CN108031829A - 热态钢包水口座砖修复模具和修复方法 - Google Patents

热态钢包水口座砖修复模具和修复方法 Download PDF

Info

Publication number
CN108031829A
CN108031829A CN201711328661.7A CN201711328661A CN108031829A CN 108031829 A CN108031829 A CN 108031829A CN 201711328661 A CN201711328661 A CN 201711328661A CN 108031829 A CN108031829 A CN 108031829A
Authority
CN
China
Prior art keywords
pocket block
hot
ladle
repairing mould
restorative procedure
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201711328661.7A
Other languages
English (en)
Inventor
赵刚
蒋强
高亮
章新军
付代雄
蒋发燕
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
GANGCHENG GROUP LIANGSHAN RUIHAI INDUSTRIAL Co Ltd
Original Assignee
GANGCHENG GROUP LIANGSHAN RUIHAI INDUSTRIAL Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by GANGCHENG GROUP LIANGSHAN RUIHAI INDUSTRIAL Co Ltd filed Critical GANGCHENG GROUP LIANGSHAN RUIHAI INDUSTRIAL Co Ltd
Priority to CN201711328661.7A priority Critical patent/CN108031829A/zh
Publication of CN108031829A publication Critical patent/CN108031829A/zh
Pending legal-status Critical Current

Abstract

本发明公开了一种热态钢包水口座砖修复模具和修复方法,特别是一种涉及炉外精炼设备钢包系统领域的热态钢包水口座砖修复模具和修复方法。本发明的热态钢包水口座砖修复模具,包括入口段、过渡段、中间段和出口段。本发明的热态钢包水口座砖修复方法,包括以下几个步骤:A、将修复模具垂直放入热态水口座砖流钢通道内;B、将热态钢包水口座砖修复模具垂直固定;C、加注浇注料填补隙。采用本申请的热态钢包水口座砖修复模具和修复方法可以有效消除因浇注料加注时修复模具移位,保证了水口座砖内流钢通道在同轴上,利于连铸时钢水从流钢通道内顺利流出。

Description

热态钢包水口座砖修复模具和修复方法
技术领域
本发明涉及一种热态钢包水口座砖修复模具和修复方法,特别是一种涉及炉外精炼设备钢包系统领域的热态钢包水口座砖修复模具和修复方法。
背景技术
在钢铁企业炼钢厂冶炼设备中,钢包是炉外精炼设备的重要组成部分,主要用于盛装钢水、在LF或RH精炼钢水,是转炉与连铸机之间的钢水唯一运输载体,水口座砖是钢水的流钢通道,但是水口座砖在长时间使用后会因为损坏而造成水口座砖孔扩大,水口座砖孔扩大会导致钢水在连铸机开浇引流,但是现有技术中还没有关于如何及时修复水口座砖,实现节能降耗,绿色生产,减少钢包维修频率的技术方案。
发明内容
本发明所说解决的技术问题是提供一种投资少,成本低,作业时间短,可以有效修复修复水口座砖,并延长水口座砖使用寿命的热态钢包水口座砖修复模具。
本发明为解决上述问题所采用的热态钢包水口座砖修复模具,包括入口段、过渡段、中间段和出口段,所述入口段的底部与过渡段的顶部相接,所述过渡段的底部与中间段的顶部相接,所述中间段的底部与出口段顶部相接的,所述入口段为顶部直径大于底部直径的锥台形,所述中间段为底部直径大于顶部直径的锥台形,所述过渡段和出口段均为圆筒形。
本发明所解决的技术另一个技术问题是提供一种投资少,成本低,作业时间短,可以有效修复修复水口座砖,并延长水口座砖使用寿命的热态钢包水口座砖修复方法。
本发明为解决上述问题所采用的热态钢包水口座砖修复方法,包括以下几个步骤:
A、将热态钢包水口座砖修复模具垂直放入热态水口座砖流钢通道内;
B、将热态钢包水口座砖修复模具垂直固定,使热态钢包水口座砖修复模具与热态钢包水口座砖之间留有间隙;
C、加注浇注料填补热态钢包水口座砖修复模具与热态钢包水口座砖之间的空隙。
进一步的是,在A步骤中利用钢绳将修复模具垂直放入热态水口座砖流钢通道内。
本发明的有益效果是:本申请可以有效消除因浇注料加注时修复模具移位,保证了水口座砖内流钢通道在同轴上,利于连铸时钢水从流钢通道内顺利流出。其优点是:投资少,制造材料只需钢管;制造简单,钢管切割而成;作业时间短,延长水口座砖的使用寿命。本申请钢包在热态修复水口座砖,实现节能降耗,绿色生产,热态钢包水口座砖修复能够提高水口座砖寿命,减少钢包维修频率。
附图说明
图1是本发明的结构示意图;
图中标记为:入口段1、过渡段2、中间段3、出口段4、水口座砖5。
具体实施方式
下面结合附图对本发明作进一步说明。
如图1所示的热态钢包水口座砖5修复模具,包括入口段1、过渡段2、中间段3和出口段4,所述入口段1的底部与过渡段2的顶部相接,所述过渡段2的底部与中间段3的顶部相接,所述中间段3的底部与出口段4顶部相接的,所述入口段1为顶部直径大于底部直径的锥台形,所述中间段3为底部直径大于顶部直径的锥台形,所述过渡段2和出口段4均为圆筒形。本申请的热态钢包水口座砖5修复模具由入口段1、过渡段2、中间段3和出口段4四个部分从上至下连接而成,与热态钢包水口座砖5的外形相匹配。将本模具垂直固定在热态钢包水口座砖5处,使其与热态钢包水口座砖5修复模具留有一定间隙,在浇注时的浇注料在本模具的约束下,形成与热态钢包水口座砖5外形一致的形状,从而实现对热态钢包水口座砖5的修补。
本申请的热态钢包水口座砖5修复方法,包括以下几个步骤:
A、将热态钢包水口座砖5修复模具垂直放入热态水口座砖5流钢通道内;
B、将热态钢包水口座砖5修复模具垂直固定,使热态钢包水口座砖5修复模具与热态钢包水口座砖5之间留有间隙;
C、加注浇注料填补热态钢包水口座砖5修复模具与热态钢包水口座砖5之间的空隙。
本发明所述的热态钢包水口座砖5修复是由水口座砖5、修复模具和浇注料三部分构成的。修复模具采用直径为140mm的钢管制作,制作长度600mm,将修复模具垂直放入热态水口座砖5流钢通道内,垂直固定,然后将搅拌好的浇注料加入,消除因浇注料加注时修复模具移位,保证了水口座砖5内流钢通道在同轴上,利于连铸时钢水从流钢通道内顺利流出。本发明的优点是:投资少,制造材料只需钢管;制造简单,钢管切割而成;作业时间短,延长水口座砖5的使用寿命。为了保证修复模具能够严格按照垂直方向放入水口座砖5流钢通道,本申请在A步骤中利用钢绳将修复模具垂直放入热态水口座砖5流钢通道内。本申请钢包在热态修复水口座砖5,实现节能降耗,绿色生产,热态钢包水口座砖5修复能够提高水口座砖5寿命,减少钢包维修频率。

Claims (3)

1.热态钢包水口座砖修复模具,其特征在于:包括入口段(1)、过渡段(2)、中间段(3)和出口段(4),所述入口段(1)的底部与过渡段(2)的顶部相接,所述过渡段(2)的底部与中间段(3)的顶部相接,所述中间段(3)的底部与出口段(4)顶部相接的,所述入口段(1)为顶部直径大于底部直径的锥台形,所述中间段(3)为底部直径大于顶部直径的锥台形,所述过渡段(2)和出口段(4)均为圆筒形。
2.热态钢包水口座砖修复方法,其特征在于:包括以下几个步骤:
A、将权利要1所述的热态钢包水口座砖修复模具垂直放入热态水口座砖(5)流钢通道内;
B、将热态钢包水口座砖(5)修复模具垂直固定,使热态钢包水口座砖(5)修复模具与热态钢包水口座砖(5)之间留有间隙;
C、加注浇注料填补热态钢包水口座砖修复模具与热态钢包水口座砖(5)之间的空隙。
3.如权利要求2所述的热态钢包水口座砖修复方法,其特征在于:在A步骤中利用钢绳将修复模具垂直放入热态水口座砖(5)流钢通道内。
CN201711328661.7A 2017-12-13 2017-12-13 热态钢包水口座砖修复模具和修复方法 Pending CN108031829A (zh)