CN109183494A - Impermeable body paper for tobacco-use tipping paper production method - Google Patents

Impermeable body paper for tobacco-use tipping paper production method Download PDF

Info

Publication number
CN109183494A
CN109183494A CN201810830430.4A CN201810830430A CN109183494A CN 109183494 A CN109183494 A CN 109183494A CN 201810830430 A CN201810830430 A CN 201810830430A CN 109183494 A CN109183494 A CN 109183494A
Authority
CN
China
Prior art keywords
paper
page
agent
dosage
tobacco
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201810830430.4A
Other languages
Chinese (zh)
Inventor
翟继岚
都业壮
梁洁
马强
刘春亮
侯丽
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
MUDANJIANG HENGFENG PAPER CO Ltd
Original Assignee
MUDANJIANG HENGFENG PAPER CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by MUDANJIANG HENGFENG PAPER CO Ltd filed Critical MUDANJIANG HENGFENG PAPER CO Ltd
Priority to CN201810830430.4A priority Critical patent/CN109183494A/en
Publication of CN109183494A publication Critical patent/CN109183494A/en
Pending legal-status Critical Current

Abstract

Impermeable body paper for tobacco-use tipping paper production method.A kind of impermeable body paper for tobacco-use tipping paper production method, comprising the following steps: step a, beater floor, using two kinds of bleaching needle-point leaf pulp, bleached hardwood pulp slurries;Double plate grinds continuous beating, bleaching needle-point leaf pulp beating consistency 3.4%~4.4%, 76 ° of SR~78 ° SR of beating degree, weight in wet base 6g~9g, bleached hardwood pulp beating consistency 3.4%~4.4%, beating degree, 74 ° of SR~76 ° SR.Bleaching needle-point leaf pulp is slurried to be slurried with bleached hardwood pulp, in mass ratio 30%~35%:65%~70%, and it is stand-by to be made into mixing slurry.

Description

Impermeable body paper for tobacco-use tipping paper production method
Technical field:
The present invention relates to a kind of impermeable body paper for tobacco-use tipping paper production methods.
Background technique:
Quick-fried pearl type cigarette, which refers to, is embedded with the cigarette of one or two small glue bead of liquid in the tow of filter tip, this small glue bead Interior liquid can make cigarette more raw fragrant during inhaling fair, strengthen fragrance or characteristic, obtain smoker more comfortable Experience.Small glue bead when pinching quick-fried, oil-based liquid in glue bead can outside splash and infiltration, in order to not influence the aesthetics of cigarette, It is required that cigarette filter tip and the tipping paper of cigarette have certain anti-permeability.
Currently on the market with the body paper for tobacco-use tipping paper of impermeable function, paper-dope spreading technique is mostly used to assign impermeable Performance, and the body paper for tobacco-use tipping paper two sides otherness after paper-dope spreading is larger, so that there is serious edge warpage and shows in page As to influence upper machine performance.In addition, paper-dope spreading will increase equipment input cost, while increase secondary specification loss, cause Unit cost is sharply increased.It realizes that on-line coater assigns body paper for tobacco-use tipping paper anti-permeability, makes body paper surfacing, thin It is greasy, machine adaptability on body paper is improved, production is easily controllable, and reduces the unit cost of production.
Summary of the invention:
The object of the present invention is to provide a kind of impermeable body paper for tobacco-use tipping paper production methods.
Above-mentioned purpose is realized by following technical scheme:
A kind of impermeable body paper for tobacco-use tipping paper production method, comprising the following steps:
Step a, beater floor, using two kinds of bleaching needle-point leaf pulp, bleached hardwood pulp slurries;Double plate grinds continuous beating, Bleaching needle-point leaf pulp beating consistency 3.4%~4.4%, 76 ° of SR~78 ° SR of beating degree, weight in wet base 6g~9g, bleached hardwood pulp Beating consistency 3.4%~4.4%, beating degree, 74 ° of SR~76 ° SR, bleaching needle-point leaf pulp is slurried to be slurried with bleached hardwood pulp, It is stand-by to be made into mixing slurry for 30%~35%:65%~70% in mass ratio;
Step b, copy paper workshop section continuously attaches filler, neutral sizing agent into the mixing slurry prepared, and attaches cationic shallow lake The double base retention agent of powder and CPAM composition, for slurry after wet end and press section drainage and formation, l Water Paper page enters preceding dry stage progress Drying, then applied agent machine to page two sides while be coated;
Step c, coating process, printing surface table apply oxidized starch, and non-printed side table applies PVA and food-grade oil-proofing agent;Oxidation Starch prepares concentration 4%, and oil-proofing agent prepares concentration 3%, PVA preparation concentration be 8%, PVA and the mass ratio of oil-proofing agent be 1~ 3:1~3, the page after coating continue to dry, and carry out press polish using page of one of soft press-polishing machine to drying, produce impermeable Body paper for tobacco-use tipping paper;
Step d, the solid content of neutral sizing agent is 15%, and dosage is opposite oven dry stock 1.0%~3.0%, is controlled with it The water imbibition of body paper for tobacco-use tipping paper processed meets printing demand and cigarette demand;
Step e, the degree of substitution 0.020~0.040 of cationic starch, dosage are opposite oven dry stock 0.5%~1.5%, The molecular weight of CPAM is 6,000,000~8,000,000, and dosage is opposite oven dry stock 0.01%~0.03%, and composition double base Retention Aid System mentions The retention rate of high fiber fines and filler;
Step f, it is 2.5 μm~3.5 μm that filler, which selects partial size, and arsenic content≤1.0mg/kg calcium carbonate, dosage is opposite Oven dry stock 12%~20%;
Step g, body paper for tobacco-use tipping paper surface treatment is carried out using one soft press-polishing machine, 105 DEG C of calender temperature, line pressure Power is 105kN/m~110kN/m, at the control of paper printing surface smoothness between 400s~600s.
A kind of impermeable body paper for tobacco-use tipping paper production method, comprising the following steps:
Step a, beater floor, using two kinds of bleaching needle-point leaf pulp, bleached hardwood pulp slurries;Double plate grinds continuous beating, Bleaching needle-point leaf pulp beating consistency 3.4%~4.4%, 76 ° of SR~78 ° SR of beating degree, weight in wet base 6g~9g, bleached hardwood pulp Beating consistency 3.4%~4.4%, beating degree, 74 ° of SR~76 ° SR;Bleaching needle-point leaf pulp is slurried to be slurried with bleached hardwood pulp, It is stand-by to be made into mixing slurry for 30%~35%:65%~70% in mass ratio;
Step b, copy paper workshop section continuously attaches filler, neutral sizing agent into the mixing slurry prepared, and attaches cationic shallow lake The double base retention agent of powder and CPAM composition, for slurry after wet end and press section drainage and formation, l Water Paper page enters preceding dry stage progress Drying, then applied agent machine to page two sides while be coated;
Step c, coating process, printing surface table apply oxidized starch, and it is anti-that non-printed side table applies oxidized starch, PVA and food-grade Finish;Printing surface oxidized starch prepares concentration 4%, and non-printed side oxidized starch prepares concentration 10%, and oil-proofing agent prepares concentration It is 5% that 5%, PVA, which prepare concentration,;The mass ratio of oxidized starch and PVA, oil-proofing agent are 1:1:1.5, and the page after coating continues to dry It is dry, press polish is carried out using page of one of soft press-polishing machine to drying, produces impermeable body paper for tobacco-use tipping paper;
Step d, the solid content of neutral sizing agent is 15%, and dosage is opposite oven dry stock 1.0%~3.0%, is controlled with it The water imbibition of body paper for tobacco-use tipping paper processed meets printing demand and cigarette demand;
Step e, the degree of substitution 0.020~0.040 of cationic starch, dosage are opposite oven dry stock 0.5%~1.5%, The molecular weight of CPAM is 6,000,000~8,000,000, and dosage is opposite oven dry stock 0.01%~0.03%, and composition double base Retention Aid System mentions The retention rate of high fiber fines and filler;
Step f, it is 2.5 μm~3.5 μm that filler, which selects partial size, and arsenic content≤1.0mg/kg calcium carbonate, dosage is opposite Oven dry stock 12%~20%;
Step g, body paper for tobacco-use tipping paper surface treatment is carried out using one soft press-polishing machine, 105 DEG C of calender temperature, line pressure Power is 105kN/m~110kN/m, at the control of paper printing surface smoothness between 400s~600s.
The utility model has the advantages that
1. impermeable body paper for tobacco-use tipping paper is produced using agent machine coating method is applied, it is another in non-printed side coating oil-proofing agent One face table applies oxidized starch, body paper two sides while rewetting, and moisture is relatively uniform consistent compared with paper-dope spreading, moisture when dry heated It distributes, is not in that grease proofing infiltration grade is detected by 559 standard method of TAPPI, can achieve 8 toward side warping phenomenon Grade or more, and page is smooth, fine and smooth, smooth, low by calender body paper roughness after ornamenting of pressurizeing, can achieve 2.40 μm with Under, ink good leveling property when being printed on the machine, color contrast is strong, picture and text are full, glossy, because disposably having produced in paper machine At, without carrying out paper-dope spreading, the expenses such as the equipment purchase cost and personnel's operation, water power vapour for avoiding paper-dope spreading consume With manufacturing cost is low, and product cutting specifications control is flexible, is lost without trimming again, meets large industrialized production requirement, product Sale obtains fine benefit, obtains commercial success.
2. the impermeable body paper for tobacco-use tipping paper produced using this method, in addition to assigning impermeable (i.e. grease proofing) function of body paper Other than energy, more prominent feature is that very big variation also has occurred in the ink penetration of body paper printing surface, in printing ink transfer amount base In the case where, detection printing permeability index is greatly lowered for this, and limited ink is made more to be retained in body paper printing Surface, so that effectively preventing the ink often occurred in previous printing process carries on the back saturating problem, it can improve press quality, again Dirty roller problem is overcome, printing efficiency is greatly improved.
3. a very crucial technology of impermeable body paper for tobacco-use tipping paper of the invention is exactly to use on the machine performance, usability It can include the sudden and violent mouth of mouth stick, picking etc., the present invention successfully solves these and uses on the machine performance issue, antiseepage produced by the invention Saturating body paper for tobacco-use tipping paper, which uses on the machine, not to lose powder, the advantages that circumference is good while also effectively preventing frequent in previous printing process The ink of appearance carries on the back saturating problem, it can improves press quality, and overcomes dirty roller problem, meets large industrialized production and want It asks, greatly improves printing efficiency.
Specific embodiment:
Embodiment 1:
The present embodiment is the technique that printing surface is coated with oxidized starch using non-printed side coating PVA and food-grade oil-proofing agent Mode produces the body paper for tobacco-use tipping paper that front meets printing and reverse side has anti-permeability requirement, specific production step It is rapid as follows:
A kind of impermeable body paper for tobacco-use tipping paper production method, comprising the following steps:
Step a, beater floor, using two kinds of bleaching needle-point leaf pulp, bleached hardwood pulp slurries;Double plate grinds continuous beating, Bleaching needle-point leaf pulp beating consistency 3.4%~4.4%, 76 ° of SR~78 ° SR of beating degree, weight in wet base 6g~9g, bleached hardwood pulp Beating consistency 3.4%~4.4%, beating degree, 74 ° of SR~76 ° SR, bleaching needle-point leaf pulp is slurried to be slurried with bleached hardwood pulp, It is stand-by to be made into mixing slurry for 30%~35%:65%~70% in mass ratio;
Step b, copy paper workshop section continuously attaches filler, neutral sizing agent into the mixing slurry prepared, and attaches cationic shallow lake The double base retention agent of powder and CPAM composition, for slurry after wet end and press section drainage and formation, l Water Paper page enters preceding dry stage progress Drying, then applied agent machine to page two sides while be coated;
Step c, coating process, printing surface table apply oxidized starch, and non-printed side table applies PVA and food-grade oil-proofing agent;Oxidation Starch prepares concentration 4%, and oil-proofing agent prepares concentration 3%, PVA preparation concentration be 8%, PVA and the mass ratio of oil-proofing agent be 1~ 3:1~3, the page after coating continue to dry, and carry out press polish using page of one of soft press-polishing machine to drying, produce impermeable Body paper for tobacco-use tipping paper;
Step d, the solid content of neutral sizing agent is 15%, and dosage is opposite oven dry stock 1.0%~3.0%, is controlled with it The water imbibition of body paper for tobacco-use tipping paper processed meets printing demand and cigarette demand;
Step e, the degree of substitution 0.020~0.040 of cationic starch, dosage are opposite oven dry stock 0.5%~1.5%, The molecular weight of CPAM is 6,000,000~8,000,000, and dosage is opposite oven dry stock 0.01%~0.03%, and composition double base Retention Aid System mentions The retention rate of high fiber fines and filler;
Step f, it is 2.5 μm~3.5 μm that filler, which selects partial size, and arsenic content≤1.0mg/kg calcium carbonate, dosage is opposite Oven dry stock 12%~20%;
Step g, body paper for tobacco-use tipping paper surface treatment is carried out using one soft press-polishing machine, 105 DEG C of calender temperature, line pressure Power is 105kN/m~110kN/m, at the control of paper printing surface smoothness between 400s~600s.
Embodiment 2:
The present embodiment is the technique that printing surface is coated with oxidized starch using non-printed side coating PVA and food-grade oil-proofing agent Mode produces the body paper for tobacco-use tipping paper that front meets printing and reverse side has anti-permeability requirement, specific production step It is rapid as follows:
A kind of impermeable body paper for tobacco-use tipping paper production method, comprising the following steps:
Step a, beater floor, using two kinds of bleaching needle-point leaf pulp, bleached hardwood pulp slurries;Double plate grinds continuous beating, Bleaching needle-point leaf pulp beating consistency 3.4%~4.4%, 76 ° of SR~78 ° SR of beating degree, weight in wet base 6g~9g, bleached hardwood pulp Beating consistency 3.4%~4.4%, beating degree, 74 ° of SR~76 ° SR;Bleaching needle-point leaf pulp is slurried to be slurried with bleached hardwood pulp, It is stand-by to be made into mixing slurry for 30%~35%:65%~70% in mass ratio;
Step b, copy paper workshop section continuously attaches filler, neutral sizing agent into the mixing slurry prepared, and attaches cationic shallow lake The double base retention agent of powder and CPAM composition, for slurry after wet end and press section drainage and formation, l Water Paper page enters preceding dry stage progress Drying, then applied agent machine to page two sides while be coated;
Step c, coating process, printing surface table apply oxidized starch, and non-printed side table applies PVA and food-grade oil-proofing agent;Oxidation Starch prepares concentration 4%, and oil-proofing agent prepares concentration 3%, and PVA preparation concentration is 5%, PVA and the mass ratio of oil-proofing agent is 2: 1.5 or 1:1, the page after coating continue to dry, and carry out press polish using page of one of soft press-polishing machine to drying, produce antiseepage Saturating body paper for tobacco-use tipping paper;
Step d, the solid content of neutral sizing agent is 15%, and dosage is opposite oven dry stock 1.0%~3.0%, is controlled with it The water imbibition of body paper for tobacco-use tipping paper processed meets printing demand and cigarette demand;
Step e, the degree of substitution 0.020~0.040 of cationic starch, dosage are opposite oven dry stock 0.5%~1.5%, The molecular weight of CPAM is 6,000,000~8,000,000, and dosage is opposite oven dry stock 0.01%~0.03%, and composition double base Retention Aid System mentions The retention rate of high fiber fines and filler;
Step f, it is 2.5 μm~3.5 μm that filler, which selects partial size, and arsenic content≤1.0mg/kg calcium carbonate, dosage is opposite Oven dry stock 12%~20%;
Step g, body paper for tobacco-use tipping paper surface treatment is carried out using one soft press-polishing machine, 105 DEG C of calender temperature, line pressure Power is 105kN/m~110kN/m, at the control of paper printing surface smoothness between 400s~600s.
Embodiment 3:
The present embodiment is using non-printed side coating oxidized starch, PVA and food-grade oil-proofing agent, and printing surface table applies oxidation and forms sediment The technology mode of powder produces the body paper for tobacco-use tipping paper that front meets printing and reverse side has anti-permeability, specific raw Steps are as follows for production:
A kind of impermeable body paper for tobacco-use tipping paper production method, comprising the following steps:
Step a, beater floor, using two kinds of bleaching needle-point leaf pulp, bleached hardwood pulp slurries;Double plate grinds continuous beating, Bleaching needle-point leaf pulp beating consistency 3.4%~4.4%, 76 ° of SR~78 ° SR of beating degree, weight in wet base 6g~9g, bleached hardwood pulp Beating consistency 3.4%~4.4%, beating degree, 74 ° of SR~76 ° SR;Bleaching needle-point leaf pulp is slurried to be slurried with bleached hardwood pulp, It is stand-by to be made into mixing slurry for 30%~35%:65%~70% in mass ratio;
Step b, copy paper workshop section continuously attaches filler, neutral sizing agent into the mixing slurry prepared, and attaches cationic shallow lake The double base retention agent of powder and CPAM composition, for slurry after wet end and press section drainage and formation, l Water Paper page enters preceding dry stage progress Drying, then applied agent machine to page two sides while be coated;
Step c, coating process, printing surface table applies oxidized starch, while non-printed side table applies oxidized starch, adds PVA With food-grade oil-proofing agent, printing surface oxidized starch prepares concentration 4%, and it is 12% that non-printed side oxidized starch, which prepares concentration, grease proofing Agent preparation concentration is that 3%, PVA preparation concentration is 3%;The mass ratio of oxidized starch and PVA, oil-proofing agent are 1:2:1, after coating Page continues to dry, and carries out press polish using page of one of soft press-polishing machine to drying, produces impermeable body paper for tobacco-use tipping paper;
Step d, the solid content of neutral sizing agent is 15%, and dosage is opposite oven dry stock 1.0%~3.0%, is controlled with it The water imbibition of body paper for tobacco-use tipping paper processed meets printing demand and cigarette demand;
Step e, the degree of substitution 0.020~0.040 of cationic starch, dosage are opposite oven dry stock 0.5%~1.5%, The molecular weight of CPAM is 6,000,000~8,000,000, and dosage is opposite oven dry stock 0.01%~0.03%, and composition double base Retention Aid System mentions The retention rate of high fiber fines and filler;
Step f, it is 2.5 μm~3.5 μm that filler, which selects partial size, and arsenic content≤1.0mg/kg calcium carbonate, dosage is opposite Oven dry stock 12%~20%;
Step g, body paper for tobacco-use tipping paper surface treatment is carried out using one soft press-polishing machine, 105 DEG C of calender temperature, line pressure Power is 105kN/m~110kN/m, at the control of paper printing surface smoothness between 400s~600s.
The impermeable body paper for tobacco-use tipping paper of this method production use on the machine do not lose powder, smoke pipe notch is neat, circumference is good etc. Advantage also effectively prevents the ink often occurred in previous printing process simultaneously and carries on the back saturating problem, it can press quality is improved, Dirty roller problem is overcome again.
Embodiment 4:
The present embodiment is using non-printed side coating oxidized starch, PVA and food-grade oil-proofing agent, and printing surface coating oxidation is formed sediment The technology mode of powder produces the body paper for tobacco-use tipping paper that front meets printing and reverse side has anti-permeability requirement, tool Body production stage is as follows:
A kind of impermeable body paper for tobacco-use tipping paper production method, comprising the following steps:
Step a, beater floor, using two kinds of bleaching needle-point leaf pulp, bleached hardwood pulp slurries;Double plate grinds continuous beating, Bleaching needle-point leaf pulp beating consistency 3.4%~4.4%, 76 ° of SR~78 ° SR of beating degree, weight in wet base 6g~9g, bleached hardwood pulp Beating consistency 3.4%~4.4%, beating degree, 74 ° of SR~76 ° SR;Bleaching needle-point leaf pulp is slurried to be slurried with bleached hardwood pulp, It is stand-by to be made into mixing slurry for 30%~35%:65%~70% in mass ratio;
Step b, copy paper workshop section continuously attaches filler, neutral sizing agent into the mixing slurry prepared, and attaches cationic shallow lake The double base retention agent of powder and CPAM composition, for slurry after wet end and press section drainage and formation, l Water Paper page enters preceding dry stage progress Drying, then applied agent machine to page two sides while be coated;
Step c, coating process, printing surface table apply oxidized starch, and it is anti-that non-printed side table applies oxidized starch, PVA and food-grade Finish;Printing surface oxidized starch prepares concentration 4%, and non-printed side oxidized starch prepares concentration 10%, and oil-proofing agent prepares concentration It is 5% that 5%, PVA, which prepare concentration,;The mass ratio of oxidized starch and PVA, oil-proofing agent are 1:1:1.5, and the page after coating continues to dry It is dry, press polish is carried out using page of one of soft press-polishing machine to drying, produces impermeable body paper for tobacco-use tipping paper;
Step d, the solid content of neutral sizing agent is 15%, and dosage is opposite oven dry stock 1.0%~3.0%, is controlled with it The water imbibition of body paper for tobacco-use tipping paper processed meets printing demand and cigarette demand;
Step e, the degree of substitution 0.020~0.040 of cationic starch, dosage are opposite oven dry stock 0.5%~1.5%, The molecular weight of CPAM is 6,000,000~8,000,000, and dosage is opposite oven dry stock 0.01%~0.03%, and composition double base Retention Aid System mentions The retention rate of high fiber fines and filler;
Step f, it is 2.5 μm~3.5 μm that filler, which selects partial size, and arsenic content≤1.0mg/kg calcium carbonate, dosage is opposite Oven dry stock 12%~20%;
Step g, body paper for tobacco-use tipping paper surface treatment is carried out using one soft press-polishing machine, 105 DEG C of calender temperature, line pressure Power is 105kN/m~110kN/m, at the control of paper printing surface smoothness between 400s~600s.
The impermeable body paper for tobacco-use tipping paper of this method production use on the machine do not lose powder, smoke pipe notch is neat, circumference is good etc. Advantage also effectively prevents the ink often occurred in previous printing process simultaneously and carries on the back saturating problem, it can press quality is improved, Dirty roller problem is overcome again.
Embodiment 5:
The present embodiment is the technique that printing surface is coated with oxidized starch using non-printed side coating PVA and food-grade oil-proofing agent Mode produces the body paper for tobacco-use tipping paper that front meets printing and reverse side has anti-permeability requirement, specific production step It is rapid as follows:
A kind of impermeable body paper for tobacco-use tipping paper production method, comprising the following steps:
Step a, beater floor, using two kinds of bleaching needle-point leaf pulp, bleached hardwood pulp slurries;Double plate grinds continuous beating, Bleaching needle-point leaf pulp beating consistency 4%, 77 ° of SR of beating degree, weight in wet base 8g, bleached hardwood pulp beating consistency 4%, beating degree, 75 ° SR, bleaching needle-point leaf pulp is slurried to be slurried with bleached hardwood pulp, and it is stand-by to be made into mixing slurry by 33%:67% in mass ratio;
Step b, copy paper workshop section continuously attaches filler, neutral sizing agent into the mixing slurry prepared, and attaches cationic shallow lake The double base retention agent of powder and CPAM composition, for slurry after wet end and press section drainage and formation, l Water Paper page enters preceding dry stage progress Drying, then applied agent machine to page two sides while be coated;
Step c, coating process, printing surface table apply oxidized starch, and non-printed side table applies PVA and food-grade oil-proofing agent;Oxidation Starch prepares concentration 4%, and oil-proofing agent prepares concentration 3%, and PVA preparation concentration is 8%, PVA and the mass ratio of oil-proofing agent is 1:1, Page after coating continues to dry, and carries out press polish to the page of drying using one of soft press-polishing machine, produces impermeable cigarette with connecing Fill paper body paper;
Step d, the solid content of neutral sizing agent is 15%, and dosage is opposite oven dry stock 2.0%, and cigarette is controlled with it with connecing The water imbibition for filling paper body paper, meets printing demand and cigarette demand;
Step e, the degree of substitution 0.030 of cationic starch, dosage are opposite oven dry stock 1.0%, and the molecular weight of CPAM is 700 Ten thousand, dosage is opposite oven dry stock 0.02%, and composition double base Retention Aid System improves the retention rate of fiber fines and filler;
Step f, it is 3 μm that filler, which selects partial size, and arsenic content≤1.0mg/kg calcium carbonate, dosage is opposite oven dry stock 18%;
Step g, body paper for tobacco-use tipping paper surface treatment is carried out using one soft press-polishing machine, 105 DEG C of calender temperature, line pressure Power is 108kN/m, at the control of paper printing surface smoothness between 500s.
Embodiment 6:
The present embodiment is the technique that printing surface is coated with oxidized starch using non-printed side coating PVA and food-grade oil-proofing agent Mode produces the body paper for tobacco-use tipping paper that front meets printing and reverse side has anti-permeability requirement, specific production step It is rapid as follows:
A kind of impermeable body paper for tobacco-use tipping paper production method, comprising the following steps:
Step a, beater floor, using two kinds of bleaching needle-point leaf pulp, bleached hardwood pulp slurries;Double plate grinds continuous beating, Bleaching needle-point leaf pulp beating consistency 4%, 77 ° of SR of beating degree, weight in wet base 7g, bleached hardwood pulp beating consistency 4%, beating degree, 75 ° SR;Bleaching needle-point leaf pulp is slurried to be slurried with bleached hardwood pulp, and it is stand-by to be made into mixing slurry by 34%:66% in mass ratio;
Step b, copy paper workshop section continuously attaches filler, neutral sizing agent into the mixing slurry prepared, and attaches cationic shallow lake The double base retention agent of powder and CPAM composition, for slurry after wet end and press section drainage and formation, l Water Paper page enters preceding dry stage progress Drying, then applied agent machine to page two sides while be coated;
Step c, coating process, printing surface table apply oxidized starch, and non-printed side table applies PVA and food-grade oil-proofing agent;Oxidation Starch prepares concentration 4%, and oil-proofing agent prepares concentration 3%, and PVA preparation concentration is 5%, PVA and the mass ratio of oil-proofing agent is 2: 1.5, the page after coating continues to dry, and carries out press polish using page of one of soft press-polishing machine to drying, produces impermeable cigarette Use base paper for tipping paper;
Step d, the solid content of neutral sizing agent is 15%, and dosage is opposite oven dry stock 2.0%, and cigarette is controlled with it with connecing The water imbibition for filling paper body paper, meets printing demand and cigarette demand;
Step e, the degree of substitution 0.030 of cationic starch, dosage are opposite oven dry stock 1.2%, and the molecular weight of CPAM is 7000000, dosage is opposite oven dry stock 0.02%, and composition double base Retention Aid System improves the retention rate of fiber fines and filler;
Step f, it is 3.0 μm that filler, which selects partial size, and arsenic content≤1.0mg/kg calcium carbonate, dosage is opposite oven dry stock 18%;
Step g, body paper for tobacco-use tipping paper surface treatment is carried out using one soft press-polishing machine, 105 DEG C of calender temperature, line pressure Power is 107kN/m, at the control of paper printing surface smoothness between 500s.
Embodiment 7:
The present embodiment is using non-printed side coating oxidized starch, PVA and food-grade oil-proofing agent, and printing surface table applies oxidation and forms sediment The technology mode of powder produces the body paper for tobacco-use tipping paper that front meets printing and reverse side has anti-permeability, specific raw Steps are as follows for production:
A kind of impermeable body paper for tobacco-use tipping paper production method, comprising the following steps:
Step a, beater floor, using two kinds of bleaching needle-point leaf pulp, bleached hardwood pulp slurries;Double plate grinds continuous beating, Bleaching needle-point leaf pulp beating consistency 4%, 77 ° of SR of beating degree, weight in wet base 7g, bleached hardwood pulp beating consistency 4%, beating degree, 75 ° SR;Bleaching needle-point leaf pulp is slurried to be slurried with bleached hardwood pulp, and it is stand-by to be made into mixing slurry by 33%:67% in mass ratio;
Step b, copy paper workshop section continuously attaches filler, neutral sizing agent into the mixing slurry prepared, and attaches cationic shallow lake The double base retention agent of powder and CPAM composition, for slurry after wet end and press section drainage and formation, l Water Paper page enters preceding dry stage progress Drying, then applied agent machine to page two sides while be coated;
Step c, coating process, printing surface table applies oxidized starch, while non-printed side table applies oxidized starch, adds PVA With food-grade oil-proofing agent, printing surface oxidized starch prepares concentration 4%, and it is 12% that non-printed side oxidized starch, which prepares concentration, grease proofing Agent preparation concentration is that 3%, PVA preparation concentration is 3%;The mass ratio of oxidized starch and PVA, oil-proofing agent are 1:2:1, after coating Page continues to dry, and carries out press polish using page of one of soft press-polishing machine to drying, produces impermeable body paper for tobacco-use tipping paper;
Step d, the solid content of neutral sizing agent is 15%, and dosage is opposite oven dry stock 1.0%~3.0%, is controlled with it The water imbibition of body paper for tobacco-use tipping paper processed meets printing demand and cigarette demand;
Step e, the degree of substitution 0.030 of cationic starch, dosage are opposite oven dry stock 0.9%, and the molecular weight of CPAM is 7000000, dosage is opposite oven dry stock 0.02%, and composition double base Retention Aid System improves the retention rate of fiber fines and filler;
Step f, it is 2.8 μm that filler, which selects partial size, and arsenic content≤1.0mg/kg calcium carbonate, dosage is opposite oven dry stock 16%;
Step g, body paper for tobacco-use tipping paper surface treatment is carried out using one soft press-polishing machine, 105 DEG C of calender temperature, line pressure Power is 107kN/m, at the control of paper printing surface smoothness between 500s.
The impermeable body paper for tobacco-use tipping paper of this method production use on the machine do not lose powder, smoke pipe notch is neat, circumference is good etc. Advantage also effectively prevents the ink often occurred in previous printing process simultaneously and carries on the back saturating problem, it can press quality is improved, Dirty roller problem is overcome again.
Embodiment 8:
The present embodiment is using non-printed side coating oxidized starch, PVA and food-grade oil-proofing agent, and printing surface coating oxidation is formed sediment The technology mode of powder produces the body paper for tobacco-use tipping paper that front meets printing and reverse side has anti-permeability requirement, tool Body production stage is as follows:
A kind of impermeable body paper for tobacco-use tipping paper production method, comprising the following steps:
Step a, beater floor, using two kinds of bleaching needle-point leaf pulp, bleached hardwood pulp slurries;Double plate grinds continuous beating, Bleaching needle-point leaf pulp beating consistency 4%, 77 ° of SR of beating degree, weight in wet base 8g, bleached hardwood pulp beating consistency 3.9%, beating degree, 75°SR;Bleaching needle-point leaf pulp is slurried to be slurried with bleached hardwood pulp, and it is stand-by to be made into mixing slurry by 32%:68% in mass ratio;
Step b, copy paper workshop section continuously attaches filler, neutral sizing agent into the mixing slurry prepared, and attaches cationic shallow lake The double base retention agent of powder and CPAM composition, for slurry after wet end and press section drainage and formation, l Water Paper page enters preceding dry stage progress Drying, then applied agent machine to page two sides while be coated;
Step c, coating process, printing surface table apply oxidized starch, and it is anti-that non-printed side table applies oxidized starch, PVA and food-grade Finish;Printing surface oxidized starch prepares concentration 4%, and non-printed side oxidized starch prepares concentration 10%, and oil-proofing agent prepares concentration It is 5% that 5%, PVA, which prepare concentration,;The mass ratio of oxidized starch and PVA, oil-proofing agent are 1:1:1.5, and the page after coating continues to dry It is dry, press polish is carried out using page of one of soft press-polishing machine to drying, produces impermeable body paper for tobacco-use tipping paper;
Step d, the solid content of neutral sizing agent is 15%, and dosage is opposite oven dry stock 1.0%~3.0%, is controlled with it The water imbibition of body paper for tobacco-use tipping paper processed meets printing demand and cigarette demand;
Step e, the degree of substitution 0.030 of cationic starch, dosage are opposite oven dry stock 1.0%, and the molecular weight of CPAM is 7000000, dosage is opposite oven dry stock 0.02%, and composition double base Retention Aid System improves the retention rate of fiber fines and filler;
Step f, it is 3 μm that filler, which selects partial size, and arsenic content≤1.0mg/kg calcium carbonate, dosage is opposite oven dry stock 15%;
Step g, body paper for tobacco-use tipping paper surface treatment is carried out using one soft press-polishing machine, 105 DEG C of calender temperature, line pressure Power is 108kN/m, at the control of paper printing surface smoothness between 500s.
The impermeable body paper for tobacco-use tipping paper of this method production use on the machine do not lose powder, smoke pipe notch is neat, circumference is good etc. Advantage also effectively prevents the ink often occurred in previous printing process simultaneously and carries on the back saturating problem, it can press quality is improved, Dirty roller problem is overcome again.
Embodiment 9:
The impermeable body paper for tobacco-use tipping paper produced using this method, in addition to assigning impermeable (i.e. grease proofing) function of body paper In addition, more prominent feature is that very big variation also has occurred in the ink penetration of body paper printing surface.It is basic in printing ink transfer amount In the case where, detection printing permeability index is greatly lowered, and limited ink is made more to be retained in body paper printing table Face, so that effectively preventing the ink often occurred in previous printing process carries on the back saturating problem, it can raising press quality, and gram Dirty roller problem has been taken, printing efficiency is greatly improved.
The impermeable body paper for tobacco-use tipping paper method of inspection, executes according to following standard procedures:

Claims (8)

1. a kind of impermeable body paper for tobacco-use tipping paper production method, characterized in that the following steps are included:
Step a, beater floor, using two kinds of bleaching needle-point leaf pulp, bleached hardwood pulp slurries;Double plate grinds continuous beating, bleaching Softwood pulp beating consistency 3.4%~4.4%, 76 ° of SR~78 ° SR of beating degree, weight in wet base 6g~9g, bleached hardwood pulp beating consistency 3.4%~4.4%, beating degree, 74 ° of SR~76 ° SR, bleaching needle-point leaf pulp is slurried to be slurried with bleached hardwood pulp, and in mass ratio 30% ~35%:65%~70%, it is stand-by to be made into mixing slurry;
Step b, copy paper workshop section continuously attaches filler, neutral sizing agent into the mixing slurry prepared, and attach cationic starch with CPAM composition double base retention agent, slurry after wet end and press section drainage and formation, l Water Paper page enter the preceding dry stage dried, Agent machine is applied again to page two sides while being coated;
Step c, coating process, printing surface table apply oxidized starch, and non-printed side table applies PVA and food-grade oil-proofing agent;Oxidized starch Concentration 4% is prepared, oil-proofing agent prepares concentration 3%, and PVA preparation concentration is 8%, PVA and the mass ratio of oil-proofing agent is 1~3:1~3, is applied Page after cloth continues to dry, and carries out press polish using page of one of soft press-polishing machine to drying, produces impermeable cigarette Paper body paper;
Step d, the solid content of neutral sizing agent is 15%, and dosage is opposite oven dry stock 1.0%~3.0%, and cigarette is controlled with it with connecing The water imbibition for filling paper body paper, meets printing demand and cigarette demand;
Step e, the degree of substitution 0.020~0.040 of cationic starch, dosage are opposite oven dry stock 0.5%~1.5%, point of CPAM Son amount is 6,000,000~8,000,000, and dosage is opposite oven dry stock 0.01%~0.03%, and composition double base Retention Aid System improves fiber fines And the retention rate of filler;
Step f, it is 2.5 μm~3.5 μm that filler, which selects partial size, and arsenic content≤1.0mg/kg calcium carbonate, dosage is opposite over dry Slurry 12%~20%;
Step g, body paper for tobacco-use tipping paper surface treatment, calender temperature 105 are carried out using one of soft press-polishing machine0C, line pressure are 105kN/m~110kN/m, at the control of paper printing surface smoothness between 400s~600s.
2. impermeable body paper for tobacco-use tipping paper production method according to claim 1, characterized in that the following steps are included:
Step a, beater floor, using two kinds of bleaching needle-point leaf pulp, bleached hardwood pulp slurries;Double plate grinds continuous beating, bleaching Softwood pulp beating consistency 3.4%~4.4%, 76 ° of SR~78 ° SR of beating degree, weight in wet base 6g~9g, bleached hardwood pulp beating consistency 3.4%~4.4%, beating degree, 74 ° of SR~76 ° SR;Bleaching needle-point leaf pulp is slurried to be slurried with bleached hardwood pulp, and in mass ratio 30% ~35%:65%~70%, it is stand-by to be made into mixing slurry;
Step b, copy paper workshop section continuously attaches filler, neutral sizing agent into the mixing slurry prepared, and attach cationic starch with CPAM composition double base retention agent, slurry after wet end and press section drainage and formation, l Water Paper page enter the preceding dry stage dried, Agent machine is applied again to page two sides while being coated;
Step c, coating process, printing surface table apply oxidized starch, and non-printed side table applies PVA and food-grade oil-proofing agent;Oxidized starch Concentration 4% is prepared, oil-proofing agent prepares concentration 3%, and PVA preparation concentration is 5%, PVA and the mass ratio of oil-proofing agent is 2:1.5 or 1:1, Page after coating continues to dry, and carries out press polish to the page of drying using one of soft press-polishing machine, produces impermeable cigarette with connecing Fill paper body paper;
Step d, the solid content of neutral sizing agent is 15%, and dosage is opposite oven dry stock 1.0%~3.0%, and cigarette is controlled with it with connecing The water imbibition for filling paper body paper, meets printing demand and cigarette demand;
Step e, the degree of substitution 0.020~0.040 of cationic starch, dosage are opposite oven dry stock 0.5%~1.5%, point of CPAM Son amount is 6,000,000~8,000,000, and dosage is opposite oven dry stock 0.01%~0.03%, and composition double base Retention Aid System improves fiber fines And the retention rate of filler;
Step f, it is 2.5 μm~3.5 μm that filler, which selects partial size, and arsenic content≤1.0mg/kg calcium carbonate, dosage is opposite over dry Slurry 12%~20%;
Step g, body paper for tobacco-use tipping paper surface treatment, calender temperature 105 are carried out using one of soft press-polishing machine0C, line pressure are 105kN/m~110kN/m, at the control of paper printing surface smoothness between 400s~600s.
3. impermeable body paper for tobacco-use tipping paper production method according to claim 1, characterized in that the following steps are included:
Step a, beater floor, using two kinds of bleaching needle-point leaf pulp, bleached hardwood pulp slurries;Double plate grinds continuous beating, bleaching Softwood pulp beating consistency 3.4%~4.4%, 76 ° of SR~78 ° SR of beating degree, weight in wet base 6g~9g, bleached hardwood pulp beating consistency 3.4%~4.4%, beating degree, 74 ° of SR~76 ° SR;Bleaching needle-point leaf pulp is slurried to be slurried with bleached hardwood pulp, and in mass ratio 30% ~35%:65%~70%, it is stand-by to be made into mixing slurry;
Step b, copy paper workshop section continuously attaches filler, neutral sizing agent into the mixing slurry prepared, and attach cationic starch with CPAM composition double base retention agent, slurry after wet end and press section drainage and formation, l Water Paper page enter the preceding dry stage dried, Agent machine is applied again to page two sides while being coated;
Step c, coating process, printing surface table applies oxidized starch, while non-printed side table applies oxidized starch, adds PVA and food Grade oil-proofing agent, printing surface oxidized starch prepare concentration 4%, and it is 12% that non-printed side oxidized starch, which prepares concentration, oil-proofing agent preparation Concentration is that 3%, PVA preparation concentration is 3%;The mass ratio of oxidized starch and PVA, oil-proofing agent are 1:2:1, and the page after coating continues Drying carries out press polish using page of one of soft press-polishing machine to drying, produces impermeable body paper for tobacco-use tipping paper;
Step d, the solid content of neutral sizing agent is 15%, and dosage is opposite oven dry stock 1.0%~3.0%, and cigarette is controlled with it with connecing The water imbibition for filling paper body paper, meets printing demand and cigarette demand;
Step e, the degree of substitution 0.020~0.040 of cationic starch, dosage are opposite oven dry stock 0.5%~1.5%, point of CPAM Son amount is 6,000,000~8,000,000, and dosage is opposite oven dry stock 0.01%~0.03%, and composition double base Retention Aid System improves fiber fines And the retention rate of filler;
Step f, it is 2.5 μm~3.5 μm that filler, which selects partial size, and arsenic content≤1.0mg/kg calcium carbonate, dosage is opposite over dry Slurry 12%~20%;
Step g, body paper for tobacco-use tipping paper surface treatment, calender temperature 105 are carried out using one of soft press-polishing machine0C, line pressure are 105kN/m~110kN/m, at the control of paper printing surface smoothness between 400s~600s.
4. impermeable body paper for tobacco-use tipping paper production method according to claim 1, characterized in that the following steps are included:
Step a, beater floor, using two kinds of bleaching needle-point leaf pulp, bleached hardwood pulp slurries;Double plate grinds continuous beating, bleaching Softwood pulp beating consistency 3.4%~4.4%, 76 ° of SR~78 ° SR of beating degree, weight in wet base 6g~9g, bleached hardwood pulp beating consistency 3.4%~4.4%, beating degree, 74 ° of SR~76 ° SR;Bleaching needle-point leaf pulp is slurried to be slurried with bleached hardwood pulp, and in mass ratio 30% ~35%:65%~70%, it is stand-by to be made into mixing slurry;
Step b, copy paper workshop section continuously attaches filler, neutral sizing agent into the mixing slurry prepared, and attach cationic starch with CPAM composition double base retention agent, slurry after wet end and press section drainage and formation, l Water Paper page enter the preceding dry stage dried, Agent machine is applied again to page two sides while being coated;
Step c, coating process, printing surface table apply oxidized starch, and non-printed side table applies oxidized starch, PVA and food-grade oil-proofing agent; Printing surface oxidized starch prepares concentration 4%, and non-printed side oxidized starch prepares concentration 10%, and oil-proofing agent prepares concentration 5%, PVA preparation Concentration is 5%;The mass ratio of oxidized starch and PVA, oil-proofing agent are 1:1:1.5, and the page after coating continues to dry, using together Soft press-polishing machine carries out press polish to the page of drying, produces impermeable body paper for tobacco-use tipping paper;
Step d, the solid content of neutral sizing agent is 15%, and dosage is opposite oven dry stock 1.0%~3.0%, and cigarette is controlled with it with connecing The water imbibition for filling paper body paper, meets printing demand and cigarette demand;
Step e, the degree of substitution 0.020~0.040 of cationic starch, dosage are opposite oven dry stock 0.5%~1.5%, point of CPAM Son amount is 6,000,000~8,000,000, and dosage is opposite oven dry stock 0.01%~0.03%, and composition double base Retention Aid System improves fiber fines And the retention rate of filler;
Step f, it is 2.5 μm~3.5 μm that filler, which selects partial size, and arsenic content≤1.0mg/kg calcium carbonate, dosage is opposite over dry Slurry 12%~20%;
Step g, body paper for tobacco-use tipping paper surface treatment, calender temperature 105 are carried out using one of soft press-polishing machine0C, line pressure are 105kN/m~110kN/m, at the control of paper printing surface smoothness between 400s~600s.
5. impermeable body paper for tobacco-use tipping paper production method according to claim 1, characterized in that the following steps are included:
Step a, beater floor, using two kinds of bleaching needle-point leaf pulp, bleached hardwood pulp slurries;Double plate grinds continuous beating, bleaching Softwood pulp beating consistency 4%, 77 ° of SR of beating degree, weight in wet base 8g, bleached hardwood pulp beating consistency 4%, beating degree, 75 ° of SR, drift White softwood pulp is slurried to be slurried with bleached hardwood pulp, and it is stand-by to be made into mixing slurry by 33%:67% in mass ratio;
Step b, copy paper workshop section continuously attaches filler, neutral sizing agent into the mixing slurry prepared, and attach cationic starch with CPAM composition double base retention agent, slurry after wet end and press section drainage and formation, l Water Paper page enter the preceding dry stage dried, Agent machine is applied again to page two sides while being coated;
Step c, coating process, printing surface table apply oxidized starch, and non-printed side table applies PVA and food-grade oil-proofing agent;Oxidized starch Concentration 4% is prepared, oil-proofing agent prepares concentration 3%, and PVA preparation concentration is 8%, PVA and the mass ratio of oil-proofing agent is 1:1, after coating Page continues to dry, and carries out press polish using page of one of soft press-polishing machine to drying, produces impermeable body paper for tobacco-use tipping paper;
Step d, the solid content of neutral sizing agent is 15%, and dosage is opposite oven dry stock 2.0%, and cigarette tipping paper original is controlled with it The water imbibition of paper meets printing demand and cigarette demand;
Step e, the degree of substitution 0.030 of cationic starch, dosage are opposite oven dry stock 1.0%, and the molecular weight of CPAM is 7,000,000, are used Amount is opposite oven dry stock 0.02%, and composition double base Retention Aid System improves the retention rate of fiber fines and filler;
Step f, it is 3 μm that filler, which selects partial size, and arsenic content≤1.0mg/kg calcium carbonate, dosage is opposite oven dry stock 18%;
Step g, body paper for tobacco-use tipping paper surface treatment, calender temperature 105 are carried out using one of soft press-polishing machine0C, line pressure are 108kN/m, at the control of paper printing surface smoothness between 500s.
6. impermeable body paper for tobacco-use tipping paper production method according to claim 1, characterized in that the following steps are included:
Step a, beater floor, using two kinds of bleaching needle-point leaf pulp, bleached hardwood pulp slurries;Double plate grinds continuous beating, bleaching Softwood pulp beating consistency 4%, 77 ° of SR of beating degree, weight in wet base 7g, bleached hardwood pulp beating consistency 4%, beating degree, 75 ° of SR;Drift White softwood pulp is slurried to be slurried with bleached hardwood pulp, and it is stand-by to be made into mixing slurry by 34%:66% in mass ratio;
Step b, copy paper workshop section continuously attaches filler, neutral sizing agent into the mixing slurry prepared, and attach cationic starch with CPAM composition double base retention agent, slurry after wet end and press section drainage and formation, l Water Paper page enter the preceding dry stage dried, Agent machine is applied again to page two sides while being coated;
Step c, coating process, printing surface table apply oxidized starch, and non-printed side table applies PVA and food-grade oil-proofing agent;Oxidized starch Concentration 4% is prepared, oil-proofing agent prepares concentration 3%, and PVA preparation concentration is 5%, PVA and the mass ratio of oil-proofing agent is 2:1.5, after coating Page continue to dry, press polish is carried out to the page of drying using one of soft press-polishing machine, it is former to produce impermeable cigarette tipping paper Paper;
Step d, the solid content of neutral sizing agent is 15%, and dosage is opposite oven dry stock 2.0%, and cigarette tipping paper original is controlled with it The water imbibition of paper meets printing demand and cigarette demand;
Step e, the degree of substitution 0.030 of cationic starch, dosage are opposite oven dry stock 1.2%, and the molecular weight of CPAM is 7,000,000, are used Amount is opposite oven dry stock 0.02%, and composition double base Retention Aid System improves the retention rate of fiber fines and filler;
Step f, it is 3.0 μm that filler, which selects partial size, and arsenic content≤1.0mg/kg calcium carbonate, dosage is opposite oven dry stock 18%;
Step g, body paper for tobacco-use tipping paper surface treatment, calender temperature 105 are carried out using one of soft press-polishing machine0C, line pressure are 107kN/m, at the control of paper printing surface smoothness between 500s.
7. impermeable body paper for tobacco-use tipping paper production method according to claim 1, characterized in that the following steps are included:
Step a, beater floor, using two kinds of bleaching needle-point leaf pulp, bleached hardwood pulp slurries;Double plate grinds continuous beating, bleaching Softwood pulp beating consistency 4%, 77 ° of SR of beating degree, weight in wet base 7g, bleached hardwood pulp beating consistency 4%, beating degree, 75 ° of SR;Drift White softwood pulp is slurried to be slurried with bleached hardwood pulp, and it is stand-by to be made into mixing slurry by 33%:67% in mass ratio;
Step b, copy paper workshop section continuously attaches filler, neutral sizing agent into the mixing slurry prepared, and attach cationic starch with CPAM composition double base retention agent, slurry after wet end and press section drainage and formation, l Water Paper page enter the preceding dry stage dried, Agent machine is applied again to page two sides while being coated;
Step c, coating process, printing surface table applies oxidized starch, while non-printed side table applies oxidized starch, adds PVA and food Grade oil-proofing agent, printing surface oxidized starch prepare concentration 4%, and it is 12% that non-printed side oxidized starch, which prepares concentration, oil-proofing agent preparation Concentration is that 3%, PVA preparation concentration is 3%;The mass ratio of oxidized starch and PVA, oil-proofing agent are 1:2:1, and the page after coating continues Drying carries out press polish using page of one of soft press-polishing machine to drying, produces impermeable body paper for tobacco-use tipping paper;
Step d, the solid content of neutral sizing agent is 15%, and dosage is opposite oven dry stock 1.0%~3.0%, and cigarette is controlled with it with connecing The water imbibition for filling paper body paper, meets printing demand and cigarette demand;
Step e, the degree of substitution 0.030 of cationic starch, dosage are opposite oven dry stock 0.9%, and the molecular weight of CPAM is 7,000,000, are used Amount is opposite oven dry stock 0.02%, and composition double base Retention Aid System improves the retention rate of fiber fines and filler;
Step f, it is 2.8 μm that filler, which selects partial size, and arsenic content≤1.0mg/kg calcium carbonate, dosage is opposite oven dry stock 16%;
Step g, body paper for tobacco-use tipping paper surface treatment, calender temperature 105 are carried out using one of soft press-polishing machine0C, line pressure are 107kN/m, at the control of paper printing surface smoothness between 500s.
8. impermeable body paper for tobacco-use tipping paper production method according to claim 1, characterized in that the following steps are included:
Step a, beater floor, using two kinds of bleaching needle-point leaf pulp, bleached hardwood pulp slurries;Double plate grinds continuous beating, bleaching Softwood pulp beating consistency 4%, 77 ° of SR of beating degree, weight in wet base 8g, bleached hardwood pulp beating consistency 3.9%, beating degree, 75 ° of SR; Bleaching needle-point leaf pulp is slurried to be slurried with bleached hardwood pulp, and it is stand-by to be made into mixing slurry by 32%:68% in mass ratio;
Step b, copy paper workshop section continuously attaches filler, neutral sizing agent into the mixing slurry prepared, and attach cationic starch with CPAM composition double base retention agent, slurry after wet end and press section drainage and formation, l Water Paper page enter the preceding dry stage dried, Agent machine is applied again to page two sides while being coated;
Step c, coating process, printing surface table apply oxidized starch, and non-printed side table applies oxidized starch, PVA and food-grade oil-proofing agent; Printing surface oxidized starch prepares concentration 4%, and non-printed side oxidized starch prepares concentration 10%, and oil-proofing agent prepares concentration 5%, PVA preparation Concentration is 5%;The mass ratio of oxidized starch and PVA, oil-proofing agent are 1:1:1.5, and the page after coating continues to dry, using together Soft press-polishing machine carries out press polish to the page of drying, produces impermeable body paper for tobacco-use tipping paper;
Step d, the solid content of neutral sizing agent is 15%, and dosage is opposite oven dry stock 1.0%~3.0%, and cigarette is controlled with it with connecing The water imbibition for filling paper body paper, meets printing demand and cigarette demand;
Step e, the degree of substitution 0.030 of cationic starch, dosage are opposite oven dry stock 1.0%, and the molecular weight of CPAM is 7,000,000, are used Amount is opposite oven dry stock 0.02%, and composition double base Retention Aid System improves the retention rate of fiber fines and filler;
Step f, it is 3 μm that filler, which selects partial size, and arsenic content≤1.0mg/kg calcium carbonate, dosage is opposite oven dry stock 15%;
Step g, body paper for tobacco-use tipping paper surface treatment, calender temperature 105 are carried out using one of soft press-polishing machine0C, line pressure are 108kN/m, at the control of paper printing surface smoothness between 500s.
CN201810830430.4A 2018-07-26 2018-07-26 Impermeable body paper for tobacco-use tipping paper production method Pending CN109183494A (en)