CN109181541A - A kind of colour raw lacquer and the preparation method and application thereof, a kind of craftwork - Google Patents

A kind of colour raw lacquer and the preparation method and application thereof, a kind of craftwork Download PDF

Info

Publication number
CN109181541A
CN109181541A CN201810844973.1A CN201810844973A CN109181541A CN 109181541 A CN109181541 A CN 109181541A CN 201810844973 A CN201810844973 A CN 201810844973A CN 109181541 A CN109181541 A CN 109181541A
Authority
CN
China
Prior art keywords
lacquer
raw lacquer
colored
mineral powder
oil
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201810844973.1A
Other languages
Chinese (zh)
Inventor
李东旭
刘帅
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
XI'AN RAW URUSHI COATING RESEARCH INSTITUTE ALL CHINA FEDERATION OF SUPPLY AND
Original Assignee
XI'AN RAW URUSHI COATING RESEARCH INSTITUTE ALL CHINA FEDERATION OF SUPPLY AND
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by XI'AN RAW URUSHI COATING RESEARCH INSTITUTE ALL CHINA FEDERATION OF SUPPLY AND filed Critical XI'AN RAW URUSHI COATING RESEARCH INSTITUTE ALL CHINA FEDERATION OF SUPPLY AND
Priority to CN201810844973.1A priority Critical patent/CN109181541A/en
Publication of CN109181541A publication Critical patent/CN109181541A/en
Pending legal-status Critical Current

Abstract

The present invention provides a kind of colored raw lacquer, belong to modern paint technical field.Colored raw lacquer of the invention includes following components in percentage by weight: transparent lacquer 30~45%, solvent naphtha 40~55%, mineral powder 10~20%.Colour raw lacquer provided by the invention is colorful, elegant nature;Application method is simple and efficient.

Description

A kind of colour raw lacquer and the preparation method and application thereof, a kind of craftwork
Technical field
The present invention relates to a kind of modern paint technical fields, more particularly to are a kind of colored raw lacquer and preparation method thereof and answer With a kind of, craftwork.
Background technique
China be find earliest in the world and using raw lacquer country.It is recorded according to ancient documents, China uses lacquerware earliest Time limit, which can push away, traced back to the Neolithic Age, and before 8000, the ancients of across lake one band of bridge of Hangzhou Xiaoshan are to the performance of paint It has gained some understanding and begins to use.It is unearthed in the lacquerware " paint bow " across the ruins Hu Qiao, is the lacquerware of earliest extant." paint bow " is unearthed Millennium has been pushed ahead into paint culture, has been known as " source of paint " of China.In China, paint skill had brilliant history, Craft and techniques are various, and exquisite workmanship is marvellous.Shang and Zhou Dynasty be always or usually as specified coat with lacquer lacquerware and gold, silver, jewel inlays skill;Spring and autumn The Warring States Period has colored drawing and folder ramie skill, is graduallyd mature using the technology of raw lacquer, produces miscellaneous lacquerware, color is gorgeous Beautiful, moulding is exquisite;The Han Dynasty, people, which have grasped, to embossed lacquer, bores that picture, technologies, the production of lacquerware such as gold, gold and silver mistake are more smart in an opposite direction Beauty.Early Medieval China period, the production of lacquerware turn to development in terms of the art work, the various lofty and steep appearance of technology.To the Tang Dynasty, ramie is pressed from both sides Technology is widely used in figure of buddha production, and skill reaches its maturity, and has grasped carved lacquerware, flat de- technology.Song, the mother-of-pearl inlay edge in first period It is embedding, the embedding patch skill and technique of goldleaf is most characteristic, has arrived bright, clear two generation, coat with lacquer paint skill and technique and be more up to 14 classes, lacquerware technology reaches unprecedented High development.
Since reforming and opening up to the outside world with China, economic prosperity and development improve the living standard of our people increasingly, substance Life Basis is abundant, and the public selection to art is increasingly diversified, and huge change also has occurred in aesthetic pattern and temperament and interest therewith.So And for these years, the lacquerware product in China is all the track of an overturned cart for following Qing Dynasty's industrial art from device shape to decorations are coated with lacquer, and is only imitated, and is made It is extremely overelaborated in skill and technique, time-consuming work consuming;And the needs of the modern life are also seldom considered on its color and type, color is dark and gloomy It is old-fashioned and inflexible, or even departing from the life of modern.
Summary of the invention
In view of this, the purpose of the present invention is to provide a kind of colored raw lacquer and the preparation method and application thereof, a kind of technique Product.Colour raw lacquer provided by the invention is colorful, elegant nature;Application method is simple and efficient, does not have technology to staff It is required that.
In order to achieve the above-mentioned object of the invention, the present invention the following technical schemes are provided:
The present invention provides a kind of colored raw lacquer, including following components in percentage by weight: transparent lacquer 30~45%, molten Agent oil 40~55%, mineral powder 10~20%.
Preferably, the solvent naphtha includes one of tung oil, turpentine oil and camphorated oil or a variety of.
Preferably, the partial size of the mineral powder is 1000~1500 mesh.
Preferably, the mineral powder includes cinnabar, realgar or green pine.
The present invention also provides the preparation methods of colour raw lacquer described in above-mentioned technical proposal, comprising the following steps:
(1) it grinds, filter after mixing mineral powder with partial solvent oil, obtain color;
(2) it grinds, filter after mixing the color that the step (1) obtains with transparent lacquer, obtain colored paint;
(3) it is filtered after mixing the colored paint that the step (2) obtains with residual solvent oil, obtains colored raw lacquer.
Preferably, the mass ratio of color and transparent lacquer is 1:1 in the step (2).
The present invention also provides colour raw lacquer described in above-mentioned technical proposal in life appliance, building decoration, furniture furnishings, public affairs The application of art, electronic product, toy for children and field of vehicles altogether.
The present invention also provides a kind of craftwork, the craftwork includes the colored raw lacquer.
The present invention provides a kind of colored raw lacquer, including following components in percentage by weight: transparent lacquer 30~45%, molten Agent oil 40~55%, mineral powder 10~20%.Mineral powder of the invention provides beautiful color, solvent naphtha conduct for colored raw lacquer Transparent lacquer and mineral powder can be mixed into uniform system by dicyandiamide solution.Colored raw lacquer of the invention is colorful, it is elegant from So;Method is simple when in use, time saving and energy saving, and the pattern of formation is elegant naturally, its decorative pattern has natural and smooth gesture, and speckle floats It is like nature itself rich in the rhythm, and its smooth in appearance, it is colorful gorgeous.
Detailed description of the invention
Fig. 1 is the picture of casket prepared by embodiment 1;
Fig. 2 is the picture of casket prepared by comparative example 2.
Specific embodiment
The present invention provides a kind of colored raw lacquer, including following components in percentage by weight: transparent lacquer 30~45%, molten Agent oil 40~55%, mineral powder 10~20%.
It is provided by the invention colour raw lacquer include weight percent be 30~45% transparent lacquer, preferably 32~ 43%, more preferably 35~40%.The present invention does not have special restriction to the source of the transparent lacquer, using art technology Commercial product known to personnel.In the present invention, the transparent lacquer is main base, can be improved the viscous of colored raw lacquer Property and transparency.
It is provided by the invention colour raw lacquer include weight percent be 40~55% solvent naphtha, preferably 43~52%, More preferably 45~50%.In the present invention, the solvent naphtha preferably includes one of tung oil, turpentine oil and camphorated oil or more Kind.In the present invention, when the solvent naphtha is mixture, the present invention is to the weight ratio of each substance in the mixture without spy Different restriction, using any weight ratio.In the present invention, the solvent naphtha plays the role of the transparent lacquer of dilution, simultaneously It can be improved the brightness of colored raw lacquer.
It is provided by the invention colour raw lacquer include weight percent be 10~20% mineral powder, preferably 12~18%, More preferably 14~16%.In the present invention, the partial size of the mineral powder is preferably 1000~1500 mesh, more preferably 1100~ 1400 mesh, most preferably 1200~1300 mesh.The present invention does not have special restriction, art technology to the type of the mineral powder Personnel select as needed, specifically, such as cinnabar, realgar or green pine.In the present invention, the mineral powder can add The color of deep colour raw lacquer.
The present invention also provides the preparation methods of colour raw lacquer described in above-mentioned technical proposal, comprising the following steps:
(1) it grinds, filter after mixing mineral powder with partial solvent oil, obtain color;
(2) it grinds, filter after mixing the color that the step (1) obtains with transparent lacquer, obtain colored paint;
(3) it is filtered after mixing the colored paint that the step (2) obtains with residual solvent oil, obtains colored raw lacquer.
Grinding, filtering, obtain color after the present invention mixes mineral powder with partial solvent oil.Time of the present invention to grinding And speed does not limit, if mineral powder is sufficiently finely ground, and no granular sensation can be mixed with solvent naphtha.In the present invention In, the filtering is preferably filtered using 300 mesh filter paper.
After obtaining color, grinding, filtering, obtain colored paint after the present invention mixes color with transparent lacquer.In the present invention, The mass ratio of the color and transparent lacquer is preferably 1:1.In the present invention, the filtering is preferably carried out using 300 mesh filter paper Filtering.In the present invention, the transparent lacquer is handled using preceding preferably through filter.
After obtaining colored paint, the present invention filters after mixing colored paint with residual solvent oil, obtains colored raw lacquer.The present invention is to institute The mode for stating mixing does not have special restriction, using hybrid mode well known to those skilled in the art, specifically, such as stirring It mixes.
The present invention is to the mass ratio of the mineral powder and partial solvent oil, the mass ratio of partial solvent oil and residual solvent oil There is no special restriction, those skilled in the art select according to actual needs, and meet the total amount ratio of mineral powder, solvent naphtha ?.
The present invention also provides colour raw lacquer described in above-mentioned technical proposal in life appliance, building decoration, furniture furnishings, public affairs The application of art, electronic product, toy for children and field of vehicles altogether.
The present invention also provides a kind of craftwork, the craftwork includes the colored raw lacquer.
In the present invention, the preparation method of the craftwork, preferably includes following steps:
(a) colored raw lacquer is put into water container and carries out dialling paint, obtain flowing lacquer painting;
(b) paint is floated after the carcass after bottoming being immersed water container and shade is done, and obtains the ornaments of colored raw lacquer modification.
Colored raw lacquer is put into water container and dials paint by the present invention, obtains flowing lacquer painting.
In the present invention, the length, width and height of the water container are preferably 3~6 times of carcass length, width and height, more preferably 3.5~ 5.5 times, most preferably 4~5 times.In the present invention, the amount of being filled with water in the water container is preferably 80~90%.In the present invention In, described group of paint preferably includes to pour into alcohol on the water surface in water container, pours into colored raw lacquer, and it is light to dial, obtain flowing lacquer painting.
After obtaining flowing lacquer painting, the present invention floats paint after the carcass after bottoming is immersed water container and shade is done, and obtains colored life Paint the ornaments of modification.In the present invention, the drift paint preferably includes after being pressed into carcass under flowing lacquer painting, proposes carcass.? In the present invention, the shady dry temperature is preferably 25 DEG C, and the shady dry humidity is preferably 75%, and the shady dry time is preferred For 36h.In the present invention, it preferably carries out wiping after shade is dry clear.In the present invention, described wipe is preferably included in clearly jewelry surface erasing Layer of transparent lacquer.
In the present invention, the carcass after the bottoming is preferably obtained using following steps: by raw lacquer 1000 mesh dark greys of reconciliation It scrapes on carcass, then brush raw lacquer, shade is dry, the carcass after obtaining bottoming.
In the present invention, it since colored raw lacquer is not soluble in water, bubbles through the water column, the carcass after bottoming is placed in flowing lacquer painting Under, flowing lacquer painting waterborne is attached to naturally on the carcass after bottoming, and because flowing lacquer painting waterborne by bamboo chip is stirred and is There is flowing grain pattern, finally forms pattern beautiful in colour, that shape is elegant on bottoming carcass.Using colored raw lacquer of the invention The method for modifying ornaments is easy, does not have the requirement of technical aspect to staff.
Colored raw lacquer provided by the invention and the preparation method and application thereof, a kind of craftwork are carried out below with reference to embodiment Detailed description, but they cannot be interpreted as limiting the scope of the present invention.
Embodiment 1
By taking the wooden tire casket as an example
It is a kind of colour raw lacquer include following components in percentage by weight: transparent lacquer 36%, 16% part of tung oil, camphorated oil 28%, mineral powder 20%;Transparent lacquer is filtered using preceding using 300 mesh filter paper, removal of impurities.
The preparation method of above-mentioned colour raw lacquer includes: that (1) mixes mineral powder with tung oil, and grinding uniformly, is filtered using 300 mesh Paper filtering, obtains color;
(2) color is mixed with transparent lacquer according to 1:1, grinding uniformly, forms colored paint;
(3) colored paint is mixed with camphorated oil, is filtered using 500 mesh filter paper, obtains colored raw lacquer.
Using obtained colored raw lacquer preparation process product, i.e., the wooden tire casket;The wood tire casket is long: 20.5cm, width: The wooden tire casket of 16cm, height: 16cm close the wooden tire box cover and drawer opening from inside, need to fit together perfectly, spare;
(1) raw lacquer 1000 mesh dark greys of reconciliation are scraped on the wooden tire, priming, shade is dry, the wooden tire jewellery after obtaining bottoming Box;
(2) in a length of 70cm, width 60cm, the water of injection 4/5, is used in the water container of a height of 60cm;On the water surface successively 90ml alcohol and colored raw lacquer are poured into, using the light water repellent face of bamboo chip, obtains flowing lacquer painting;
(3) it by the wooden tire casket indentation water container after bottoming, proposes, is 25 DEG C in temperature, the ring that humidity is 75% Shady dry 36h, is wiped clearly by traditional handicraft under border, obtains the wooden tire casket of colored raw lacquer modification.
The wooden tire casket of gained colour raw lacquer modification is as shown in Figure 1, as can be seen from Figure 1: smooth in appearance, decorative pattern are natural Flowing is rich in variation, colorful gorgeous, highest quality.
Using adhesive force traditional test methods, the adhesive force of colored raw lacquer and ornaments is determined, test result is ASTM etc. Grade: 4B;It is observed by cross-hatching, there are small pieces to peel off in notch intersection damaged no more than 5% in the area Hua Ge.
Comparative example
The group of colored raw lacquer is divided into transparent lacquer, mineral powder and tung oil 4:4:2 in mass ratio and is mixed to get.
The preparation method of colored raw lacquer includes mixing transparent lacquer, mineral powder with tung oil, and grinding uniformly, is filtered with 100 mesh Paper filtering, removes impurity, obtains colored raw lacquer;
The colored raw lacquer preparation process product that will be prepared, i.e., the wooden tire casket, comprising the following steps:
(a) bottoming scrapes raw lacquer 1000 mesh dark greys of reconciliation on the wooden tire, and priming, shade is dry, the wood after obtaining bottoming Tire;
(b) original text is opened up, the rough sketch drawn is opened up on jewellery box top, it is spare;
(c) graining is integrally overlying on thereon using plastic film with hooking pen according to one of pattern thickness bluing paint, adjusts pleat Wrinkle, takes film off after shade is dry, washes away residual paint with gasoline, continues shady dry;
(d) dusting, with hooking pen along the transparent lacquer of rough sketch brush together, spread that 40 mesh are dilute to spread yellow paint powder on it, shade is dry;
(e) solid powder brushes transparent lacquer together (protective paint powder prevents from falling off) after shade is dry, shade is dry;
(f) paint is coated with lacquer, coats with lacquer red colored paint together, shade is dry;Coat with lacquer yellow colored paint together, shade is dry;Coat with lacquer red colored paint together, shade is dry;
(g) it corrects, corrects graining with scalpel or other tools and repeatedly coat with lacquer rough sketch caused by paint and lose partially;
(h) it repeats, by the process of step 3 to step 8, be sequentially completed left and right side and front-back coats with lacquer painting process;
(i) cover paint, after the completion of the coating with lacquer and apply process of each face of casket, using the transparent lacquer three of hair brush piece cover, shade is dry;
(j) polish, successively with 240 mesh, 360 mesh, 600 mesh, 1000 mesh, 1500 mesh, 2000 mesh, 3000 mesh waterproof abrasive paper from It is thick to polish to thin;
(k) light is pushed away, vegetable oil (soybean oil, peanut oil etc.) 5mL is added on casket, then spread 5000 mesh dark greys, with hair Group Tui Guang tri-;
(l) it wipes clear, is stained with transparent lacquer with cotton yarn hard waste and dabs casket Ge Mian tri- (must not there are scratches), shade is dry;
(m) it repeats, by the process of step (k) and step (l), being repeated several times can complete.
The wooden tire casket of gained colour raw lacquer is as shown in Fig. 2, as can be seen from Figure 2: though the wooden tire casket smooth in appearance, Production is fine, but human factor it is more be very much it is affected, the stiff stiff, color of decorative pattern is familiar with.
The adhesive force of colored raw lacquer and ornaments, test result are determined using adhesive force traditional test methods are as follows: ASTM etc. Grade 2B;It is observed by cross-hatching, there is part peeling or full wafer to peel off in notching edge, peeling off area is more than 15%, but less than 35%.
Comparative example and comparative example, it can be seen that when modifying ornaments using colored raw lacquer of the invention, required process Less, the time is short;Moreover, the method is simple and quick, there is no the requirement of technical aspect to staff.
The above is only a preferred embodiment of the present invention, it is noted that for the ordinary skill people of the art For member, various improvements and modifications may be made without departing from the principle of the present invention, these improvements and modifications are also answered It is considered as protection scope of the present invention.

Claims (8)

1. a kind of colour raw lacquer, including following components in percentage by weight: transparent lacquer 30~45%, solvent naphtha 40~55%, Mineral powder 10~20%.
2. colour raw lacquer according to claim 1, which is characterized in that the solvent naphtha includes tung oil, turpentine oil and camphor One of oil is a variety of.
3. colour raw lacquer according to claim 1, which is characterized in that the partial size of the mineral powder is 1000~1500 mesh.
4. colour raw lacquer according to claim 1 or 3, which is characterized in that the mineral powder includes cinnabar, realgar or green Pine.
5. the preparation method of any one of Claims 1 to 4 colored raw lacquer, comprising the following steps:
(1) it grinds, filter after mixing mineral powder with partial solvent oil, obtain color;
(2) it grinds, filter after mixing the color that the step (1) obtains with transparent lacquer, obtain colored paint;
(3) it is filtered after mixing the colored paint that the step (2) obtains with residual solvent oil, obtains colored raw lacquer.
6. preparation method according to claim 5, which is characterized in that the matter of color and transparent lacquer in the step (2) Amount is than being 1:1.
7. made from preparation method described in any one of Claims 1 to 4 colored raw lacquer or claim 5~6 any one Colored raw lacquer is in life appliance, building decoration, furniture furnishings, public art, electronic product, toy for children and field of vehicles In application.
8. a kind of craftwork, which is characterized in that including colored raw lacquer described in claim 1.
CN201810844973.1A 2018-07-27 2018-07-27 A kind of colour raw lacquer and the preparation method and application thereof, a kind of craftwork Pending CN109181541A (en)