CN106883687A - The benefit gold repair materials and method repaired for ancient times painted clay sculpture layer gold - Google Patents
The benefit gold repair materials and method repaired for ancient times painted clay sculpture layer gold Download PDFInfo
- Publication number
- CN106883687A CN106883687A CN201710180478.0A CN201710180478A CN106883687A CN 106883687 A CN106883687 A CN 106883687A CN 201710180478 A CN201710180478 A CN 201710180478A CN 106883687 A CN106883687 A CN 106883687A
- Authority
- CN
- China
- Prior art keywords
- gold
- parts
- repair materials
- benefit
- ancient times
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
Benefit gold repair materials the present invention relates to be used for the reparation of ancient times painted clay sculpture layer gold, in terms of mass fraction, the gold repair materials of mending are made up of the raw material of following quality proportionings:100 parts of zapon, 28 34 parts of boiled wood oil, 14 parts of Zhu.The invention further relates to the benefit gold restorative procedure repaired for ancient times painted clay sculpture layer gold.It is of the invention to mend golden repair materials and formed by the zapon that necessarily matches, boiled wood oil, cinnabar hybrid modulation, compared to the lacquer of traditional reparation, have the advantages that to have no irritating odor, to mend golden effect good, especially its bonding force intensity is suitable, it is easy to prepare, constructing operation flexibility is high, and will not bring injury to its secondary layer gold reparation after reparation.
Description
Technical field
The present invention relates to for painted clay sculpture layer gold recovery technique field, be specifically related to be repaiied for ancient times painted clay sculpture layer gold
Multiple benefit gold repair materials, have further related to the benefit gold restorative procedure repaired for ancient times painted clay sculpture layer gold.
Background technology
Technique of gilding is one of technology category of Chinese tradition, is made in substantial amounts of painted clay sculpture, palace mural painting, colored drawing stone inscription
Many historical relic classifications such as picture, ancient building oil colored paintings (based on northern area), historic building fire prevention (based on southern area)
In have application.The technique has a wide range of application, throughout domestic the South and the North each province, but because making material and technique and environment etc.
The composite factor influence of aspect, often produce cracking, rise first, warp, come off, local discoloration, gold size lacquering be on surface etc.
Damage Types.Can solve to gild all kinds of diseases of layer well currently without highly effective material and technology;Again due to various
The influence of factor, a large amount of historical relics occur layer gold obscission because of not protected timely.In order that historical relic is returned to
Initial complexion, it is to avoid the layer gold disease of historical relic is aggravated, becomes very necessary to carrying out mending gold and repairing at the disease of these historical relics.
The benefit gold to ancient times painted clay sculpture layer gold repairs used repair materials mainly lacquer at present, although the material
The reparation to layer gold can be completed, but lacquer can give out a large amount of noxious odors in use, and personnel are repaired to layer gold
Jiankang it is unfavorable;The technics comparing that other lacquer prepares gold size paint is complicated, prepares inconvenience.
The content of the invention
The technical problems to be solved by the invention are to provide a kind of good color for ancient times of easy to operate, nontoxic, repairing effect
The benefit gold repair materials of clay sculpture layer gold reparation are painted, is additionally provided and is used the benefit gold restorative procedure of benefit gold repair materials.
In order to solve the above technical problems, the present invention provides following technical scheme:Repaired for ancient times painted clay sculpture layer gold
Golden repair materials are mended, in terms of mass fraction, the gold repair materials of mending are made up of following quality proportioning raw materials:
100 parts of zapon
Boiled wood oil 28-34 parts
Cinnabar 1-4 parts.
On the basis of such scheme, in terms of mass fraction, the raw material group for mending golden repair materials by following quality proportionings
Into:
100 parts of zapon
34 parts of boiled wood oil
4 parts of cinnabar.
On the basis of such scheme, in terms of mass fraction, the raw material group for mending golden repair materials by following quality proportionings
Into:
100 parts of zapon
32 parts of boiled wood oil
3 parts of cinnabar.
On the basis of such scheme, in terms of mass fraction, the raw material group for mending golden repair materials by following quality proportionings
Into:
100 parts of zapon
30 parts of boiled wood oil
2 parts of cinnabar.
On the basis of such scheme, in terms of mass fraction, the raw material group for mending golden repair materials by following quality proportionings
Into:
100 parts of zapon
28 parts of boiled wood oil
1 part of cinnabar.
For the benefit gold restorative procedure that ancient times painted clay sculpture layer gold is repaired, including following technical step:
(1) take in 28-34 parts of the zapon of 100 parts of boiled wood oil addition, then add 1-4 parts of cinnabar, stir
To uniform color, deployed benefit gold repair materials gold size paint is obtained;
(2) the former aging gold size paint at place to be repaired in clay sculpture layer gold is disposed with cleaning agent;After removing totally, fur is used
Brush or paintbrush dip step (1) obtained in gold size paint, it is equably applied to place to be repaired;
(3) one block of cotton paper of humidity is taken, goldleaf is attached on cotton paper, then pinched cotton paper and goldleaf is affixed on place to be repaired
The gold size that painting is wiped is painted;After the completion for the treatment of that goldleaf is pasted, cotton paper is dabbed with hair brush, finally gently sweep paint with soft wool brush, will
Unnecessary goldleaf is swept down.
The present invention has an advantageous effect in that compared with prior art:It is of the invention to mend golden repair materials by necessarily matching
Zapon, boiled wood oil, cinnabar hybrid modulation are formed, compared to the lacquer of traditional reparation, with the gold effect that has no irritating odor, mends
Really good the advantages of, especially its bonding force intensity is suitable, is easy to prepare, and constructing operation flexibility is high, and after repairing pair secondly
Secondary layer gold reparation will not bring injury.
Specific embodiment
In order to make the purpose , technical scheme and advantage of the present invention be clearer, with reference to embodiments, to the present invention
It is further elaborated.It should be appreciated that the specific embodiments described herein are merely illustrative of the present invention, it is not used to
Limit the present invention.
Embodiment one:
It is described to mend golden repair materials in terms of mass fraction for the benefit gold repair materials that ancient times painted clay sculpture layer gold is repaired
It is made up of the raw material of following quality proportionings:
100 parts of zapon
34 parts of boiled wood oil
4 parts of cinnabar.
Preparation method:Take in 34 parts of the zapon of 100 parts of boiled wood oil addition, then add 4 parts of cinnabar, stir
To uniform color, deployed benefit gold repair materials gold size paint is obtained.
Embodiment two:
It is described to mend golden repair materials in terms of mass fraction for the benefit gold repair materials that ancient times painted clay sculpture layer gold is repaired
It is made up of the raw material of following quality proportionings:
100 parts of zapon
32 parts of boiled wood oil
3 parts of cinnabar.
Preparation method:Take in 32 parts of the zapon of 100 parts of boiled wood oil addition, then add 3 parts of cinnabar, stir
To uniform color, deployed benefit gold repair materials gold size paint is obtained.
Embodiment three:
It is described to mend golden repair materials in terms of mass fraction for the benefit gold repair materials that ancient times painted clay sculpture layer gold is repaired
It is made up of the raw material of following quality proportionings:
100 parts of zapon
30 parts of boiled wood oil
2 parts of cinnabar.
Preparation method:Take in 30 parts of the zapon of 100 parts of boiled wood oil addition, then add 2 parts of cinnabar, stir
To uniform color, deployed benefit gold repair materials gold size paint is obtained.
Example IV:
It is described to mend golden repair materials in terms of mass fraction for the benefit gold repair materials that ancient times painted clay sculpture layer gold is repaired
It is made up of the raw material of following quality proportionings:
100 parts of zapon
28 parts of boiled wood oil
1 part of cinnabar.
Preparation method:Take in 28 parts of the zapon of 100 parts of boiled wood oil addition, then add 1 part of cinnabar, stir
To uniform color, deployed benefit gold repair materials gold size paint is obtained.
Component proportion according to aforementioned four embodiment can be obtained four kinds of benefit gold repair materials gold sizes of different viscosityes
Paint, and the bond properties of four kinds of gold size paints is almost identical;According to all kinds of of layer gold inner skeleton, carcass and painted layer appearance
The destructiveness of disease and prepare, use the gold size paint of different viscosityes;Rule be with the increase of disease destructiveness,
The gold size paint viscosity of selection is ascending.
For the benefit gold restorative procedure that ancient times painted clay sculpture layer gold is repaired, including following technical step:(1) benefit gold is taken to repair
Material gold size paint is standby;(2) the former aging gold size paint at place to be repaired in clay sculpture layer gold is disposed with cleaning agent;Remove clean
Afterwards, the gold size paint of step (1) is dipped with banister brush or paintbrush, it is equably applied to place to be repaired;(3) one piece of humidity is taken
Cotton paper, goldleaf is attached on cotton paper, is then pinched cotton paper and goldleaf is affixed on place to be repaired is applied the gold size that wipes and paints;Treat goldleaf
After the completion of stickup (i.e. after 1min), cotton paper is dabbed with hair brush, finally gently sweep paint with soft wool brush, unnecessary goldleaf is swept down
.
Gold repair materials of mending of the invention are formed by zapon, boiled wood oil, cinnabar hybrid modulation, are repaired compared to tradition and used
Lacquer, have the advantages that to have no irritating odor, mend that golden effect is good, especially its bonding force intensity is suitable, is easy to prepare, construction
Operating flexibility is high, and will not bring injury to its secondary layer gold reparation after reparation.
Claims (6)
1. the benefit gold repair materials that ancient times painted clay sculpture layer gold is repaired are used for, it is characterised in that described to mend gold in terms of mass fraction
Repair materials are made up of the raw material of following quality proportionings:
100 parts of zapon
Boiled wood oil 28-34 parts
Cinnabar 1-4 parts.
2. it is according to claim 1 for ancient times painted clay sculpture layer gold repair benefit gold repair materials, it is characterised in that with
Mass fraction meter, the benefit gold repair materials are made up of the raw material of following quality proportionings:
100 parts of zapon
34 parts of boiled wood oil
4 parts of cinnabar.
3. it is according to claim 1 for ancient times painted clay sculpture layer gold repair benefit gold repair materials, it is characterised in that with
Mass fraction meter, the benefit gold repair materials are made up of the raw material of following quality proportionings:
100 parts of zapon
32 parts of boiled wood oil
3 parts of cinnabar.
4. it is according to claim 1 for ancient times painted clay sculpture layer gold repair benefit gold repair materials, it is characterised in that with
Mass fraction meter, the benefit gold repair materials are made up of the raw material of following quality proportionings:
100 parts of zapon
30 parts of boiled wood oil
2 parts of cinnabar.
5. it is according to claim 1 for ancient times painted clay sculpture layer gold repair benefit gold repair materials, it is characterised in that with
Mass fraction meter, the benefit gold repair materials are made up of the raw material of following quality proportionings:
100 parts of zapon
28 parts of boiled wood oil
1 part of cinnabar.
6. the benefit gold restorative procedure that ancient times painted clay sculpture layer gold is repaired is used for, it is characterised in that including following technical step:
(1) take in 28-34 parts of the zapon of 100 parts of boiled wood oil addition, then add 1-4 parts of cinnabar, stirring to color
It is damp uniform, obtain deployed benefit gold repair materials gold size paint;
(2) the former aging gold size paint at place to be repaired in clay sculpture layer gold is disposed with cleaning agent;Remove it is clean after, with banister brush or
Paintbrush dip step (1) obtained in gold size paint, it is equably applied to place to be repaired;
(3) one block of cotton paper of humidity is taken, goldleaf is attached on cotton paper, then pinched cotton paper and goldleaf is affixed on place's smearing to be repaired
Good gold size is painted;After the completion for the treatment of that goldleaf is pasted, cotton paper is dabbed with hair brush, finally gently sweep paint with soft wool brush, will be unnecessary
Goldleaf sweep down.