inwall of gypsum plane hard mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times.
6) the three-dimensional hard mold of system gypsum:
(1) system sylphon: vary in size according to goods, make different size,, fix with 502 glue than 2 big 0.5~10 centimeter sylphons of model;
(2) fixed model: model is placed on the tabula rasa, fixes, again sylphon is enclosed within on the model, fix with 502 glue with 502 glue;
(3) system gypsum mold: add land plaster with 801 glue, mix well, water sylphon, till flooding over half 0.5~10 centimeter of model by the mixing of 100: 40~70 ratio;
(4) drying: dried in the shade 5~10 minutes;
(5) remove mould: the gypsum mold that will make 0.5~10 centimeter gypsum mold over half has been carved, and cleans up;
(6) go up cured: the floor is cured or mould is cured or it is cured to spray the spray of table leather board, brush or be sprayed on half the model that does not water gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(7) system gypsum hard mold 1: resin is added the ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush was being gone up on the model of cured half, spread on two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth, again above-mentioned hybrid resin is brushed on thick glass fibre cloth, after drying in the shade 10~30 minutes, again 801 glue are added land plaster, mix in 100: 40~70 ratio and mix well, water and be filled on the thick glass fibre cloth of brushing above-mentioned hybrid resin, till flooding 0,5~10 centimeters on model;
(8) drying: dried in the shade 5~10 minutes;
(9) remove mould: second half the gypsum mold that will make the hard mold made good use of is all removed, and cleans up;
(10) go up cured: the floor is cured or mould is cured or it is cured to spray the spray of table leather board, brush or be sprayed on half the model of having removed gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(11) system hard mold 2: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 0~30 is mixed well, brush was being gone up on that cured half model, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth, again above-mentioned hybrid resin is brushed on thick glass fibre cloth, after drying in the shade 10~30 minutes, again 801 glue are added land plaster, mix in 100: 40~70 ratio and mix well, water and be filled on the thick glass fibre cloth of brushing above-mentioned hybrid resin, till flooding 0,5~10 centimeters of thick glass fibre cloth;
(12) die sinking tool: the gypsum hard mold is opened respectively, taken out the model of the inside;
(13) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on the inwall of gypsum hard mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
7) make hollow hard mold:
(1) system box: vary in size according to external model, make different size, than 2 big 0.5~10 centimeter sylphons of model;
(2) fixing external model: model is placed on the tabula rasa, with 502 glue fixing after, sylphon is enclosed within on the model;
(3) system gypsum mold: 801 glue are added land plaster, mix by 100: 40~70 ratio and mix well, water sylphon, to flooding over half 0.5~10 centimeter of model, till solidifying;
(4) remove mould: the gypsum mold over half 0,5~10 centimeters above gypsum mold removed, cleaned up;
(5) go up cured: the cured mould in floor is cured or the spray of table leather board is cured, brush or be sprayed on second half the external model of having made gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(6) system outer mold 1: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush is on second half model of the gypsum mold of having made, spread two layers of fine glass fibre cloth, again with above-mentioned hybrid resin, brush is on fine glass fibre cloth, layer overlay thick glass fibre cloth, again with above-mentioned hybrid resin, water and be filled on the thick glass fibre cloth, till flooding 0.5~10 centimeter of thick glass fibre cloth;
(7) drying: dried in the shade 10~30 minutes;
(8) remove mould: second half gypsum mold of the outer mold 1 that will make is all removed, and cleans up;
(9) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on half the model of having removed gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(10) system outer mold 2: resin is added ketone slurry add and buy liquid and add talcum powder, mixing is mixed well, brush is on the model of half of removing gypsum mold, spread on two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth waters above-mentioned hybrid resin and is filled on the thick glass fibre cloth, till flooding 0.5~10 centimeter of thick glass fibre cloth;
(11) drying: dried in the shade 10~30 minutes;
(12) die sinking tool: hard mold is opened respectively, taken out the model of the inside;
(13) polishing: with the machine polishing, to smooth straight and even;
(14) system box:, make different size, than 2 big 0.5~10 centimeter sylphons of inner model according to inner model size shape difference;
(15) fixing inner mold: inner mold 1 is placed on the tabula rasa, with 502 glue fixing after, again sylphon is enclosed within on the inner model, fix with 502 glue;
(16) system inner mold 1: resin is added ketone slurry add and buy liquid and add talcum powder, the ratio by 100: 10~30: 10~30: 10~30 is mixed and is mixed well, and waters sylphon, till flooding inner model;
(17) drying: dried in the shade 15~20 minutes;
(18) system inner mold 2: inner mold 2 is placed on the tabula rasa, is used for resin and adds ketone slurry and add and buy liquid and add talcum powder, the ratio by 100: 10~30: 10~30: 10~30 is mixed and is mixed well, and waters sylphon, till flooding inner model;
(19) engraving: unnecessary hybrid resin has been carved, cleaned up;
(20) die sinking tool: hard mold is opened respectively, taken out inner model;
(21) polishing: the corase grind machine, finish grind by hand, till the light cleaning;
(22) go up cured: with the mould brush or the floor is cured or the spray of table leather board is cured, brush or be sprayed on the inner mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
8) the imitative ice and snow material of system: transparent resin is added diluent add curing agent=100: 10~30: 10~30 or talcum powder is added transparent resin and add diluent and add curing agent and add required color, ratio mixing in 100: 1~10: 10~30: 10~30: 1~10 is mixed well, be sprinkling upon on the clean floor, till solidifying;
9) imitative ice and snow material of system and goods:
(1) mould: soft mold is put in the hard mold;
(2) goods: transparent resin is added diluent add curing agent, ratio mixing in 100: 10~30: 10~30 is mixed well, water with vessel and to be filled in soft mold or soft or hard mould or hard mold or the gypsum mold, buckle the pressing mold tool, clamp the limit of mould with a plurality of clips, above-mentioned hybrid resin can't be leached, till solidifying; Or talcum powder is added transparent resin add diluent and add required color, the ratio in 100: 1~10: 10~30: 10~30: 1~10 is mixed to mix well and is sprinkling upon on the clean floor, till solidifying;
(3) drying: dry in the shade to just solidifying;
(4) die sinking tool: open mould, take out early-products;
(5) engraving: early-products is engraved as the goods that adhere to specification;
(6) cool off: goods are placed in the cold water soaked 30 minutes~1 hour;
(7) polishing: the corase grind machine, finish grind by hand, to the light cleaning;
(8) gluing: with above-mentioned mixed transparent resin goods are described repeatedly, till satisfied;
(9) drying: dried in the shade 10~30 minutes;
(10) japanning: with blowing varnish goods are sprayed repeatedly, dried in the shade 15~20 minutes, this step needs 2~3 times repeatedly.
10), combination shaping:
(1) bonding main body: flower, skill, leaf, bar making by above-mentioned same process method, all be combined on the main body goods with methods such as perforating bondings, allow body reach designing requirement;
(2) engraving: adhesive has been carved, cleaned up;
(3) polishing: carry out with fine sandpaper, from thick number to thin number, to the light cleaning;
(4) ice making snow: with above-mentioned mixed transparent resin, dial or drench on all article in the garden, till icing sensation of solidifying arranged; Or above-mentioned mixing talcum powder is sprinkling upon article or on the ground, till having ice and snow to exist;
(5) drying: dried in the shade 30 minutes~1 hour;
(7) drying: with being sprayed on the duplicate from spraying paint, dried in the shade 15~20 minutes, this step need be carried out repeatedly.

Claims (9)

1, the process for making of art architecture or artificial snow garden, its particular-trade are to carry out according to the following steps:
1) simulation:
(1) system wooden mold: timber is sawed, cuts, carves, bondd, the model that joggle becomes to adhere to specification;
(2) system plaster cast: gypsum is added 801 glue, mix well, water and be filled in, after solidifying it is engraved as the model that adheres to specification than in big 0.5~10 centimeter sylphon of model by the mixing of 100: 40~70 ratio;
(3) system mud model: the model that foundry loam or rubber cement kneading model are become to adhere to specification;
(4) engraving: work with great care according to layout;
(5) polishing: the corase grind machine, finish grind by hand, to the light cleaning;
(6) bonding: add talcum powder with 502 glue and add saw wood ash=100: 10~30: 10~30;
(7) play putty: add diluent with transparent resin and add curing agent=100: 10~30: 10~30;
(8) polishing: with the sand polishing, from thick number to thin number, to the light cleaning;
(9) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on the model, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
2) the three-dimensional soft or hard mould of system:
(1) fixed model: the position that model is narrow down, wide position stands on the tabula rasa up, adds talcum powder with 502 glue, by 100: 10~30 fixed ratio;
(2) system soft mold: add with silicon rubber and to solidify Ji, mix well, water and be filled on the model, up catch up with the mixing silicon rubber that grey cutter will down drop down from the model, till solidifying by 100: 5~20 ratio mixing;
(3) drying: dried in the shade slow curing 224 hours 1~2 hour;
(4) system gypsum mold: add curing agent with 801 glue, mix by 100: 50~80 ratio and mix well, be put on half of soft mold, extremely above till over half 0,5~10 centimeters of soft mold;
(5) drying: dried in the shade 5~10 minutes;
(6) remove mould: the plaster mold over half 0,5~10 centimeters above soft mold removed;
(7) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on half soft mold that does not water gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(8) system hard mold 1: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush was being gone up on the soft mold of cured half, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth is brushed above-mentioned hybrid resin on thick glass fibre cloth again;
(9) drying: dried in the shade 10~30 minutes;
(10) remove mould: the gypsum mold of second half of the hard mold that will make is all removed, and cleans up;
(11) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on half the soft mold of having removed gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(12) system hard mold 2: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush is on the soft mold of half of removing gypsum mold, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth is brushed above-mentioned hybrid resin on thick glass fibre cloth again;
(13) drying: dried in the shade 10~30 minutes;
(14) die sinking: hard mold is opened respectively, taken out soft mold, soft mold is cut a mouth, take out the model of the inside;
(15) cut edge: the burr around the hard mold are cut off,
(16) polishing: corase grind machine, correct grinding are by hand, and be extremely smooth straight and even;
(17) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on the inwall of soft or hard mould, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
3) system plane soft or hard mould:
(1) system sylphon: vary in size according to model, make the sylphon of different size;
(2) system soft mold: silicon rubber is added curing agent, mix well in 100: 5~20 ratio mixing, brush was being gone up on that cured half model;
(3) drying: dried in the shade slow curing 2~24 hours 1~2 hour;
(4) system hard mold; Resin is added ketone slurry to be added and buys liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush do not water gypsum mold half soft mold on, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed at fine glass fibre cloth, layer overlay thick glass fibre cloth waters above-mentioned hybrid resin and is filled on the thick glass fibre cloth till flood over half 0,5~10 centimeters of thick glass fibre cloth;
(5) drying: dried in the shade 10~30 minutes;
(6) go up cured: analyse ground cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on the soft or hard mould inner wall, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
4) system plane soft mold:
(1) system box: vary in size according to model, make different size, than model big 0.5 centimeter~10 centimeters sylphon;
(2) fixed model: model is placed on the tabula rasa, model bottom packing paper plate or fiberboard or plank or laminate, thickness determines what according to goods, goods fill up slab more, and goods fill up rich plate less, after fixing with 502 glue, again the sylphon of making is enclosed within on the model, fixes with 502 glue;
(3) system soft mold: silicon rubber is added curing agent, mix by 100: 5~20 ratio and mix well, water sylphon, till flooding 0.5~10 centimeter on model;
(4) drying: dried in the shade slow curing 2~24 hours 1~2 hour;
(5) die sinking tool: open box, remove tabula rasa, take out the model of the inside;
(6) go up cured: the floor is cured or mould is cured or it is cured to spray the spray of table leather board, brush or be sprayed on the soft mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
5) system gypsum plane hard mold:
(1) system sylphon: vary in size according to model, make a different size, than big 0.5~10 centimeter sylphon of model:
(2) fixed model: model is placed on the tabula rasa, after fixing with 502 glue, again the sylphon of making is put on the model, fix with 502 glue again
(3) system gypsum hard mold: resin is added the ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush is not watering on that half model of gypsum mold, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth, again above-mentioned hybrid resin is brushed on thick glass fibre cloth, after drying in the shade 10~30 minutes, add talcum powder with 801 glue, ratio mixing in 100: 40~70 is mixed well, waters to be filled on the thick glass fibre cloth, and be last to flooding 0.5~10 centimeter of thick glass fibre cloth;
(4) drying: dried in the shade 5~10 minutes;
(5) die sinking: open sylphon, remove tabula rasa, take out the model of the inside;
(6) go up cured: the floor is cured or mould is cured or the table leather board sprays cured brush or be sprayed on the inwall of gypsum plane hard mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times.
6) the three-dimensional hard mold of system gypsum:
(1) system sylphon: vary in size according to goods, make different size,, fix with 502 glue than 2 big 0.5~10 centimeter sylphons of model;
(2) fixed model: model is placed on the tabula rasa, fixes, again sylphon is enclosed within on the model, fix with 502 glue with 502 glue;
(3) system gypsum mold: add land plaster with 801 glue, mix well, water sylphon, till flooding over half 0.5~10 centimeter of model by the mixing of 100: 40~70 ratio;
(4) drying: dried in the shade 5~10 minutes;
(5) remove mould: the gypsum mold that will make 0.5~10 centimeter gypsum mold over half has been carved, and cleans up;
(6) go up cured: the floor is cured or mould is cured or it is cured to spray the spray of table leather board, brush or be sprayed on half the model that does not water gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(7) system gypsum hard mold 1: resin is added the ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush was being gone up on the model of cured half, spread on two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth, again above-mentioned hybrid resin is brushed on thick glass fibre cloth, after drying in the shade 10~30 minutes, again 801 glue are added land plaster, mix in 100: 40~70 ratio and mix well, water and be filled on the thick glass fibre cloth of brushing above-mentioned hybrid resin, till flooding 0,5~10 centimeters on model;
(8) drying: dried in the shade 5~10 minutes;
(9) remove mould: second half the gypsum mold that will make the hard mold made good use of is all removed, and cleans up;
(10) go up cured: the floor is cured or mould is cured or it is cured to spray the spray of table leather board, brush or be sprayed on half the model of having removed gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(11) system hard mold 2: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush was being gone up on that cured half model, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth, again above-mentioned hybrid resin is brushed on thick glass fibre cloth, after drying in the shade 10~30 minutes, again 801 glue are added land plaster, mix in 100: 40~70 ratio and mix well, water and be filled on the thick glass fibre cloth of brushing above-mentioned hybrid resin, till flooding 0,5~10 centimeters of thick glass fibre cloth;
(12) die sinking tool: the gypsum hard mold is opened respectively, taken out the model of the inside;
(13) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on the inwall of gypsum hard mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
7) make hollow hard mold:
(1) system box: vary in size according to external model, make different size, than 2 big 0.5~10 centimeter sylphons of model;
(2) fixing external model: model is placed on the tabula rasa, with 502 glue fixing after, sylphon is enclosed within on the model;
(3) system gypsum mold: 801 glue are added land plaster, mix by 100: 40~70 ratio and mix well, water sylphon, to flooding over half 0.5~10 centimeter of model, till solidifying;
(4) remove mould: the gypsum mold over half 0,5~10 centimeters above gypsum mold removed, cleaned up;
(5) go up cured: the cured mould in floor is cured or the spray of table leather board is cured, brush or be sprayed on second half the external model of having made gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(6) system outer mold 1: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush is on second half model of the gypsum mold of having made, spread two layers of fine glass fibre cloth, again with above-mentioned hybrid resin, brush is on fine glass fibre cloth, layer overlay thick glass fibre cloth, again with above-mentioned hybrid resin, water and be filled on the thick glass fibre cloth, till flooding 0.5~10 centimeter of thick glass fibre cloth;
(7) drying: dried in the shade 10~30 minutes;
(8) remove mould: second half gypsum mold of the outer mold 1 that will make is all removed, and cleans up;
(9) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on half the model of having removed gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(10) system outer mold 2: resin is added ketone slurry add and buy liquid and add talcum powder, mixing is mixed well, brush is on the model of half of removing gypsum mold, spread on two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth waters above-mentioned hybrid resin and is filled on the thick glass fibre cloth, till flooding 0.5~10 centimeter of thick glass fibre cloth;
(11) drying: dried in the shade 10~30 minutes;
(12) die sinking tool: hard mold is opened respectively, taken out the model of the inside;
(13) polishing: with the machine polishing, to smooth straight and even;
(14) system box:, make different size, than 2 big 0.5~10 centimeter sylphons of inner model according to inner model size shape difference;
(15) fixing inner mold: inner mold 1 is placed on the tabula rasa, with 502 glue fixing after, again sylphon is enclosed within on the inner model, fix with 502 glue;
(16) system inner mold 1: resin is added ketone slurry add and buy liquid and add talcum powder, the ratio by 100: 10~30: 10~30: 10~30 is mixed and is mixed well, and waters sylphon, till flooding inner model;
(17) drying: dried in the shade 15~20 minutes;
(18) system inner mold 2: inner mold 2 is placed on the tabula rasa, is used for resin and adds ketone slurry and add and buy liquid and add talcum powder, the ratio by 100: 10~30: 10~30: 10~30 is mixed and is mixed well, and waters sylphon, till flooding inner model;
(19) engraving: unnecessary hybrid resin has been carved, cleaned up;
(20) die sinking tool: hard mold is opened respectively, taken out inner model;
(21) polishing: the corase grind machine, finish grind by hand, till the light cleaning;
(22) go up cured: with the mould brush or the floor is cured or the spray of table leather board is cured, brush or be sprayed on the inner mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
8) the imitative ice and snow material of system: transparent resin is added diluent add curing agent=100: 10~30: 10~30 or talcum powder is added transparent resin and add diluent and add curing agent and add required color, ratio mixing in 100: 1~10: 10~30: 10~30: 1~10 is mixed well, be sprinkling upon on the clean floor, till solidifying;
9) imitative ice and snow material of system and goods:
(1) mould: soft mold is put in the hard mold;
(2) goods: transparent resin is added diluent add curing agent, ratio mixing in 100: 10~30: 10~30 is mixed well, with syringe or other vessel, inject or water and be filled in soft mold or soft or hard mould or hard mold or the gypsum mold, buckle the pressing mold tool, with the limit that a plurality of clips are clamped mould, above-mentioned hybrid resin can't be leached, till solidifying; Or talcum powder is added transparent resin add diluent and add required color, the ratio in 100: 1~10: 10~30: 10~30: 1~10 is mixed to mix well and is sprinkling upon on the clean floor, till solidifying;
(3) drying: dry in the shade to just solidifying;
(4) die sinking tool: open mould, take out early-products;
(5) engraving: early-products is engraved as the goods that adhere to specification;
(6) cool off: goods are placed in the cold water soaked 30 minutes~1 hour;
(7) polishing: the corase grind machine, finish grind by hand, to the light cleaning;
(8) gluing: with above-mentioned mixed transparent resin goods are described repeatedly, till satisfied;
(9) drying: dried in the shade 10~30 minutes;
(1) japanning: with blowing varnish goods are sprayed repeatedly, dried in the shade 15~20 minutes, this step needs 2~3 times repeatedly.
10), combination shaping:
(1) bonding main body: flower, skill, leaf, bar making by above-mentioned same process method, all be combined on the main body goods with methods such as perforating bondings, allow body reach designing requirement;
(2) engraving: adhesive has been carved, cleaned up;
(3) polishing: carry out with fine sandpaper, from thick number to thin number, to the light cleaning;
(4) ice making snow: with above-mentioned mixed transparent resin, dial or drench on all article in the garden, till icing sensation of solidifying arranged; Or above-mentioned mixing talcum powder is sprinkling upon article or on the ground, till having ice and snow to exist;
(5) drying: dried in the shade 30 minutes~1 hour;
(6) drying: with being sprayed on the duplicate from spraying paint, dried in the shade 15~20 minutes, this step need be carried out repeatedly.
2, model: the preparation method of art architecture artificial snow garden according to claim 1 is characterized in that described cast material is that wood, 801 glue add the shape that land plaster=100: 40~70 or foundry loam, rubber engraving, kneading model become designing requirement.
3, main body bonding: the preparation method of art architecture artificial snow garden according to claim 1 is characterized in that described binding material is that 302 glue or 502 glue add talcum powder=100: 10~30: 10~30.
4, moulding: the method for manufacturing technology of art architecture according to claim 1 or artificial snow garden is characterized in that described Modeling Material is reinforcing bar or steel pipe or iron wire or iron pipe or iron nail or fastener or copper wire or copper pipe.
5, putty: art architecture according to claim 1 or artificial snow garden process for making, it is characterized in that described putty material is that transparent resin adds diluent and adds talcum powder and add required color=100: 10~30: 10~30: 10~30 or atom ash and add curing agent and add required color=100: 10~30: 10~30.
6, soft mold: the process for making of art architecture according to claim 1 or artificial snow garden is characterized in that described soft model material is that silicon rubber adds curing agent=100: 5~20.
7, hard mold and hollow mould: the process for making of art architecture according to claim 1 or artificial snow garden, it is characterized in that described hard mold and hollow mould material are that resin adds ketone slurry and adds and buy liquid and add talcum powder=100: 10~30: 10~30: 10~30 and add two layers of fine glass fibre cloth, one deck thick glass fibre cloth.
8, ice making snow: the process for making of art architecture according to claim 1 or artificial snow garden is characterized in that described ice and snow material is that transparent resin adds the diluent curing agent and adds required color=100: 10~30: 10~30: 10~30.
9, required color: the manufacture craft process of art architecture according to claim 1 or artificial snow garden is characterized in that described coloration material is that transparent resin is with food additives or color inks=100: 10~30: 100: 10~30.
CN 200410070786 2004-07-27 2004-07-27 Manufacturing method of artistic building or artificial snow garden Pending CN1597348A (en)