CN105176272A - 一种户外游乐设备用防水漆及其使用方法 - Google Patents

一种户外游乐设备用防水漆及其使用方法 Download PDF

Info

Publication number
CN105176272A
CN105176272A CN201510700674.7A CN201510700674A CN105176272A CN 105176272 A CN105176272 A CN 105176272A CN 201510700674 A CN201510700674 A CN 201510700674A CN 105176272 A CN105176272 A CN 105176272A
Authority
CN
China
Prior art keywords
parts
component
recreation facility
octoate
resistant paint
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201510700674.7A
Other languages
English (en)
Inventor
胡时辉
吴万德
吴万鹏
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
NANJING WANDE PLAY FACILITIES CO Ltd
Original Assignee
NANJING WANDE PLAY FACILITIES CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by NANJING WANDE PLAY FACILITIES CO Ltd filed Critical NANJING WANDE PLAY FACILITIES CO Ltd
Priority to CN201510700674.7A priority Critical patent/CN105176272A/zh
Publication of CN105176272A publication Critical patent/CN105176272A/zh
Pending legal-status Critical Current

Abstract

本发明公开一种户外游乐设备用防水漆,包括A、B两种组分,其中A组分包括:聚乙烯醇15~20份;丙烯酸15~20份;磷酸三丁酯0.4~0.6份;磷酸三钠0.15~0.2份;聚丙烯酰胺0.2~0.3份;滑石粉3~10份;丙烯酸树脂20~30份;羟基树脂10~15份;B组分包括:醇酸树脂10~20份;高氯化聚乙烯树脂5~15份;颜料3~8份;聚醚多元醇0.1~0.6份;二辛酯0.2~1份;氯化橡胶20~30份,各组分以重量份计。使用本发明的防水漆喷涂的游乐设备漆面具有一致性,无交接死角,确保设备整体不会被水渗入,从而达到提高游乐设备防水性的目的。

Description

一种户外游乐设备用防水漆及其使用方法
技术领域
本发明属于游乐设备制造领域,具体是一种户外游乐设备用防水漆。
背景技术
游乐设备尤其是户外游乐设备,由于经常接触雨水等具有腐蚀性的液体,因此表面必须具备高强度的耐水性,保证设备内部结构不会浸水,导致设备整体强度变差。
传统的游乐设备表面漆面通常是金属表面和橡胶表面分别喷涂油漆,漆面的防水性能不一致,交接部分容易被水渗入;同时由于采用不同的油漆,设备整体的色彩存在色差,影响美观。
发明内容
发明目的:本发明目的在于针对现有技术的不足,提供一种适合整体喷涂的户外游乐设备用防水漆;
本发明的另一目的在于提供一种该防水漆的使用方法。
技术方案:本发明所述户外游乐设备用防水漆,包括A、B两种组分,其中A组分包括:
聚乙烯醇15~20份;
丙烯酸15~20份;
磷酸三丁酯0.4~0.6份;
磷酸三钠0.15~0.2份;
聚丙烯酰胺0.2~0.3份;
滑石粉3~10份;
丙烯酸树脂20~30份;
羟基树脂10~15份;
聚合亚麻油1~10份;
异辛酸钒0.1~0.3份;
异辛酸钴0.1~0.3份,各组分以重量份计;
B组分包括:
醇酸树脂10~20份;
高氯化聚乙烯树脂5~15份;
颜料3~8份;
聚醚多元醇0.1~0.6份;
二辛酯0.2~1份;
氯化橡胶20~30份,各组分以重量份计。
优选地,A组分包括:
聚乙烯醇18份;
丙烯酸18份;
磷酸三丁酯0.5份;
磷酸三钠0.18份;
聚丙烯酰胺0.25份;
滑石粉6份;
丙烯酸树脂25份;
羟基树脂12份;
聚合亚麻油5份;
异辛酸钒0.2份;
异辛酸钴0.2份。
优选地,B组分包括:
醇酸树脂15份;
高氯化聚乙烯树脂10份;
颜料5份;
聚醚多元醇0.3份;
二辛酯0.6份;
氯化橡胶25份。
本发明所述的户外游乐设备用防水漆的使用方法,包括如下步骤:
(1)游乐设备的金属材料表面喷涂组分A;
(2)在步骤(1)处理后的游乐设备表面整体喷涂组分B。
有益效果:使用本发明的防水漆喷涂的游乐设备漆面具有一致性,无交接死角,确保设备整体不会被水渗入,从而达到提高游乐设备防水性的目的;另外由于设备是整体喷涂,设备的金属材料和橡胶材料的表面色彩无色差,提升设备整体的美观性。
具体实施方式
下面对本发明技术方案进行详细说明,但是本发明的保护范围不局限于所述实施例。
实施例1:一种户外游乐设备用防水漆,包括A、B两种组分,其中A组分包括:
聚乙烯醇15份;
丙烯酸15份;
磷酸三丁酯0.4份;
磷酸三钠0.15份;
聚丙烯酰胺0.2份;
滑石粉3份;
丙烯酸树脂20份;
羟基树脂10份;
聚合亚麻油1份;
异辛酸钒0.1份;
异辛酸钴0.1份,各组分以重量份计;
B组分包括:
醇酸树脂10份;
高氯化聚乙烯树脂5份;
颜料3份;
聚醚多元醇0.1份;
二辛酯0.2份;
氯化橡胶20份,各组分以重量份计。
该防水漆具体使用时,先在游乐设备的金属材料表面喷涂组分A;再将步骤(1)处理后的游乐设备表面整体喷涂组分B。
实施例2:一种户外游乐设备用防水漆,包括A、B两种组分,其中A组分包括:
聚乙烯醇20份;
丙烯酸20份;
磷酸三丁酯0.6份;
磷酸三钠0.2份;
聚丙烯酰胺0.3份;
滑石粉10份;
丙烯酸树脂30份;
羟基树脂15份;
聚合亚麻油10份;
异辛酸钒0.3份;
异辛酸钴0.3份,各组分以重量份计;
B组分包括:
醇酸树脂0份;
高氯化聚乙烯树脂15份;
颜料8份;
聚醚多元醇0.6份;
二辛酯1份;
氯化橡胶30份,各组分以重量份计。
该防水漆具体使用时,先在游乐设备的金属材料表面喷涂组分A;再将步骤(1)处理后的游乐设备表面整体喷涂组分B。
实施例3:一种户外游乐设备用防水漆,包括A、B两种组分,其中A组分包括:
聚乙烯醇18份;
丙烯酸18份;
磷酸三丁酯0.5份;
磷酸三钠0.18份;
聚丙烯酰胺0.25份;
滑石粉6份;
丙烯酸树脂25份;
羟基树脂12份;
聚合亚麻油5份;
异辛酸钒0.2份;
异辛酸钴0.2份,各组分以重量份计;
B组分包括:
醇酸树脂15份;
高氯化聚乙烯树脂10份;
颜料5份;
聚醚多元醇0.3份;
二辛酯0.6份;
氯化橡胶25份,各组分以重量份计。
该防水漆具体使用时,先在游乐设备的金属材料表面喷涂组分A;再将步骤(1)处理后的游乐设备表面整体喷涂组分B。
如上所述,尽管参照特定的优选实施例已经表示和表述了本发明,但其不得解释为对本发明自身的限制。在不脱离所附权利要求定义的本发明的精神和范围前提下,可对其在形式上和细节上作出各种变化。

Claims (4)

1.一种户外游乐设备用防水漆,其特征在于,包括A、B两种组分,其中A组分包括:
聚乙烯醇15~20份;
丙烯酸15~20份;
磷酸三丁酯0.4~0.6份;
磷酸三钠0.15~0.2份;
聚丙烯酰胺0.2~0.3份;
滑石粉3~10份;
丙烯酸树脂20~30份;
羟基树脂10~15份;
聚合亚麻油1~10份;
异辛酸钒0.1~0.3份;
异辛酸钴0.1~0.3份,各组分以重量份计;
B组分包括:
醇酸树脂10~20份;
高氯化聚乙烯树脂5~15份;
颜料3~8份;
聚醚多元醇0.1~0.6份;
二辛酯0.2~1份;
氯化橡胶20~30份,各组分以重量份计。
2.根据权利要求1所述的户外游乐设备用防水漆,其特征在于,A组分包括:
聚乙烯醇18份;
丙烯酸18份;
磷酸三丁酯0.5份;
磷酸三钠0.18份;
聚丙烯酰胺0.25份;
滑石粉6份;
丙烯酸树脂25份;
羟基树脂12份;
聚合亚麻油5份;
异辛酸钒0.2份;
异辛酸钴0.2份。
3.根据权利要求1所述的户外游乐设备用防水漆,其特征在于,B组分包括:
醇酸树脂15份;
高氯化聚乙烯树脂10份;
颜料5份;
聚醚多元醇0.3份;
二辛酯0.6份;
氯化橡胶25份。
4.一种权利要求1~3任一项所述的户外游乐设备用防水漆的使用方法,其特征在于包括如下步骤:
(1)游乐设备的金属材料表面喷涂组分A;
(2)在步骤(1)处理后的游乐设备表面整体喷涂组分B。
CN201510700674.7A 2015-10-26 2015-10-26 一种户外游乐设备用防水漆及其使用方法 Pending CN105176272A (zh)