CN107574620A - A kind of all-cotton yarn-dyed three-resistance coating printed fabric production method - Google Patents
A kind of all-cotton yarn-dyed three-resistance coating printed fabric production method Download PDFInfo
- Publication number
- CN107574620A CN107574620A CN201711002372.8A CN201711002372A CN107574620A CN 107574620 A CN107574620 A CN 107574620A CN 201711002372 A CN201711002372 A CN 201711002372A CN 107574620 A CN107574620 A CN 107574620A
- Authority
- CN
- China
- Prior art keywords
- dyed
- production method
- printed fabric
- resistance coating
- cotton yarn
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The present invention relates to a kind of production method of three proofings printed fabric, more particularly, to a kind of all-cotton yarn-dyed three-resistance coating printed fabric production method.Fabric in the presence of its three-resistance coating printed fabric production process mainly present in solution prior art is dry and astringent, and feel is harder, and the not high technical problem of oily grade is refused after repeatedly washing.The method of the present invention includes:Singe, desizing, mercerising, peracid sizing, stamp, wash, sizing, bake and preshrunk.The setting process of the present invention is 60 150 g/l of three proofings auxiliary agent, three proofings assistant types are C6 fluorocarbon resins, and 15 30 g/l of crosslinking agent, crosslinking agent type is block copolymerization isocyanates, 2 10 g/l of bleeding agent, bleeding agent type are alkylphosphonic and fat alcohol ethoxyl compound.
Description
Technical field
The present invention relates to a kind of production method of three proofings printed fabric, is printed more particularly, to a kind of all-cotton yarn-dyed three-resistance coating
Flower fabric plus material producing method.
Background technology
With social development, diversification is diversified requires more and more higher, traditional sense for the consumer goods and consumption by consumer
On common all cotton fibers textile can meet the needs of modern consumers in general.
The color-woven fabric medium-to-high grade as textile, is liked by consumers in general, especially as high finish
Stamp+three proofings functional treatment fabric;Using stamp+three proofings feature underlinen fabric of produced in conventional processes, generally existing face
Expect dry and astringent, feel is harder, the not high production technology problem of oily grade is refused after repeatedly washing, so as to have influence on such Yarn-dyed fabric
Exploitation and production.
The content of the invention
Present invention topic is to provide a kind of all-cotton yarn-dyed three-resistance coating printed fabric production method, and it mainly solves existing skill
The fabric in the presence of three-resistance coating printed fabric production process present in art is dry and astringent, and feel is harder, and oil etc. is refused after repeatedly washing
The not high technical problem of level.
The above-mentioned technical problem of the present invention is mainly what is be addressed by following technical proposals:
A kind of all-cotton yarn-dyed three-resistance coating printed fabric production method of the present invention, it is characterised in that described method includes:Burn
Hair, desizing, mercerising, peracid sizing, stamp, wash, sizing, bake and preshrunk.
Preferably, described singeing is 90-110 ms/min of speed, firepower 8-14 shelves, position is 1-3 shelves.
Preferably, described desizing uses ferment treatment, temperature is 65-85 degree, and speed is 40-80 ms/min.
Preferably, the base amount 14-24 Baumes of described mercerization, pH are set as 4.0-6.5.
Preferably, described peracid setting process is HAC 0.5-1.5 g/l, and 50-90 ms/min of speed, temperature 130-
160 degree.
Include being formulated preferably, described stamp is pigment printing, pigment printing, dry set and bake etc. and produce work
Sequence,
Preferably, described washing process is 30-70 ms/min of speed, temperature is 40-70 degree.
Preferably, described setting process is 60-150 g/l of three proofings auxiliary agent, three proofings assistant types are C6 fluorine carbon trees
Fat, 15-30 g/l of crosslinking agent, crosslinking agent type are block copolymerization isocyanates, 2-10 g/l of bleeding agent, and bleeding agent type is
Alkylphosphonic and fat alcohol ethoxyl compound.
Preferably, it is 150-170 degree that described baking, which is temperature, 25-45 ms/min of speed.
Therefore of the invention compared with existing conventional art, advantage is the three-resistance coating stamp for solving produced in conventional processes
Fabric present in fabric is dry and astringent, and feel is harder, and the shortcomings of oily grade is not high is refused after repeatedly washing so that the finished product fabric tool of production
Have and good refuse the wearability such as oil.
Embodiment
Below by embodiment, technical scheme is described in further detail.
Embodiment 1:A kind of all-cotton yarn-dyed three-resistance coating printed fabric production method of this example, its step are:Singe, move back
Slurry, mercerising, peracid sizing, stamp, wash, sizing, bake and preshrunk.
Twill dark color color-woven fabric, yarn count is used as CM32 through weft yarn, warp count is 140 pieces/inch, and weft count is
76 pieces/inch.Fabric, which is singed, uses speed as 90 ms/min, and firepower is 14 grades, and position of singing removes fabric face filoplumes for 3 grades,
Enzyme desizing treatment temperature is used as 85 degree, speed is 40 ms/min of slurries removed on fabrics, and mercerising base amount is 14 Baumes, PH
It is set as 6.5 carry out mercerisings, peracid sizing HAC is 1.5 g/l, 50 ms/min of speed, 130 degree of temperature, the water after the completion of stamp
Carwash speed is 30 ms/min, and temperature is 70 degree, is fixed to pad 150 g/l of three proofings auxiliary agent, 30 g/l of crosslinking agent, bleeding agent 10
G/l, baking temperature is 170 degree, and 25 ms/min of speed is baked, then carries out the production technology of preshrunk and produced, so as to must
To final finished product, fabric is soft, has the good oily effect and wearability of refusing, and related physical and chemical index meet
National Grade A related request.
Key index test data result is as follows:Refuse to refuse isopropanol 5.0, ultimate strength after oil is washed for 3.0,20 times after washing for 20 times
The lbs of warp-wise 111.2, the lbs of broadwise 55.1;Warp-wise tears 2.8 lbs, and broadwise tears 2.0 lbs.
Embodiment 2:A kind of all-cotton yarn-dyed three-resistance coating printed fabric production method of this example, its step are:Singe, move back
Slurry, mercerising, peracid sizing, stamp, wash, sizing, bake and preshrunk.
Color color-woven fabric in twill, yarn count is used as CM32 through weft yarn, warp count is 140 pieces/inch, and weft count is
76 pieces/inch.Fabric, which is singed, uses speed as 100 ms/min, and firepower is 10 grades, and 2 grades of removal fabric face hairs is in position of singing
Plumage, enzyme desizing treatment temperature is used as 75 degree, speed is 60 ms/min of slurries removed on fabric, and mercerising base amount is 22 Baumes,
PH is set as 5.0 carry out mercerisings, and peracid sizing HAC is 0.5 g/l, 70 ms/min of speed, 150 degree of temperature, after the completion of stamp
It is 40 ms/min to wash speed, and temperature is 60 degree, is fixed to pad 120 g/l of three proofings auxiliary agent, 15 g/l of crosslinking agent, bleeding agent 5
G/l, baking temperature is 170 degree, and 45 ms/min of speed is baked, then carries out the production technology of preshrunk and produced, so as to must
To final finished product, fabric is soft, has the good oily effect and wearability of refusing, and related physical and chemical index meet
National Grade A related request.
Key index test data result is as follows:Refuse to refuse isopropanol 5.5, ultimate strength after oil is washed for 4.5,20 times after washing for 20 times
The lbs of warp-wise 88.7, the lbs of broadwise 52.7;Warp-wise tears 3.0 lbs, and broadwise tears 2.5 lbs.
Embodiment 3:A kind of all-cotton yarn-dyed three-resistance coating printed fabric production method of this example, its step are:Singe, move back
Slurry, mercerising, peracid sizing, stamp, wash, sizing, bake and preshrunk.
Twill light color color-woven fabric, yarn count is used as CM32 through weft yarn, warp count is 140 pieces/inch, and weft count is
76 pieces/inch.Fabric, which is singed, uses speed as 110 ms/min, and firepower is 14 grades, and 1 grade of removal fabric face hair is in position of singing
Plumage, enzyme desizing treatment temperature is used as 65 degree, speed is 40 ms/min of slurries removed on fabric, and mercerising base amount is 24 Baumes,
PH is set as 4.0 carry out mercerisings, and peracid sizing HAC is 0.5 g/l, 90 ms/min of speed, 160 degree of temperature, after the completion of stamp
It is 50 ms/min to wash speed, and temperature is 70 degree, is fixed to pad 60 g/l of three proofings auxiliary agent, 30 g/l of crosslinking agent, bleeding agent 5
G/l, baking temperature is 150 degree, and 25 ms/min of speed is baked, then carries out the production technology of preshrunk and produced, so as to must
To final finished product, fabric is soft, has the good oily effect and wearability of refusing, and related physical and chemical index meet
National Grade A related request.
Key index test data result is as follows:Refuse to refuse isopropanol 5.0, ultimate strength after oil is washed for 4.0,20 times after washing for 20 times
The lbs of warp-wise 112.2, the lbs of broadwise 47.4;Warp-wise tears 3.6 lbs, and broadwise tears 2.9 lbs.
The specific embodiment of the present invention is the foregoing is only, but the architectural feature of the present invention is not limited thereto, Ren Heben
The technical staff in field in the field of the invention, all cover among the scope of the claims of the present invention by the change or modification made.
Claims (8)
1. a kind of all-cotton yarn-dyed three-resistance coating printed fabric production method, it is characterised in that described method includes:Singe, move back
Slurry, mercerising, peracid sizing, stamp, wash, sizing, bake and preshrunk.
2. a kind of all-cotton yarn-dyed three-resistance coating printed fabric production method according to claim 1, it is characterised in that described
Singeing be 90-110 ms/min of speed, firepower 8-14 shelves, position is 1-3 shelves.
3. a kind of all-cotton yarn-dyed three-resistance coating printed fabric production method according to claim 1, it is characterised in that described
Desizing use ferment treatment, temperature is 65-85 degree, and speed is 40-80 ms/min.
4. a kind of all-cotton yarn-dyed three-resistance coating printed fabric production method according to claim 1, it is characterised in that described
Mercerization base amount 14-24 Baumes, pH is set as 4.0-6.5.
5. a kind of all-cotton yarn-dyed three-resistance coating printed fabric production method according to claim 1, it is characterised in that described
Peracid setting process be HAC 0.5-1.5 g/l, 50-90 ms/min of speed, temperature 130-160 degree.
6. a kind of all-cotton yarn-dyed three-resistance coating printed fabric production method according to claim 1, it is characterised in that described
Stamp include formula for pigment printing, pigment printing, dry set and the production process such as bake,
A kind of all-cotton yarn-dyed three-resistance coating printed fabric production method according to claim 1, it is characterised in that described
Washing process is 30-70 ms/min of speed, and temperature is 40-70 degree.
7. a kind of all-cotton yarn-dyed three-resistance coating printed fabric production method according to claim 1, it is characterised in that described
Setting process be 60-150 g/l of three proofings auxiliary agent, three proofings assistant types are C6 fluorocarbon resins, 15-30 g/l of crosslinking agent, are handed over
It is block copolymerization isocyanates to join agent type, and 2-10 g/l of bleeding agent, bleeding agent type is alkylphosphonic and fatty alcohol ethoxy
Based compound.
8. a kind of all-cotton yarn-dyed three-resistance coating printed fabric production method according to claim 1, it is characterised in that described
Baking be that temperature is 150-170 degree, 25-45 ms/min of speed.