CN1250379C - Technology for bleaching wooden products and products thereof - Google Patents

Technology for bleaching wooden products and products thereof Download PDF

Info

Publication number
CN1250379C
CN1250379C CN 03130262 CN03130262A CN1250379C CN 1250379 C CN1250379 C CN 1250379C CN 03130262 CN03130262 CN 03130262 CN 03130262 A CN03130262 A CN 03130262A CN 1250379 C CN1250379 C CN 1250379C
Authority
CN
China
Prior art keywords
woodwork
bleaching
solution
wooden product
hour
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN 03130262
Other languages
Chinese (zh)
Other versions
CN1472050A (en
Inventor
朴贤镇
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN 03130262 priority Critical patent/CN1250379C/en
Publication of CN1472050A publication Critical patent/CN1472050A/en
Application granted granted Critical
Publication of CN1250379C publication Critical patent/CN1250379C/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

The present invention relates to a technical method and a product for bleaching a wooden product. The present invention is characterized in that the present invention is composed of the following technical processes: (1) bleaching solution is prepared; (2) the wooden product is arranged in a container which is provided with the prepared bleaching solution, and is immersed; (3) the wooden product is fetched out of the bleaching solution, the liquid is dried, and the wooden product is cleaned by clear water; (4) fixing solution with the pH valve of 4 to 4.5 is prepared; (5) the wooden product which is treated by the process (3) is arranged in the compounded fixing solution and is immersed; (6) the wooden product which is treated by the process (5) is arranged in the clear water and is immersed; (7) the dried wooden product is arranged in a drying box to be dried. The bleaching wooden product can be cosmetic handles, handicrafts or other household goods. The present invention has the advantages that the wooden product is beautiful and clean, and the grade of the wooden product is enhanced.

Description

A kind of process of bleaching woodwork
(1) technical field:
The present invention relates to a kind of woodwork coloring process, particularly a kind of process of bleaching woodwork.
(2) background technology:
At present, the handle of brush for make-up adopts woodwork in the majority for seeking variation and naturalization, in the woodwork coloring process, is many with japanning generally.The effect of japanning generally has coating, has the situation generation that enamelled coating comes off in the use, woodwork is become be difficult to see.
(3) summary of the invention:
The objective of the invention is to design a kind of process of bleaching woodwork, it makes woodwork become magnificent and clean by chemical treatment method, is the novel process method of a kind of novelty, practicality.
Technical scheme of the present invention: a kind of process of bleaching woodwork is characterized in that it is made of following technological process:
1. prepare liquid lime chloride: water, hydrogen peroxide, aqua ammonia are mixed with the solution of 3: 1: 0.03 mass ratio, and above-mentioned each proportioning components error is ± 2%;
2. woodwork is put in the container that the liquid lime chloride for preparing is housed and soaked 3-5 hour, water temperature should be at 70-90 degree Celsius;
3. after woodwork being pulled out from solution and the liquid control being done, clean 2-5 time with clear water;
4. be mixed with pH value and remain on 4 ~ 4.5 glacial acetic acid typing solution of measuring;
5. the woodwork that 3. technology handled is placed in the good glacial acetic acid typing solution of proportioning and soaks after 12-20 hour, woodwork is pulled out control do from glacial acetic acid solution;
6. the woodwork that 5. technology handled is put into to soak after 12-20 hour in the clear water woodwork is being pulled out;
7. will control in the drying baker that the woodwork of doing is placed on 28-40 degree Celsius and dry 12-24 hour.
The above-mentioned said container that holds liquid lime chloride can be metal bucket, mould bucket, wooden barrel.
The product that a kind of process of above-mentioned bleaching woodwork makes is characterised in that the bleaching look permeates in the woodwork texture, is natural white, can be cosmetics handle, handicraft or other daily necessities.
Operation principle of the present invention is: bleaching process uses in woodwork, can use in toiletry especially.This bleaching process is discharged the oxygen molecule in the hydrogen peroxide by chemical reaction, makes that original color becomes white in the woodwork.
Superiority of the present invention is: make woodwork become magnificent and clean, improved the class of woodwork.
(4) specific embodiment:
Embodiment: a kind of process of bleaching woodwork is characterized in that it is made of following technological process:
1. prepare liquid lime chloride: the mass ratio that water, hydrogen peroxide, aqua ammonia is made into into 3: 1: 0.03;
2. woodwork is put in the metal bucket that the liquid lime chloride for preparing is housed and soaked 3 hours, water temperature should be at 70 degree Celsius;
3. after woodwork being pulled out from solution and the liquid control being done, clean 2 times with clear water;
4. be mixed with the glacial acetic acid typing solution that pH value remains on 4 ~ 4.5 amounts with glacial acetic acid;
5. the woodwork that 3. technology handled is placed on and soaks in the good glacial acetic acid solution of proportioning after 12 hours, woodwork is pulled out control do from glacial acetic acid solution;
6. the woodwork that 5. technology handled is put into to soak after 12 hours in the clear water woodwork is being pulled out;
7. will control in the drying bakers that the woodwork of doing is placed on 40 degree Celsius and dry 12 hours.
The product that a kind of process of above-mentioned bleaching woodwork makes is characterised in that the bleaching look permeates in the woodwork texture, is natural white, and said bleaching woodwork can be the cosmetics handle.

Claims (2)

1, a kind of process of bleaching woodwork is characterized in that it is made of following technological process:
1. prepare liquid lime chloride: water, hydrogen peroxide, aqua ammonia are mixed with the solution of 3: 1: 0.03 mass ratio, and above-mentioned each proportioning components error is ± 2%;
2. woodwork is put in the container that the liquid lime chloride for preparing is housed and soaked 3-5 hour, water temperature should be at 70-90 degree Celsius;
3. after woodwork being pulled out from solution and the liquid control being done, clean 2-5 time with clear water;
4. be mixed with pH value and remain on 4 ~ 4.5 glacial acetic acid typing solution of measuring;
5. the woodwork that 3. technology handled is placed in the good glacial acetic acid typing solution of proportioning and soaks after 12-20 hour, woodwork is pulled out control do from glacial acetic acid solution;
6. the woodwork that 5. technology handled is put into to soak after 12-20 hour in the clear water woodwork is being pulled out;
7. will control in the drying baker that the woodwork of doing is placed on 28-40 degree Celsius and dry 12-24 hour.
2, according to the said a kind of process of bleaching woodwork of claim 1, it is characterized in that the said container that holds liquid lime chloride be metal bucket, mould the bucket or wooden barrel.
CN 03130262 2003-06-26 2003-06-26 Technology for bleaching wooden products and products thereof Expired - Fee Related CN1250379C (en)