CN110144657A - A kind of losing fibre preventing cashmere class yarn and its manufacturing method, cashmere class yarn product first product, finished product and its manufacturing method - Google Patents

A kind of losing fibre preventing cashmere class yarn and its manufacturing method, cashmere class yarn product first product, finished product and its manufacturing method Download PDF

Info

Publication number
CN110144657A
CN110144657A CN201910602653.XA CN201910602653A CN110144657A CN 110144657 A CN110144657 A CN 110144657A CN 201910602653 A CN201910602653 A CN 201910602653A CN 110144657 A CN110144657 A CN 110144657A
Authority
CN
China
Prior art keywords
cashmere
yarn
product
manufacturing
mesh belt
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201910602653.XA
Other languages
Chinese (zh)
Inventor
蔡君
李娜
王友
金永乐
高锡光
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
INNER MONGOLIA ORDOS RESOURCE CO Ltd
Original Assignee
INNER MONGOLIA ORDOS RESOURCE CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by INNER MONGOLIA ORDOS RESOURCE CO Ltd filed Critical INNER MONGOLIA ORDOS RESOURCE CO Ltd
Priority to CN201910602653.XA priority Critical patent/CN110144657A/en
Publication of CN110144657A publication Critical patent/CN110144657A/en
Pending legal-status Critical Current

Abstract

The present invention relates to textile technology fields, provide a kind of losing fibre preventing cashmere class yarn, and including the mesh belt with inner cavity and the rove item and thermo-fuse that are filled in mesh belt, rove item is the cashmere sliver or cashmere and wool mixing sliver for having the twist.Additionally provide a kind of manufacturing method of above-mentioned losing fibre preventing cashmere class yarn, comprising: rove item and thermo-fuse are fed while manufacturing mesh belt.The yarn obtained is not easy hair loss, good hand touch after being made into cashmere product hot iron.A kind of manufacturing method of cashmere class yarn product first product, the cashmere yarn that above-mentioned losing fibre preventing cashmere class yarn or the above method manufacture is weaved.A kind of cashmere class yarn product first product is made using above-mentioned manufacturing method, hair loss is not easy after ironing.A kind of manufacturing method of cashmere class yarn product finished product, comprising: by above-mentioned cashmere class yarn product first product ironing.A kind of cashmere class yarn product finished product is made using above-mentioned manufacturing method.The finished product is not easy hair loss, and quality is good.

Description

A kind of losing fibre preventing cashmere class yarn and its manufacturing method, cashmere class yarn product first product, Finished product and its manufacturing method
Technical field
The present invention relates to textile technology field, in particular to a kind of losing fibre preventing cashmere class yarn and its manufacturing method, Cashmere class yarn product first product and its manufacturing method, cashmere class yarn product finished product and its manufacturing method.
Background technique
Currently, cashmere is given the title of " soft gold " by insider as raw material the most precious in textile industry.Mountain Cashmere not only low output but also also more difficult during the extraction process, therefore have to ensure few consumption, sufficiently using cashmere Realize use value;Traditional cashmere class yarn product has preferable feel, but is easy in this way in washing and wearing process The drawbacks of hair loss, this is also cashmere class yarn product;And we are it is desirable that both soft cashmere class yarn systems for being unable to hair loss Product.
In consideration of it, special propose the application.
Summary of the invention
The present invention provides a kind of losing fibre preventing cashmere class yarns and preparation method thereof, it is intended to improve existing cashmere class yarn The problem of easy hair loss after product is made.
The present invention also provides a kind of cashmere class yarn product first product and its manufacturing methods, it is desirable to provide a kind of hot iron It is not easy the cashmere class yarn product of hair loss afterwards.
The present invention also provides a kind of cashmere class yarn product finished product and its manufacturing methods, it is desirable to provide a kind of good hand touch, It is not easy the cashmere class yarn product of hair loss.
The present invention is implemented as follows:
A kind of losing fibre preventing cashmere class yarn, including the mesh belt with inner cavity and the rove item and hot melt that are filled in mesh belt Silk, rove item are the cashmere sliver or cashmere and wool mixing sliver for having the twist.
A kind of manufacturing method of above-mentioned losing fibre preventing cashmere class yarn, comprising:
Rove item and thermo-fuse are fed while manufacturing mesh belt.
A kind of manufacturing method of cashmere class yarn product first product, comprising: by above-mentioned losing fibre preventing cashmere class yarn or above-mentioned side The cashmere yarn that method manufactures is weaved.
A kind of cashmere class yarn product first product is made using above-mentioned manufacturing method.
A kind of manufacturing method of cashmere class yarn product finished product, comprising: by above-mentioned cashmere class yarn product first product 85 ~95 degrees Celsius of lower ironings.
A kind of cashmere class yarn product finished product is made using above-mentioned manufacturing method.
The beneficial effects of the present invention are: the losing fibre preventing cashmere class yarn that the present invention obtains by above-mentioned design, due to will be hot Fuse and rove item containing cashmere are filled in mesh belt, and part cashmere fiber is appeared by the gap of mesh belt, is made The feel that there can be cashmere softness of the losing fibre preventing cashmere class yarn is obtained, losing fibre preventing cashmere class yarn obtained is in subsequent weaving For that thermo-fuse high-temperature digestion milkiness shape therein can be made cashmere fiber when hot iron before factory after cashmere class yarn product Cladding, make it is cooling after in obtained finished product cashmere fiber be not easy it is free fall off, therefore finished product is made in the losing fibre preventing cashmere class yarn Afterwards not only with cashmere feel while but also can effectively avoid cashmere fiber from falling off the cashmere yarn of hair loss.
The present invention obtains the manufacturing method of losing fibre preventing cashmere class yarn by above-mentioned design, simple and convenient, this can be made The losing fibre preventing cashmere class yarn provided is provided.
The manufacturing method for the cashmere class yarn product first product that the present invention obtains by above-mentioned design can be manufactured by weaving Cashmere class yarn product first product is obtained, when which carries out ironing under 85~95 degrees Celsius, thermo-fuse High-temperature digestion is that milkiness shape coats cashmere fiber, so that cashmere fiber is not easy free fall off after the part cooling.
The cashmere class yarn product first product that the present invention obtains by above-mentioned design, first product cashmere after ironing are not easy to dissociate It falls off, and good hand touch.
The manufacturing method for the cashmere class yarn product finished product that the present invention obtains by above-mentioned design, since it uses the present invention It is made after the cashmere class yarn product first product ironing of offer, therefore cashmere class yarn product finished product good hand touch obtained, it is not easy to Hair loss, warmth retention property are good.
The cashmere class yarn product finished product that the present invention obtains by above-mentioned design, due to providing cashmere class yarn using the present invention The manufacturing method of wire work finished product is made, therefore its quality is good.
Detailed description of the invention
It, below will be to use required in embodiment in order to illustrate more clearly of the technical solution of embodiment of the present invention Attached drawing be briefly described, it should be understood that the following drawings illustrates only certain embodiments of the present invention, therefore is not to be seen as It is the restriction to range, it for those of ordinary skill in the art, without creative efforts, can be with root Other relevant attached drawings are obtained according to these attached drawings.
Fig. 1 is the first cross-sectional view for the losing fibre preventing cashmere class yarn that embodiment of the present invention provides;
Fig. 2 is second of cross-sectional view of the losing fibre preventing cashmere class yarn that embodiment of the present invention provides;
Fig. 3 is the micro-structure diagram of the mesh belt for the losing fibre preventing cashmere class yarn that embodiment of the present invention provides.
Icon: 111- mesh belt;112- rove item;113- thermo-fuse;The cashmere fiber that 114- is appeared.
Specific embodiment
It in order to make the object, technical scheme and advantages of the embodiment of the invention clearer, below will be in the embodiment of the present invention Technical solution be clearly and completely described.The person that is not specified actual conditions in embodiment, according to normal conditions or manufacturer builds The condition of view carries out.Reagents or instruments used without specified manufacturer is the conventional production that can be obtained by commercially available purchase Product.
A kind of losing fibre preventing cashmere class yarn, finished product and its manufacturing method, cashmere fabric are provided to the embodiment of the present invention below And clothes are specifically described.
A kind of losing fibre preventing cashmere class yarn provided by the present application including the mesh belt 111 with inner cavity and is filled in the net With the rove item 112 and thermo-fuse 113 in 111, rove item 112 is the cashmere sliver or cashmere and wool hybrid yams for having the twist Item.Part cashmere fiber in the losing fibre preventing cashmere class yarn rove item 112 of the structure can appear mesh belt, visible in figure to appear Cashmere fiber 114.
The structure of finished product losing fibre preventing cashmere class yarn is as depicted in figs. 1 and 2, and Fig. 1 is perpendicular to losing fibre preventing cashmere class yarn Length direction schematic cross-section.Fig. 2 is parallel to the schematic cross-section of the length direction of losing fibre preventing cashmere class yarn.Here The described mesh belt with inner cavity be integrally in pipe dress, in the present invention belt surface texture as shown in Figure 3 or as fishing net texture Similar, the texture that can also be seemed such as most of shoestring surfaces is similar.The specific manufacture of mesh belt is existing in this application There is technology, does not do excessively repeat herein.
The losing fibre preventing cashmere class yarn, since thermo-fuse and rove item containing cashmere to be filled in mesh belt, so that portion Divide cashmere fiber that can appear by the gap of mesh belt, so that the hand that there can be cashmere softness of the losing fibre preventing cashmere class yarn Sense, losing fibre preventing cashmere class yarn obtained weave thermo-fuse therein can be made molten in subsequent ironing after cashmere class yarn product Solution is that milkiness shape coats cashmere fiber, and the cashmere fiber of cooling obtained cashmere class yarn product, which is not easy to dissociate, to fall off, therefore The finished product good hand touch obtained after product through ironing is made in the losing fibre preventing cashmere class yarn, is not easy hair loss.
A kind of manufacturing method of losing fibre preventing cashmere class yarn provided by the present application, comprising:
Rove item and thermo-fuse are fed while manufacturing mesh belt.
Specifically, it to make losing fibre preventing cashmere class yarn matter obtained more preferable, is manufactured using cashmere and wool blended yarns Mesh belt, and in order to further such that losing fibre preventing cashmere class yarn obtained feeling is better, intensity more preferably, manufactures the yarn of mesh belt Metric count be 1/50~1/55Nm;The wool metric count that the yarn of manufacture mesh belt uses is greater than or equal to 100, and length is big In or equal to 35mm, cashmere fiber fineness used in the yarn of mesh belt is manufactured less than or equal to 15.5 μm.
Further, the twist for manufacturing the yarn of mesh belt is 500~600T/M, and mesh belt needle number is fixed as 3 when manufacturing mesh belt ~5 needles.That is, the needle number of manufacture mesh belt is fixed as 3~5 needles.Mesh belt gap size obtained is suitable under this condition, can make It obtains proper amount of cashmere fiber to appear from mesh belt gap, is securely not easy the premise of hair loss in guarantee losing fibre preventing cashmere class yarn texture Under, the rough structure of mesh belt is sufficiently hidden, also can guarantee that the feel of losing fibre preventing cashmere class yarn is the feel of cashmere, is guaranteed anti- The skin-friendly of hair loss cashmere class yarn is good.
Further, more preferable for performances such as the feel of guarantee losing fibre preventing cashmere class yarn and warmth retention properties, manufacture the yarn of mesh belt Line wool content is 65%~75%, and cashmere content is 25%~35%.
While manufacturing mesh belt, the feeding ratio control of rove item is 55~59%, so then makes losing fibre preventing obtained The 55~59% of the total losing fibre preventing cashmere class yarn gross mass of rove Zhan in cashmere class yarn;The feeding ratio control of thermo-fuse exists 3%~10%, so then make the total losing fibre preventing cashmere class yarn gross mass of thermo-fuse Zhan in losing fibre preventing cashmere class yarn obtained 3%~10%.Surplus is then mass ratio shared by mesh belt.When above-mentioned several component contents of composition losing fibre preventing cashmere class yarn are at this When in the range of invention requirement, it further can not only guarantee the feel of losing fibre preventing cashmere class yarn, but also hair loss can be prevented.
Further, the wool in rove item containing 50%~60% cashmere and 40%~50%.It is well known that cashmere its But cost more soft compared to wool is higher than wool, when the wool of incorporation 40%~50% in rove item, can accomplish to drop The feel and warmth retention property of losing fibre preventing cashmere class yarn are not influenced while low manufacturing cost again.
Further, the twist of rove item is 50~80T/M, and the rove item in this twist number range can further avoid Wool or cashmere fiber, which dissociate, to fall off.Preferably, the rove item that item weight is 0.45~0.55g/m is selected to feed net in manufacturing process In band.
Further, the cashmere fiber length in rove item is greater than or equal to 60mm.When cashmere fiber length is greater than or waits When 60mm, rove item is after the combing of miniature carding machine, and fiber is evenly distributed each other and length can be maintained at 40mm or so, in heat It can further prevent cashmere fiber is free to fall off under the action of melten gel.
Further, thermo-fuse is 100% polyamide fibre thermo-fuse.The fusion temperature of polyamide fibre thermo-fuse is 85 degrees Celsius, is compared It is low in other thermo-fuse fusion temperatures, therefore, when thermo-fuse is polyamide fibre thermo-fuse, manufactured using losing fibre preventing cashmere class yarn Product under relatively lower temp ironing also can thermo-fuse be melted, while capable of achieving the effect that losing fibre preventing, moreover it is possible to protect Card cashmere fiber structure is not destroyed, and is further ensured that the feel of final finished product obtained is best.
A kind of manufacturing method of cashmere class yarn product first product, comprising: by losing fibre preventing cashmere class yarn provided by the invention Or the cashmere yarn that manufacturing method provided by the invention manufactures is weaved.
The thermo-fuse contained in losing fibre preventing cashmere class yarn forms milkiness shape liquid in 85~95 degrees Celsius of lower ironing fusings Cashmere fiber is coated, temperature is down to room temperature after cooling, and nylon fibre therein has been uniformly distributed in rove item, by mesh belt Middle cashmere fiber connects, and under the constraint of mesh belt, can effectively prevent cashmere fiber and falls off, so that cashmere class yarn product has Have the characteristics that be not easy hair loss after having ironing.
A kind of cashmere class yarn product first product uses manufacturing method provided by the present application to be made, therefore it is not easy hair loss, Good hand touch.
A kind of manufacturing method of cashmere class yarn product finished product, comprising: will be at the beginning of cashmere class yarn product provided by the invention Product are in 85~95 degrees Celsius of lower ironings.
Since it is that cashmere class yarn product first product provided by the invention is carried out ironing, so that the cashmere class that ironing obtains Yarn product finished product good hand touch, is not easy hair loss.
A kind of cashmere class yarn product finished product, due to the manufacturer using cashmere class yarn product finished product provided by the present application Method manufactures to obtain, therefore its good hand touch, is not easy hair loss.
Below in conjunction with specific embodiment to a kind of losing fibre preventing cashmere class yarn provided by the invention, finished product and its manufacturing method It is specifically described.
Embodiment 1
A kind of manufacturing method of losing fibre preventing cashmere class yarn provided in this embodiment, specifically:
The yarn of 1/52Nm 70% wool, 30% cashmere is selected to manufacture mesh belt, the metric count of the yarn is 1/ 52Nm, the twist for manufacturing the yarn of mesh belt is 500T/M;The wool metric count that the yarn of manufacture mesh belt uses is greater than or equal to 100, length is greater than or equal to 35mm, manufactures cashmere fiber fineness used in the yarn of mesh belt less than or equal to 15.5 μm.
It manufactures the mesh belt hour hands number and is fixed on 3 needles, it is 0.5g/m, ingredient 55% that item weight is fed while manufacturing mesh belt The rove item of cashmere and 45% wool, the feeding ratio of rove item are 55%, and the twist of the rove item is 50T/M, in rove item The length of cashmere fiber is greater than or equal to 60mm.
100% polyamide fibre thermo-fuse is also fed while manufacturing mesh belt, the feed quantity of polyamide fibre thermo-fuse is 3%.
While constantly manufacture mesh belt, losing fibre preventing cashmere class yarn provided in this embodiment is constantly produced.
The present embodiment is obtained into cashmere yarn progress textile process and obtains cashmere yarn product first product.The first product is taken the photograph 85 Ironing obtains cashmere yarn product finished product under family name's degree.
Embodiment 2
A kind of manufacturing method of losing fibre preventing cashmere class yarn provided in this embodiment, specifically:
The yarn of 1/50Nm 65% wool, 35% cashmere is selected to manufacture mesh belt, the metric count of the yarn is 1/ 50Nm, the twist for manufacturing the yarn of mesh belt is 600T/M;The wool metric count that the yarn of manufacture mesh belt uses is greater than or equal to 100, length is greater than or equal to 35mm, manufactures cashmere fiber fineness used in the yarn of mesh belt less than or equal to 15.5 μm.
It manufactures the mesh belt hour hands number and is fixed on 5 needles, it is 0.45g/m that item weight is fed while manufacturing mesh belt, and ingredient is The rove item of 50% cashmere and 50% wool, the feeding ratio of rove item are 59%, and the twist of the rove item is 80T/M, rove The length of cashmere fiber is greater than or equal to 60mm in item.
100% polyamide fibre thermo-fuse is also fed while manufacturing mesh belt, the feed quantity of polyamide fibre thermo-fuse is 10%.
While constantly manufacture mesh belt, losing fibre preventing cashmere class yarn provided in this embodiment is constantly produced.
The present embodiment is obtained into cashmere yarn progress textile process and obtains cashmere yarn product first product.The first product is taken the photograph 90 Ironing obtains cashmere yarn product finished product under family name's degree.
Embodiment 3
A kind of manufacturing method of losing fibre preventing cashmere class yarn provided in this embodiment, specifically:
The yarn of 1/55Nm 75% wool, 25% cashmere is selected to manufacture mesh belt, the metric count of the yarn is 1/ 50Nm, the twist for manufacturing the yarn of mesh belt is 550T/M;The wool metric count that the yarn of manufacture mesh belt uses is greater than or equal to 100, length is greater than or equal to 35mm, manufactures cashmere fiber fineness used in the yarn of mesh belt less than or equal to 15.5 μm.
It manufactures the mesh belt hour hands number and is fixed on 4 needles, it is 0.55g/m that item weight is fed while manufacturing mesh belt, and ingredient is The rove item of 60% cashmere and 40% wool, the feeding ratio of rove item are 57%, and the twist of the rove item is 60T/M, rove The length of cashmere fiber is greater than or equal to 60mm in item.
100% polyamide fibre thermo-fuse is also fed while manufacturing mesh belt, the feed quantity of polyamide fibre thermo-fuse is 5%.
While constantly manufacture mesh belt, losing fibre preventing cashmere class yarn provided in this embodiment is constantly produced.
The present embodiment is obtained into cashmere yarn progress textile process and obtains cashmere yarn product first product.The first product is taken the photograph 95 Ironing obtains cashmere yarn product finished product under family name's degree.
Embodiment 4
A kind of manufacturing method of losing fibre preventing cashmere class yarn provided in this embodiment, specifically:
The yarn of 1/51Nm 72% wool, 28% cashmere is selected to manufacture mesh belt, the metric count of the yarn is 1/ 50Nm, the twist for manufacturing the yarn of mesh belt is 580T/M;The wool metric count that the yarn of manufacture mesh belt uses is greater than or equal to 100, length is greater than or equal to 35mm, manufactures cashmere fiber fineness used in the yarn of mesh belt less than or equal to 15.5 μm.
It manufactures the mesh belt hour hands number and is fixed on 4 needles, it is 0.52g/m that item weight is fed while manufacturing mesh belt, and ingredient is The rove item of 58% cashmere and 42% wool, the feeding ratio of rove item are 56%, and the twist of the rove item is 70T/M, rove The length of cashmere fiber is greater than or equal to 60mm in item.
100% polyamide fibre thermo-fuse is also fed while manufacturing mesh belt, the feed quantity of polyamide fibre thermo-fuse is 7%.
While constantly manufacture mesh belt, losing fibre preventing cashmere class yarn provided in this embodiment is constantly produced.
The present embodiment is obtained into cashmere yarn progress textile process and obtains cashmere yarn product first product.The first product is taken the photograph 85 Ironing obtains cashmere yarn product finished product under family name's degree.
Embodiment 5
A kind of manufacturing method of losing fibre preventing cashmere class yarn provided in this embodiment, specifically:
The yarn of 1/54Nm 68% wool, 32% cashmere is selected to manufacture mesh belt, the metric count of the yarn is 1/ 54Nm, the twist for manufacturing the yarn of mesh belt is 520T/M;The wool metric count that the yarn of manufacture mesh belt uses is greater than or equal to 100, length is greater than or equal to 35mm, manufactures cashmere fiber fineness used in the yarn of mesh belt less than or equal to 15.5 μm.
It manufactures the mesh belt hour hands number and is fixed on 4 needles, it is 0.52g/m that item weight is fed while manufacturing mesh belt, and ingredient is The rove item of 52% cashmere and 48% wool, the feeding ratio of rove item are 56%, and the twist of the rove item is 65T/M, rove The length of cashmere fiber is greater than or equal to 60mm in item.
100% polyamide fibre thermo-fuse is also fed while manufacturing mesh belt, the feed quantity of polyamide fibre thermo-fuse is 8%.
While constantly manufacture mesh belt, losing fibre preventing cashmere class yarn provided in this embodiment is constantly produced.
The present embodiment is obtained into cashmere yarn progress textile process and obtains cashmere yarn product first product.The first product is taken the photograph 85 Ironing obtains cashmere yarn product finished product under family name's degree.
Comparative example 1
This comparative example is mixed with embodiment 1 using rove item and the identical polyamide fibre of identical component, the twist at the same scale Spinning is cashmere yarn.
Comparative example 2
This comparative example is substantially the same manner as Example 1, the difference is that being added without polyamide fibre.
Experimental example 1
Fabric 50g made of losing fibre preventing cashmere class yarn finished product made from Example 1 takes comparative example 1 as experimental group 1 With fabric 50g made of yarn made from comparative example 21, control group 2 as a control group, the top grade of certain commercially available reputable brand is taken Cashmere fabric 50g as a control group 3, experimental group 1, control group 1-3 are washed under the conditions of 40 degree or so and dried after taking.It weighs Experimental group weight after washing.It records to table 1.
Quality after each experimental group washing and drying of table 1
Group Experimental group 1 Control group 1 Control group 2 Control group 3
Quality after experiment 49.23 48.20 37.61 48.50
From table 1, it can be seen that after the washing of fabric made from losing fibre preventing cashmere class yarn finished product made from the embodiment of the present invention Mass lost amount is few, and the fabric quality of control group 1 and control group 2 changes greatly, and explanation can be significant using mesh belt respectively Prevent cashmere fiber is free from falling off, adding hot melt adhesive in the yarn also can significantly prevent cashmere fiber is free to fall off, and the two It interacts indispensable, any factor missing, which is all not achieved significantly, prevents the free effect to fall off of cashmere fiber.It will Experimental group 1 and control group 3 compare, and the fabric quality of control group 3 is significantly lower than experimental group 1, can illustrate that the embodiment of the present application 1 is made The more existing cashmere fabric of fabric made from the losing fibre preventing cashmere class yarn finished product obtained is less susceptible to hair loss depilation.
Experimental example 2
Senior technical staff that 50 are obtained employment 5 years or more in cashmere product production and processing industry is chosen to testing in experimental example 1 The fabric of group 1 and the fabric of control group 3 carry out feel assessment, and give a mark, everyone divides at total score 10, by the total score peace of marking Equal member record is to table 2.
2 experimental group of table marking situation
Group Experimental group 1 Control group 3
Total score 439 446
Average mark 8.78 8.92
From table 2, it can be seen that fabric made of losing fibre preventing cashmere class yarn finished product made from the embodiment of the present application 1 is from total score On see slightly worse than control group 3, and from average mark, the two difference is minimum, almost without gap, illustrate, personally for, Both fabric hand feels are almost the same.Thus, it is possible to illustrate, the good hand touch of losing fibre preventing cashmere class yarn finished product provided by the invention.
In conclusion losing fibre preventing cashmere class yarn provided by the invention is due to filling out thermo-fuse and rove item containing cashmere It fills in mesh belt, part cashmere fiber is appeared by the gap of mesh belt, so that the energy of the losing fibre preventing cashmere class yarn Enough with the feel of cashmere softness, losing fibre preventing cashmere class yarn obtained after subsequent weaving is cashmere class yarn product before dispatching from the factory When hot iron thermo-fuse high-temperature digestion milkiness shape therein can coat cashmere fiber, make in the finished product obtained after cooling Cashmere fiber, which is not easy to dissociate, to fall off, therefore the losing fibre preventing cashmere class yarn is made after finished product not only while having cashmere feel but also energy Cashmere fiber is effectively avoided to fall off the cashmere yarn of hair loss.
The manufacturing method of losing fibre preventing cashmere class yarn provided by the invention, it is simple and convenient, it can be made provided by the invention Losing fibre preventing cashmere class yarn.
The manufacturing method of cashmere class yarn product first product provided by the invention can manufacture to obtain cashmere class yarn by weaving Wire work first product, when which carries out ironing under 85~95 degrees Celsius, thermo-fuse high-temperature digestion is cream Turbid shape coats cashmere fiber, so that cashmere fiber is not easy free fall off after the part cooling.
Cashmere class yarn product first product provided by the invention, first product cashmere after ironing, which is not easy to dissociate, to fall off, and feel It is good.
The manufacturing method of cashmere class yarn product finished product provided by the invention, since it uses cashmere class provided by the invention It is made after yarn product first product ironing, therefore cashmere class yarn product finished product good hand touch obtained, it is not easy to hair loss, warmth retention property It is good.
Cashmere class yarn product finished product provided by the invention, due to providing cashmere class yarn product finished product using the present invention Manufacturing method is made, therefore its quality is good.
The foregoing is merely the preferred embodiment of the present invention, are not intended to restrict the invention, for this field For technical staff, the invention may be variously modified and varied.All within the spirits and principles of the present invention, made any Modification, equivalent replacement, improvement etc., should all be included in the protection scope of the present invention.

Claims (10)

1. a kind of losing fibre preventing cashmere class yarn, which is characterized in that including the mesh belt with inner cavity and be filled in the mesh belt Rove item and thermo-fuse, the rove item are the sliver containing cashmere.
2. losing fibre preventing cashmere class yarn according to claim 1, which is characterized in that the quality of the rove item accounts for described anti- The 55%~59% of hair loss cashmere class yarn gross mass, the quality of the thermo-fuse accounts for the losing fibre preventing cashmere class yarn gross mass 3%~10%.
3. losing fibre preventing cashmere class yarn according to claim 1, which is characterized in that the cashmere and wool mixing sliver contain There is the wool of 50%~60% cashmere and 40%~50%;
Preferably, the twist of the rove item is 50~80T/M;
Preferably, the item weight of the rove item is 0.45~0.55g/m;
Preferably, the cashmere fiber length in the rove item is greater than or equal to 60mm.
4. losing fibre preventing cashmere class yarn according to claim 1, which is characterized in that manufacture the ingredient of the yarn of the mesh belt Including 65%~75% wool and 25%~35% cashmere;
Preferably, the metric count for manufacturing the yarn of the mesh belt is 1/50~1/55Nm;
Preferably, the twist for manufacturing the yarn of the mesh belt is 500~600T/M, and mesh belt needle number is fixed as when producing the mesh belt 3~5 needles;
Preferably, it manufactures the wool metric count that the yarn of the mesh belt uses and is greater than or equal to 100, length is greater than or equal to 35mm manufactures cashmere fiber fineness used in the yarn of the mesh belt less than or equal to 15.5 μm.
5. losing fibre preventing cashmere class yarn according to claim 1, which is characterized in that the thermo-fuse is 100% polyamide fibre heat Fuse.
6. a kind of manufacturing method of losing fibre preventing cashmere class yarn as claimed in any one of claims 1 to 5, which is characterized in that packet It includes:
The rove item and the thermo-fuse are fed while manufacturing the mesh belt.
7. a kind of manufacturing method of cashmere class yarn product first product characterized by comprising will be such as any one of Claims 1 to 5 The cashmere yarn that the losing fibre preventing cashmere class yarn or manufacturing method as claimed in claim 6 manufacture is weaved.
8. a kind of cashmere class yarn product first product, which is characterized in that be made using manufacturing method as claimed in claim 7.
9. a kind of manufacturing method of cashmere class yarn product finished product characterized by comprising by sheep as claimed in claim 8 Suede class yarn product first product is in 85~95 degrees Celsius of lower ironings.
10. a kind of cashmere class yarn product finished product, which is characterized in that be made using manufacturing method as claimed in claim 9.
CN201910602653.XA 2019-07-05 2019-07-05 A kind of losing fibre preventing cashmere class yarn and its manufacturing method, cashmere class yarn product first product, finished product and its manufacturing method Pending CN110144657A (en)