CN106867349A - A kind of aqueous colorful paint preparation method - Google Patents
A kind of aqueous colorful paint preparation method Download PDFInfo
- Publication number
- CN106867349A CN106867349A CN201710099272.5A CN201710099272A CN106867349A CN 106867349 A CN106867349 A CN 106867349A CN 201710099272 A CN201710099272 A CN 201710099272A CN 106867349 A CN106867349 A CN 106867349A
- Authority
- CN
- China
- Prior art keywords
- added
- protection glue
- paint
- prepare
- base paint
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The present invention relates to a kind of aqueous colorful paint preparation method, its step is as follows:(1)Prepare protection glue;(2)Prepare base paint:During preparation, the Protection glue liquid that will be prepared is slowly added into other mixed materials, is granulated again after carrying out after base paint after 24 hours;During granulation, 400 parts of the base paint that will mix up color is added to during 300 parts of concentration are 6% protection glue, is granulated with screen granulator or dispersion impeller after standing 35 minutes;(3)Prepare continuous items;(4)By step(2)Ready-made particle is added in continuous items, and particle presses 1 with slurry:1 mass ratio is added, and is slowly stirred and is uniformly made finished product.The of the invention prepared aqueous colorful paint preparation method for obtaining is simple, prepares that multi-color using effect is good, and bright in luster with preferable biocidal efficacies, performance is good, easy to use.
Description
Technical field
The present invention relates to a kind of aqueous colorful paint preparation method, belong to paint preparing technical field.
Background technology
Paint is that one kind can firmly be covered in body surface, and the chemistry for playing protection, decoration, mark and other specific uses is mixed
Compound coating.Chinese coating circle is more authoritative《Coating process》What one book was defined as:" coating is a kind of material, this
Material can be coated in object surface with different construction technologies, form adhesion firm, thin with some strength, continuous solid-state
Film.The film common name film for so being formed, also known as paint film or coating." coating is typically by film forming matter, filler(Color stuffing), solvent,
The part of auxiliary agent etc. four constitutes.According to performance requirement, composition can be slightly changed sometimes, and such as varnish can in not having color stuffing, powdery paints
With no solvent.Belong to organic chemical industry's macromolecular material, the film for being formed belongs to macromolecular compound type.It is logical according to the modern times
The classification of capable chemical products, coating belongs to fine chemical product.Modern coating progressively turns into class multifunctionality
Engineering material, is an important industry in chemical industry.
The content of the invention
It is an object of the invention to provide a kind of aqueous colorful paint preparation method, effect is prepared preferably to improve paint
Really, there is provided a kind of aqueous colorful paint with more preferable performance, and prepare it is simple, it is easy to use.
To achieve these goals, technical scheme is as follows.
A kind of aqueous colorful paint preparation method, its step is as follows:
(1)Prepare protection glue:Protection glue is added in running water, acquisition protection glue is mixed with, wherein, originally water quality
Amount number accounts for 94%, and Protection glue mass fraction accounts for 6%;
(2)Prepare base paint:Acquisition base paint is mixed with according to following mass fraction material:Running water 59.22%, dispersant
0.22%th, wetting agent 0.56%, defoamer 0.22%, rutile titanium white powder 1.12%, kaolin 11.17%, hydroxyethyl cellulose
1.45%th, 2-amino-2-methyl-1-propanol 0.28%, bactericide 0.28%, ethylene glycol 0.89%, Lauryl Alcohol ester 1.12%, silicon third
Emulsion 12.2%, protection glue 11.17%, during preparation, the Protection glue liquid that will be prepared is slowly added into other mixed materials, is done
After good base paint after 24 hours after granulate again;During granulation, 400 parts of the base paint that will mix up color is added to the guarantor that 300 parts of concentration is 6%
In shield glue, granulated with screen granulator or dispersion impeller after standing 3-5 minutes;
(3)Prepare continuous items:Material according to following mass fraction is mixed with acquisition continuous items:Running water 34.54%, true stone
Paint emulsion 59.21%, defoamer 0.33%, ethylene glycol 1.97%, Lauryl Alcohol ester 2.63%, preservative 0.66%, thickener 0.66%;
(4)By step(2)Ready-made particle is added in continuous items, and particle presses 1 with slurry:1 mass ratio is added, and is slowly stirred
Mix and be uniformly made finished product.
The beneficial effect of the invention is:The prepared aqueous colorful paint preparation method for obtaining of the invention is simple, and preparation is obtained
Multi-color using effect it is good, bright in luster with preferable biocidal efficacies, performance is good, easy to use.
Specific embodiment
Specific embodiment of the invention is described with reference to embodiment, to be better understood from the present invention.
Embodiment
Aqueous colorful paint preparation method in the present embodiment, its step is as follows:
(1)Prepare protection glue:Protection glue is added in running water, acquisition protection glue is mixed with, wherein, originally water quality
Amount number accounts for 94%, and Protection glue mass fraction accounts for 6%;
(2)Prepare base paint:Acquisition base paint is mixed with according to following mass fraction material:Running water 59.22%, dispersant
0.22%th, wetting agent 0.56%, defoamer 0.22%, rutile titanium white powder 1.12%, kaolin 11.17%, hydroxyethyl cellulose
1.45%th, 2-amino-2-methyl-1-propanol 0.28%, bactericide 0.28%, ethylene glycol 0.89%, Lauryl Alcohol ester 1.12%, silicon third
Emulsion 12.2%, protection glue 11.17%, during preparation, the Protection glue liquid that will be prepared is slowly added into other mixed materials, is done
After good base paint after 24 hours after granulate again;During granulation, 400 parts of the base paint that will mix up color is added to the guarantor that 300 parts of concentration is 6%
In shield glue, granulated with screen granulator or dispersion impeller after standing 3-5 minutes;
(3)Prepare continuous items:Material according to following mass fraction is mixed with acquisition continuous items:Running water 34.54%, true stone
Paint emulsion 59.21%, defoamer 0.33%, ethylene glycol 1.97%, Lauryl Alcohol ester 2.63%, preservative 0.66%, thickener 0.66%;
(4)By step(2)Ready-made particle is added in continuous items, and particle presses 1 with slurry:1 mass ratio is added, and is slowly stirred
Mix and be uniformly made finished product.
The of the invention prepared aqueous colorful paint preparation method for obtaining is simple, and it is good to prepare multi-color using effect, tool
There are preferable biocidal efficacies, bright in luster, performance is good, easy to use.
The above is the preferred embodiment of the present invention, it is noted that for those skilled in the art
For, under the premise without departing from the principles of the invention, some improvements and modifications can also be made, these improvements and modifications are also considered as
Protection scope of the present invention.
Claims (1)
1. a kind of aqueous colorful paint preparation method, it is characterised in that:Its step is as follows:
(1)Prepare protection glue:Protection glue is added in running water, acquisition protection glue is mixed with, wherein, originally water quality
Amount number accounts for 94%, and Protection glue mass fraction accounts for 6%;
(2)Prepare base paint:Acquisition base paint is mixed with according to following mass fraction material:Running water 59.22%, dispersant
0.22%th, wetting agent 0.56%, defoamer 0.22%, rutile titanium white powder 1.12%, kaolin 11.17%, hydroxyethyl cellulose
1.45%th, 2-amino-2-methyl-1-propanol 0.28%, bactericide 0.28%, ethylene glycol 0.89%, Lauryl Alcohol ester 1.12%, silicon third
Emulsion 12.2%, protection glue 11.17%, during preparation, the Protection glue liquid that will be prepared is slowly added into other mixed materials, is done
After good base paint after 24 hours after granulate again;During granulation, 400 parts of the base paint that will mix up color is added to the guarantor that 300 parts of concentration is 6%
In shield glue, granulated with screen granulator or dispersion impeller after standing 3-5 minutes;
(3)Prepare continuous items:Material according to following mass fraction is mixed with acquisition continuous items:Running water 34.54%, true stone
Paint emulsion 59.21%, defoamer 0.33%, ethylene glycol 1.97%, Lauryl Alcohol ester 2.63%, preservative 0.66%, thickener 0.66%;
(4)By step(2)Ready-made particle is added in continuous items, and particle presses 1 with slurry:1 mass ratio is added, and is slowly stirred
Mix and be uniformly made finished product.