CN1183623A - Electric special alloy contact material for low-voltage electric appliance - Google Patents

Electric special alloy contact material for low-voltage electric appliance Download PDF

Info

Publication number
CN1183623A
CN1183623A CN 97125818 CN97125818A CN1183623A CN 1183623 A CN1183623 A CN 1183623A CN 97125818 CN97125818 CN 97125818 CN 97125818 A CN97125818 A CN 97125818A CN 1183623 A CN1183623 A CN 1183623A
Authority
CN
China
Prior art keywords
alloy
contact material
low
carbide
special alloy
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN 97125818
Other languages
Chinese (zh)
Other versions
CN1050215C (en
Inventor
王千
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
HARBIN DONGDAGAO NEW MATERIAL CO Ltd
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN97125818A priority Critical patent/CN1050215C/en
Publication of CN1183623A publication Critical patent/CN1183623A/en
Application granted granted Critical
Publication of CN1050215C publication Critical patent/CN1050215C/en
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Abstract

A special alloy material for making electric contacts in low-voltage electric appliances contains C (0.1-3 Wt.%), vanadium carbide (0.5-5 Wt.%), niobium carbide (0.5-10 Wt.%), zirconium oxide (0.5-5 Wt.%), lanthanum oxide (0.01-1 Wt.%), Te (0.1-1 Wt.%), Pb (0.5-5 Wt.%), Se (0.1-1 Wt.%) and Cu (the rest) and features better electric conductivity, heat conductivity, arc ablating resistance and fusion welding resistance, and excellent antioxidizing and comprehensive natures.

Description

Electric special alloy contact material for low-voltage electric appliance
The invention belongs to a kind of electrical contact material, particularly a kind of electric special alloy contact material for low-voltage electric appliance.
Low-voltage electrical apparatus is a kind of electrical equipment that is of wide application, and its electrical contact then is one of key element of low-voltage electrical apparatus, and its effect is to connect and breaking current.Electrical contact material adopts the silver-base alloy of series such as Ag-Ni, Ag-CdO, Ag-SnO mostly at present, so traditional a large amount of precious metals silver of electrical contact consumption.Therefore, research and applied cost are cheap, and the no silver alloy electrical contact material of dependable performance is significant.For guaranteeing the low-voltage electrical apparatus reliability during operation, electrical contact material must have good electrical conductivity, thermal conductivity, anti-electrical arc erosion and resistance fusion welding, also must have good antioxygenic property simultaneously.For satisfying above-mentioned performance requirement, the novel alloy electrical contact material must be the following a kind of composite material of composition: add a certain amount of high-melting-point in the metallic copper matrix with good heat-conductivity conducting performance, the carbide of high rigidity, oxide are to increase the anti-electrical arc erosion of alloy, the ability of anti-melting welding also will add the non-oxidizability that alloying elements or compound make contact material have certain arc extinguishing ability and improve alloy contact material in addition.
The purpose of this invention is to provide the special alloy electrical contact material that a kind of low-voltage electrical apparatus is used, this kind alloy contact material has good electrical conductivity, thermal conductivity, anti-electrical arc erosion and resistance fusion welding, this alloy material also has excellent non-oxidizability and combination property simultaneously, replaces the silver alloy contact material in low-voltage electrical apparatus.
The low-voltage electrical apparatus that the present invention proposes is (percentage by weight) with the composition proportion of special alloy contact material: carbon 0.1-3; Vanadium carbide 0.5-5; Niobium carbide 0.5-10; Zirconia 0.5-5; Lanthana 0.01-1; Tellurium 0.1-1; Plumbous 0.5-5; Selenium 0.1-1; Copper surplus.
In alloy, add carbon, can improve the anti-electrical arc erosion and the resistance fusion welding of alloy electrical contact.
The carbide that adds high-melting-point high rigidity such as vanadium carbide, niobium carbide in alloy can increase the anti-electrical arc erosion and the resistance fusion welding of alloy electrical contact, when particularly these carbide and carbon add alloy simultaneously, can increase the electric life of alloy electrical contact.
In alloy, add zirconia, lanthana and can increase the arc extinction performance and the resistance fusion welding of alloy electrical contact.
In alloy, add tellurium, selenium, lead, can increase the arc extinction performance of alloy electrical contact.
The advantage of alloy contact material provided by the invention is: have excellent conducting performance, heat conductivility, anti-electrical arc erosion performance and resistance fusion welding, have excellent non-oxidizability and excellent comprehensive performance simultaneously, can replace the silver alloy contact material in the low-voltage electrical apparatus, reduce cost.
Provide embodiment below.
Embodiment 1
The composition of alloy contact material and percentage by weight are:
Carbon 0.1; Vanadium carbide 0.5; Niobium carbide 0.5; Zirconia 0.5; Lanthana 0.01; Tellurium 0.1; Selenium 0.1; Plumbous 0.5; Copper surplus.
The alloy property index:
Resistivity 1.8 μ Ω .cm
Density 8.90g/cm 3
Hardness HB (2.5/62.5) 40
Embodiment 2
The composition of alloy contact material and percentage by weight are:
Carbon 0.2; Vanadium carbide 1; Niobium carbide 0.5; Zirconia 1; Lanthana 0.03; Tellurium 0.2; Selenium 0.2; Plumbous 1; Copper surplus.
The alloy property index:
Resistivity 2.0 μ Ω .cm
Density 8.80g/cm 3
Hardness HB (2.5/62.5) 50
Embodiment 3
The composition of alloy contact material and percentage by weight are:
Carbon 0.5; Vanadium carbide 1.5; Niobium carbide 1; Zirconia 1.5; Lanthana 0.08; Tellurium 0.3; Selenium 0.3; Plumbous 1.5; Copper surplus.
The alloy property index:
Resistivity 2.3 μ Ω .cm
Density 8.73g/cm 3
Hardness HB (2.5/62.5) 62
Embodiment 4
The composition of alloy contact material and percentage by weight are:
Carbon 0.8; Vanadium carbide 2; Niobium carbide 1.5; Zirconia 2; Lanthana 0.1; Tellurium 0.4; Selenium 0.4; Plumbous 2; Copper surplus.
The alloy property index:
Resistivity 2.7 μ Ω .cm
Density 8.63g/cm 3
Hardness HB (2.5/62.5) 64
Embodiment 5
The composition of alloy contact material and percentage by weight are:
Carbon 1; Vanadium carbide 2.5; Niobium carbide 2; Zirconia 2.5; Lanthana 0.2; Tellurium 0.5; Selenium 0.5; Plumbous 2.5; Copper surplus.
The alloy property index:
Resistivity 2.95 μ Ω .cm
Density 8.50g/cm 3
Hardness HB (2.5/62.5) 63
Embodiment 6
The composition of alloy contact material and percentage by weight are:
Carbon 1.5; Vanadium carbide 3; Niobium carbide 4; Zirconia 3; Lanthana 0.5; Tellurium 0.6; Selenium 0.6; Plumbous 3; Copper surplus.
The alloy property index;
Resistivity 3.4 μ Ω .cm
Density 8.42g/cm 3
Hardness HB (2.5/62.5) 63
Embodiment 7
The composition of alloy contact material and percentage by weight are:
Carbon 2; Vanadium carbide 3.5; Niobium carbide 7; Zirconia 3.5; Lanthana 0.8; Tellurium 0.7; Selenium 0.7; Plumbous 5; Copper surplus.
The alloy property index:
Resistivity 3.9 μ Ω .cm
Density 8.40g/cm 3
Hardness HB (2.5/62.5) 70
Embodiment 8
The composition of alloy contact material and percentage by weight are:
Carbon 3; Vanadium carbide 5; Niobium carbide 10; Zirconia 5; Lanthana 1; Tellurium 1; Selenium 1; Plumbous 5; Copper surplus.
The alloy property index:
Resistivity 4.8 μ Ω .cm
Density 8.17g/cm 3
Hardness HB (2.5/62.5) 87

Claims (1)

1, a kind of electric special alloy contact material for low-voltage electric appliance, the composition proportion of its material are (percentage by weight); Carbon 0.1-3; Vanadium carbide 0.5-5; Niobium carbide 0.5-10; Zirconia 0.5-5; Lanthana 0.01-1; Tellurium 0.1-1; Plumbous 0.5-5; Selenium 0.1-1; Copper surplus.
CN97125818A 1997-12-24 1997-12-24 Electric special alloy contact material for low-voltage electric appliance Expired - Lifetime CN1050215C (en)