一种用于垃圾焚烧尾气处理的吸附剂及其制备方法 Download PDF

Info

Publication number
CN104826611A
CN104826611A CN201510192745.7A CN201510192745A CN104826611A CN 104826611 A CN104826611 A CN 104826611A CN 201510192745 A CN201510192745 A CN 201510192745A CN 104826611 A CN104826611 A CN 104826611A
Authority
CN
China
Prior art keywords
added
adsorbent
preparation
distilled water
stalk
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201510192745.7A
Other languages
English (en)
Inventor
王春保
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
MAANSHAN SHUNDA ENVIRONMENT PROTECTION EQUIPMENT CO Ltd
Original Assignee
MAANSHAN SHUNDA ENVIRONMENT PROTECTION EQUIPMENT CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by MAANSHAN SHUNDA ENVIRONMENT PROTECTION EQUIPMENT CO Ltd filed Critical MAANSHAN SHUNDA ENVIRONMENT PROTECTION EQUIPMENT CO Ltd
Priority to CN201510192745.7A priority Critical patent/CN104826611A/zh
Publication of CN104826611A publication Critical patent/CN104826611A/zh
Pending legal-status Critical Current

Abstract

本发明公开了一种用于垃圾焚烧尾气处理的吸附剂及其制备方法,其特征在于,由以下重量份的原料制成:秸秆90-100、碳酸氢氨0.4-1、钛酸正丁酯25-40、硼酸酯偶联剂0.1-0.5、聚乙二醇3-4、刚玉砂8-12、四氧化三铁4-6、硅藻泥13-16、蒸馏水适量;本发明原料来源丰富,价格低廉,制备工艺简单,不造成二次污染,环境友好,净化垃圾尾气效果好,值得推广。

Description

一种用于垃圾焚烧尾气处理的吸附剂及其制备方法
技术领域
    本发明涉及一种吸附剂领域,具体涉及一种用于垃圾焚烧尾气处理的吸附剂及其制备方法。
背景技术
垃圾焚烧是实现垃圾无害化、减量化、资源化的有效途径,但垃圾焚烧不可避免的会产生二氧化硫、二恶英、重金属等有毒有害气体,其中二恶英是一种强致癌物质,重金属的危害在于它不能被微生物分解且能在生物体内富集,最终通过食物链对人体造成危害,导致癌症及各种疾病;而且重金属还会污染土壤、水体和大气,造成对环境的严重破坏。二恶英和重金属是垃圾焚烧重要的污染源之一,会破坏生态环境的同时严重危害人类健康。
秸秆是农作物生产系统中一项重要的生物质资源,其纤维素含量较高。天然纤维素既是一种可再生资源又是一种新型的吸附材料,它以天然纤维素为基体,有良好的亲水性和多孔结构,具有来源广泛、可再生、可降解、环境友好、价格低廉等多种优点。中国是农业大国,有丰富的秸秆资源,占世界秸秆资源的25%的左右,但是目前对其处置方式依然滞后,大量秸秆被废弃于田间或直接焚烧,这既造成大量的生物质能源的浪费,也给环境带来严重的污染。纳米二氧化钛作为一种友好型光催化剂,具有很好的氧化还原能力,因此在污水处理、空气净化等领域得到了广泛的应用。但是近年来利用各种载体固定纳米二氧化钛制成的吸附剂的光催化效果和回收利用率不高,本发明旨在制备出一种廉价、产率高、能耗少、吸附时间短、制备工艺简单的吸附剂,为吸附剂的发展奠定基础。
发明内容
本发明的目的是提供一种用于垃圾焚烧尾气处理的吸附剂及其制备方法。
为了实现本发明的目的,本发明通过以下方案实施:
一种用于垃圾焚烧尾气处理的吸附剂及其制备方法,由下列重量份的原料制成:秸秆90-100、碳酸氢氨0.4-1、钛酸正丁酯25-40、硼酸酯偶联剂0.1-0.5、聚乙二醇3-4、刚玉砂8-12、四氧化三铁4-6、硅藻泥13-16、蒸馏水适量;
本发明所述一种用于垃圾焚烧尾气处理的吸附剂及其制备方法,由以下具体步骤制成:
(1)将秸秆先用蒸馏水清洗干净,烘干粉碎至8-20目后加到0.3mol/l的盐酸溶液中浸渍,浸渍1-2天后用蒸馏水洗涤成中性后烘干,再将秸秆和碳酸氢氨混合加到马弗炉中以每分钟10~30°C的速度升温,升高温度至600-700°C,恒温保持60-80min,自然冷却至室温;
(2)将刚玉砂、四氧化三铁和硅藻泥加到球磨机中湿法球磨,再加到窑炉中在600-700°C下高温煅烧1-2小时,煅烧后和步骤(1)所得的炭化秸秆、硼酸酯偶联剂混合研磨分散均匀,再将该混合物和聚乙二醇、蒸馏水混合搅拌均匀,加热至50-60°C,形成浆料,喷雾干燥后备用;
(3)将钛酸正丁酯加到3-4倍量的无水乙醇中,搅拌均匀后加入步骤(2)所得的混合物,加速搅拌,搅拌的过程中缓慢加入75%的乙醇70-100ml,用硝酸调节PH至1-2,搅拌30min后,静置陈化1-2天,把溶胶放置在烘箱中于105°C干燥,干燥后研磨成粉末状,放入马弗炉中,于480-520°C下煅烧4-6h即可。
本发明的优点是:本发明利用废弃的秸秆制备生物质炭,实现了废物利用,制备的活性炭比表面积大,吸附效果好,并且利用硼酸酯偶联剂和其他具有吸附作用的材料研磨,增强了材料本身的物理吸附作用,且作为二氧化钛的载体,提高了二氧化钛的光催化活性,且回收利用方便,提高经济效益,本发明原料来源丰富,价格低廉,制备工艺简单,不造成二次污染,环境友好,净化垃圾尾气效果好,值得推广。
具体实施方式
下面通过具体实例对本发明进行详细说明。
一种用于垃圾焚烧尾气处理的吸附剂及其制备方法,由下列重量份(公斤)的原料制成:秸秆96、碳酸氢氨0.6、钛酸正丁酯33、硼酸酯偶联剂0.2、聚乙二醇3、刚玉砂8、四氧化三铁5、硅藻泥16、蒸馏水适量;
本发明所述一种用于垃圾焚烧尾气处理的吸附剂及其制备方法,由以下具体步骤制成:
(1)将秸秆先用蒸馏水清洗干净,烘干粉碎至20目后加到0.3mol/l的盐酸溶液中浸渍,浸渍2天后用蒸馏水洗涤成中性后烘干,再将秸秆和碳酸氢氨混合加到马弗炉中以每分钟10~30°C的速度升温,升高温度至650°C,恒温保持80min,自然冷却至室温;
(2)将刚玉砂、四氧化三铁和硅藻泥加到球磨机中湿法球磨,再加到窑炉中在700°C下高温煅烧1小时,煅烧后和步骤(1)所得的炭化秸秆、硼酸酯偶联剂混合研磨分散均匀,再将该混合物和聚乙二醇、蒸馏水混合搅拌均匀,加热至60°C,形成浆料,喷雾干燥后备用;
(3)将钛酸正丁酯加到3倍量的无水乙醇中,搅拌均匀后加入步骤(2)所得的混合物,加速搅拌,搅拌的过程中缓慢加入75%的乙醇80ml,用硝酸调节PH至1-2,搅拌30min后,静置陈化2天,把溶胶放置在烘箱中于105°C干燥,干燥后研磨成粉末状,放入马弗炉中,于520°C下煅烧6h即可。
经测定,按本发明制备的吸附剂吸附容量为4.51mmol/g,捕集微尘效率为98.2%。

Claims (2)

1.一种用于垃圾焚烧尾气处理的吸附剂及其制备方法,其特征在于,由以下重量份的原料制成:秸秆90-100、碳酸氢氨0.4-1、钛酸正丁酯25-40、硼酸酯偶联剂0.1-0.5、聚乙二醇3-4、刚玉砂8-12、四氧化三铁4-6、硅藻泥13-16、蒸馏水适量。
2.根据权利要求1所述一种用于垃圾焚烧尾气处理的吸附剂及其制备方法,其特征在于,由以下具体步骤制成:
(1)将秸秆先用蒸馏水清洗干净,烘干粉碎至8-20目后加到0.3mol/l的盐酸溶液中浸渍,浸渍1-2天后用蒸馏水洗涤成中性后烘干,再将秸秆和碳酸氢氨混合加到马弗炉中以每分钟10~30°C的速度升温,升高温度至600-700°C,恒温保持60-80min,自然冷却至室温;
(2)将刚玉砂、四氧化三铁和硅藻泥加到球磨机中湿法球磨,再加到窑炉中在600-700°C下高温煅烧1-2小时,煅烧后和步骤(1)所得的炭化秸秆、硼酸酯偶联剂混合研磨分散均匀,再将该混合物和聚乙二醇、蒸馏水混合搅拌均匀,加热至50-60°C,形成浆料,喷雾干燥后备用;
(3)将钛酸正丁酯加到3-4倍量的无水乙醇中,搅拌均匀后加入步骤(2)所得的混合物,加速搅拌,搅拌的过程中缓慢加入75%的乙醇70-100ml,用硝酸调节PH至1-2,搅拌30min后,静置陈化1-2天,把溶胶放置在烘箱中于105°C干燥,干燥后研磨成粉末状,放入马弗炉中,于480-520°C下煅烧4-6h即可。
CN201510192745.7A 2015-04-22 2015-04-22 一种用于垃圾焚烧尾气处理的吸附剂及其制备方法 Pending CN104826611A (zh)