CN107475867A - High Zhi Haimian towels and preparation method thereof - Google Patents
High Zhi Haimian towels and preparation method thereof Download PDFInfo
- Publication number
- CN107475867A CN107475867A CN201710669632.0A CN201710669632A CN107475867A CN 107475867 A CN107475867 A CN 107475867A CN 201710669632 A CN201710669632 A CN 201710669632A CN 107475867 A CN107475867 A CN 107475867A
- Authority
- CN
- China
- Prior art keywords
- haimian
- water
- warp
- towels
- yarn
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention discloses high Zhi Haimian towels and preparation method thereof, belong to textile technology field, high Zhi Haimian towels include wool warp, body warp and weft yarn, the wool warp is the non-twist long wool cotton yarn of 60s/1 combing, the body warp is 40s/2 combed cotton yarns, the weft yarn is 40s/1 combed cotton yarns, and the non-twist long wool cotton yarn of combing is wrapped with water-soluble silk;Product it is highly flexible is it is fluffy, using comfortable, water absorption rate improves, and the more washes the more fluffy, and plucking rate is low, is not in depilation phenomenon after washing, and appearance after laundering is good.
Description
Technical field
The present invention relates to textile technology field, and in particular to high Zhi Haimian towels and preparation method thereof.
Background technology
Cotton maximum is characterized in fluffy softness, and sucting wet air permeability is strong, and usually used twist yarn is the fibre to cotton
What dimension was twisted and formed, still, during twisting spinning and being woven into cloth, the intrinsic characteristic of cotton has qualitative change, comfortably
Degree is affected.In contrast, Untwisted yarn is to make twist yarn untwisting, is formed with untwisted state, Untwisted yarn hair
Enclose soft and fluffy, many air are contained between fiber.Therefore, untwisted yarn towel soft feel, is surpassed with the bulkiness of uniqueness
Strong water absorbing properties obtain the favor of consumer.Compared with the general towel with twist yarn looped pile, there is Untwisted yarn hair
The sponge towel of circle has soft skin feel, and the feature that the volume sense than seeming is light, further, since between fiber
Gap absorbs moisture, thus with the high feature of water imbibition.
With the continuous improvement of living standard, requirement of the people for towel also more and more higher, the sea as expensive goods
Wool towel, however it remains following defect:Soft fluffy degree is inadequate, and feel is hardened;Filoplume is more, easily depilation, influences outward appearance after washing;Inhale
Water-based deficiency.
The content of the invention
For above-mentioned technical problem, the present invention provides high Zhi Haimian towels and preparation method thereof, product it is highly flexible is it is fluffy,
Using comfortable, water absorption rate improves, and the more washes the more fluffy, and plucking rate is low, is not in depilation phenomenon after washing, and appearance after laundering is good.
To achieve the above object, the present invention uses following technical scheme:
High Zhi Haimian towels, including wool warp, body warp and weft yarn, the wool warp are the non-twist long-staple cotton of 60s/1 combing
Yarn, the body warp are 40s/2 combed cotton yarns, and the weft yarn is 40s/1 combed cotton yarns, the non-twist long wool cotton yarn looping of combing
There is water-soluble silk.
Preferably, the twist of the non-twist long wool cotton yarn raw yarn of the combing is 90 sth. made by twisting/10cm, is twisted with the fingers after the water-soluble silk of looping and untwisting
Spend for 45 sth. made by twisting/10cm.
Preferably, the water-soluble silk is the water-soluble silks of 80s.
Preferably, the high Zhi Haimian towels through it is close be 68/5.08cm, filling density is 74.28/2.54cm.
Preferably, the hair of the high Zhi Haimian towels is 8.6-9.8 again.
Preferably, the terry height of the high Zhi Haimian towels is 0.4 ㎝.
The present invention also provides the production method of high Zhi Haimian towels, comprises the following steps:
(1) pre-treatment is weaved:Wool warp, body warp, weft material are chosen, the hair that the raw yarn twist is 90 sth. made by twisting/10cm is passed through
The water-soluble silk of yarn looping and untwisting, the twist is 45 sth. made by twisting/10cm;
(2) warping:Wool warp, body warp and weft yarn are distinguished into warping;
(3) starching:To wool warp, body warp starching simultaneously;
(4) weave:Wool warp, body warp, weft yarn are weaved by loom, from 68# reed;
(5) water-soluble silk stripping:In 90-105 DEG C of water temperature, bath raio 1:Washing 40-60min is carried out under conditions of 48, strips water
Molten silk;
(6) desizing is washed:In desizing agent 0.8-1.2g/L, temperature carries out desizing washing process 30min under the conditions of being 85 DEG C,
The impurity such as the wax in yarn, cotton seed hulls are eliminated so that product has good feel;
(7) bleaching and dyeing;
(8) supple-settlement is added:Carry out adding supple-settlement in hydrophilic softener solution;
(9) dry.
Preferably, the speed of loom is 450r/min during step (4) weaving.
Preferably, the concrete technology that the step (7) is bleachinged and dyeing is:Using high temperature-pressure dyeing machine, water absorbing agent high temperature is added
40min is handled, discharges liquid after slow cooling;Back into water, add oxygenic bleaching aids and bleached, in high temperature, pressure 3kpa
Under the conditions of handle 30min, be then depressurized to 0kpa, discharge liquid after slow cooling;Back into water, in high temperature, pressure 1kpa
Under the conditions of handle 20min, liquid is discharged after slow cooling;Back into water, room temperature treatment 15min, by liquid after slow cooling
Discharge, goes out machine;Normal temperature and pressure sprays overflow dyeing agent, adds removal of impurities auxiliary agent high-temperature process 30min, arranges liquid after slow cooling
Put.
The present invention advantageous effects be:Using special twisting mode so that product cotton fiber after each washing
Meeting self-return, so the more can wash the more fluffy;High-count yarn is used, so can feel very light when we are using towel, it is very soft;
The residual of yarn is twisted as 45 sth. made by twisting/10cm after the water-soluble silk of looping, and bigger than common product, filoplume will lack, in addition when bleachinging and dyeing processing at
The reason time is short, as far as possible few destruction cotton fiber, so product plucking rate very little, is 0.2%, reaches the standard of high-class product;With it is general
Logical towel is preferable compared to hygroscopicity, and diffusion time of dripping is less than 1s.
Embodiment
With reference to specific embodiment, the invention will be further described.
Embodiment 1
High Zhi Haimian towels, including wool warp, body warp and weft yarn, the wool warp are the non-twist long-staple cotton of 60s/1 combing
Yarn, the body warp are 40s/2 combed cotton yarns, and the weft yarn is 40s/1 combed cotton yarns, the non-twist long wool cotton yarn looping of combing
There is water-soluble silk.
The production method of the high Zhi Haimian towels, comprises the following steps:(1) pre-treatment is weaved:Raw material are handled,
Using the non-twist long wool cotton yarn of 60s/1 combing as wool warp, 40s/2 combed cotton yarns as body warp, 40s/1 combed cotton yarns as latitude
Yarn material, by the water-soluble silks of the wool warp looping 80s simultaneously untwisting that the raw yarn twist is 90 sth. made by twisting/10cm, the twist is 45 sth. made by twisting/10cm;(2) it is whole
Through:Wool warp, body warp and weft yarn are distinguished into warping;(3) starching:To wool warp, body warp starching simultaneously;(4) weave:By hair
Warp thread, body warp, weft yarn are weaved by loom, and from 68# reed, the speed of loom is 450r/min during weaving;(5) water-soluble silk
Stripping:In 90-105 DEG C of water temperature, bath raio 1:Washing 40min is carried out under conditions of 48, strips water-soluble silk;(6) desizing is washed:Moving back
Agent 0.8g/L is starched, temperature carries out desizing washing process 30min under the conditions of being 85 DEG C, eliminates wax in yarn, cotton seed hulls etc.
Impurity causes product to have good feel;(7) bleaching and dyeing:Using high temperature-pressure dyeing machine, water absorbing agent high-temperature process is added
40min, liquid is discharged after slow cooling;Back into water, add oxygenic bleaching aids and bleached, in high temperature, pressure 3kpa conditions
Lower processing 30min, 0kpa is then depressurized to, discharges liquid after slow cooling;Back into water, in high temperature, pressure 1kpa conditions
Lower processing 20min, liquid is discharged after slow cooling;Back into water, room temperature treatment 15min, liquid is discharged after slow cooling,
Go out machine;Normal temperature and pressure sprays overflow dyeing agent, adds removal of impurities auxiliary agent high-temperature process 30min, discharges liquid after slow cooling;(8)
Add supple-settlement:Carry out adding supple-settlement in hydrophilic softener solution;(9) dry.
The high Zhi Haimian towels of products obtained therefrom through it is close be 68/5.08cm, filling density is 74.28/2.54cm, and hair is again
8.9, terry height is 0.4 ㎝.
Contrast experiment:Selection square grammes per square metre is 251g/m2Common towel and this towel (respectively taking 9.63g), immerse respectively
Filling and observed in the beaker of 50g water, it is found that after this towel is immersed in beaker, the water almost all in beaker is absorbed, with
Common towel forms sharp contrast, illustrates that this towel is big compared with the water absorption of common towel, good water absorption.
Embodiment 2
High Zhi Haimian towels, including wool warp, body warp and weft yarn, the wool warp are the non-twist long-staple cotton of 60s/1 combing
Yarn, the body warp are 40s/2 combed cotton yarns, and the weft yarn is 40s/1 combed cotton yarns, the non-twist long wool cotton yarn looping of combing
There is water-soluble silk.
The production method of the high Zhi Haimian towels, comprises the following steps:(1) pre-treatment is weaved:Raw material are handled,
Using the non-twist long wool cotton yarn of 60s/1 combing as wool warp, 40s/2 combed cotton yarns as body warp, 40s/1 combed cotton yarns as latitude
Yarn material, by the water-soluble silks of the wool warp looping 80s simultaneously untwisting that the raw yarn twist is 90 sth. made by twisting/10cm, the twist is 45 sth. made by twisting/10cm;(2) it is whole
Through:Wool warp, body warp and weft yarn are distinguished into warping;(3) starching:To wool warp, body warp starching simultaneously;(4) weave:By hair
Warp thread, body warp, weft yarn are weaved by loom, and from 68# reed, the speed of loom is 450r/min during weaving;(5) water-soluble silk
Stripping:In 90-105 DEG C of water temperature, bath raio 1:Washing 60min is carried out under conditions of 48, strips water-soluble silk;(6) desizing is washed:Moving back
Agent 1.2g/L is starched, temperature carries out desizing washing process 30min under the conditions of being 85 DEG C, eliminates wax in yarn, cotton seed hulls etc.
Impurity causes product to have good feel;(7) bleaching and dyeing:Using high temperature-pressure dyeing machine, water absorbing agent high-temperature process is added
40min, liquid is discharged after slow cooling;Back into water, add oxygenic bleaching aids and bleached, in high temperature, pressure 3kpa conditions
Lower processing 30min, 0kpa is then depressurized to, discharges liquid after slow cooling;Back into water, in high temperature, pressure 1kpa conditions
Lower processing 20min, liquid is discharged after slow cooling;Back into water, room temperature treatment 15min, liquid is discharged after slow cooling,
Go out machine;Normal temperature and pressure sprays overflow dyeing agent, adds removal of impurities auxiliary agent high-temperature process 30min, discharges liquid after slow cooling;(8)
Add supple-settlement:Carry out adding supple-settlement in hydrophilic softener solution;(9) dry.
The high Zhi Haimian towels of products obtained therefrom through it is close be 68/5.08cm, filling density is 74.28/2.54cm, and hair is again
8.8, terry height is 0.4 ㎝.
The foregoing is merely illustrative of the preferred embodiments of the present invention, is not intended to limit the invention, all skills in the present invention
On the basis of art scheme, those skilled in the art need not pay the various modifications that creative work can make or deformation still exists
In protection scope of the present invention.
Claims (9)
1. high Zhi Haimian towels, it is characterised in that including wool warp, body warp and weft yarn, the wool warp be 60s/1 combing without
Length of lay suede cotton yarn, the body warp are 40s/2 combed cotton yarns, and the weft yarn is 40s/1 combed cotton yarns, the non-twist long wool of combing
Cotton yarn is wrapped with water-soluble silk.
2. high Zhi Haimian towels according to claim 1, it is characterised in that the sth. made by twisting of the non-twist long wool cotton yarn raw yarn of combing
Spend for 90 sth. made by twisting/10cm, the twist is 45 sth. made by twisting/10cm after the water-soluble silk of looping and untwisting.
3. high Zhi Haimian towels according to claim 1, it is characterised in that the water-soluble silk is the water-soluble silks of 80s.
4. high Zhi Haimian towels according to claim 1, it is characterised in that the high Zhi Haimian towels through it is close be 68
Root/5.08cm, filling density are 74.28/2.54cm.
5. high Zhi Haimian towels according to claim 1, it is characterised in that the hair of the high Zhi Haimian towels is 8.6- again
9.8。
6. high Zhi Haimian towels according to claim 1, it is characterised in that the terry height of the high Zhi Haimian towels is
0.4㎝。
7. the production method of high Zhi Haimian towels according to claim 1, it is characterised in that comprise the following steps:
(1) pre-treatment is weaved:Wool warp, body warp, weft material are chosen, by the wool warp bag that the raw yarn twist is 90 sth. made by twisting/10cm
Water-soluble silk and untwisting are twined, the twist is 45 sth. made by twisting/10cm;
(2) warping:Wool warp, body warp and weft yarn are distinguished into warping;
(3) starching:To wool warp, body warp starching simultaneously;
(4) weave:Wool warp, body warp, weft yarn are weaved by loom;
(5) water-soluble silk stripping:In 90-105 DEG C of water temperature, bath raio 1:Washing 40-60min is carried out under conditions of 48, strips water-soluble silk;
(6) desizing is washed:In desizing agent 0.8-1.2g/L, temperature carries out desizing washing process 30min under the conditions of being 85 DEG C, removes
The impurity such as wax, cotton seed hulls in yarn cause the product to have good feel;
(7) bleaching and dyeing;
(8) supple-settlement is added:Carry out adding supple-settlement in hydrophilic softener solution;
(9) dry.
8. the production method of high Zhi Haimian towels according to claim 7, it is characterised in that during step (4) weaving
The speed of loom is 450r/min.
9. the production method of high Zhi Haimian towels according to claim 7, it is characterised in that what the step (7) was bleachinged and dyeing
Concrete technology is:Using high temperature-pressure dyeing machine, water absorbing agent high-temperature process 40min is added, discharges liquid after slow cooling;Weight
Newly enter water, add oxygenic bleaching aids and bleached, handle 30min under the conditions of high temperature, pressure 3kpa, be then depressurized to 0kpa, delay
Liquid is discharged after slow cooling;Back into water, 20min is handled under the conditions of high temperature, pressure 1kpa, arranges liquid after slow cooling
Put;Back into water, room temperature treatment 15min, liquid is discharged after slow cooling, go out machine;Normal temperature and pressure sprays overflow dyeing agent, adds
Clean auxiliary agent high-temperature process 30min, discharges liquid after slow cooling.