CN103741558B - A kind of manufacture method of antique artistic paper - Google Patents

A kind of manufacture method of antique artistic paper Download PDF

Info

Publication number
CN103741558B
CN103741558B CN201310751596.4A CN201310751596A CN103741558B CN 103741558 B CN103741558 B CN 103741558B CN 201310751596 A CN201310751596 A CN 201310751596A CN 103741558 B CN103741558 B CN 103741558B
Authority
CN
China
Prior art keywords
paper
fibre bundle
slurry
pulp
cylinder
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201310751596.4A
Other languages
Chinese (zh)
Other versions
CN103741558A (en
Inventor
宋俊富
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Shanghai Junyuan Industrial Co., Ltd.
Original Assignee
Spring Source New Material (shanghai) Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Spring Source New Material (shanghai) Co Ltd filed Critical Spring Source New Material (shanghai) Co Ltd
Priority to CN201310751596.4A priority Critical patent/CN103741558B/en
Publication of CN103741558A publication Critical patent/CN103741558A/en
Application granted granted Critical
Publication of CN103741558B publication Critical patent/CN103741558B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention provides a kind of manufacture method of antique artistic paper, it comprises: papermaking part, top sizing and complete part.The main feature of the method adds fibre bundle in slurry, the method adding fibre bundle is adopted to make paper more distinct brilliant, and these fibre bundles present Rejoice sensation through making beating, in excellent paper pulp, drop into fibre bundle can make antique artistic paper have the high-quality performance of modern art paper, makes again the graceful bearing which are added rough ancient paper somewhat.In addition, the present invention selects two following currents paddle cylinder that overflows to have larger shaping area as Kothen sheet former feature, can low concentration online to be ferreted out formation of sheet even, there is good physical property.Therefore antique artistic paper of the present invention can be used in the packaging, business card etc. of printing ancient books books and periodicals, picture album, local and special products.

Description

A kind of manufacture method of antique artistic paper
Technical field
The speciality paper that the invention belongs to culture and arts manufactures field, relates to a kind of manufacture method of antique artistic paper particularly.
Background technology
The artistic paper using all too produced in modern paper technology is perfect, and paper is careful, smooth has no time, bright-colored brilliant, but blemish in an otherwise perfect thing, paper is too dull, so people carry out embossing processing to paper, suppresses three-dimensional pattern, but too regularization.So add again colorful chemical fiber or plastics sand point in dyestuff.They, in paper random distribution, overcome regularization, but chemical fibre is into single state, and fiber is very thin, not eye-catching, and the profile of chemical fibre and sand point is all more stiff.
Summary of the invention
In order to solve the defect existing for the artistic paper using mentioned in background technology, the invention provides a kind of manufacture method of antique artistic paper.The manufacture method of antique artistic paper of the present invention focuses on manufacturing paper with pulp of page, is equipped with the most key again in the process of manufacturing paper with pulp with slurry.Wherein the type selecting of fibre bundle is also crucial especially with preparation.Adopting the fibre bundle of separate sources in order to reach different effects, forming a series of antique artistic paper product with the paper of different color light.The concrete technical scheme of the manufacture method of antique artistic paper of the present invention is as follows:
A manufacture method for antique artistic paper, it comprises: papermaking part, top sizing and complete part, wherein
1. papermaking part
1.1 get the raw materials ready
1.1.1 auxiliary material liquid prepares: auxiliary material comprises dyestuff, color-fixing agent, sizing agent, determines agent and reinforcing agent, accurately take auxiliary material and dissolve stand-by in the dissolvers of specifying completely, and wherein dyestuff must be incubated stored for future use with 90-95 DEG C of hot water dissolving;
1.1.2 the preparation of fibre bundle: the raw material of fibre bundle is be selected from not steam fresh material (i.e. screening reject) in sulfate pulp-making factory in boil house; According to different shape requirement, dogstail, needlebush, leaf wood or not steaming of bast fiber is selected to separate thing as raw material; The concrete preparation flow of fibre bundle is: 1. break into pieces; 2. pull an oar: adopt small-sized beater process, beating consistency 1-2wt%, the maximum fibre bundle of making beating terminal point control by no more than 20 fibrous; 3. wash: carry out in beater; 4. dewater for subsequent use: adopt centrifugal dehydrator dehydration, after dehydration, measure fibre bundle mass dryness fraction, so that metering drops into; Preferably, the colourity in order to improve fibre bundle make more eye-catching step 3. and step 4. between add staining procedure and the washing step after dyeing; Fibre bundle mass dryness fraction: 23-30wt% (fibre bundle in suspension, still has large water gaging to be present in the middle of fibre bundle, i.e. fibre bundle mass dryness fraction=dry fibre bundle weight/(dry fibre bundle weight+water weight) in water after processed)
1.1.3 the preparation of wood pulp: select masson pine, this wood pulp comprises softwood pulp and hardwood pulp, softwood pulp is 1:1 with the operating weight ratio of hardwood pulp, by conical refiner process after hydrabrusher fibration, beating degree is 22-24 ° of SR, and wood pulp refining concentration is 3.5-4.0wt%;
1.1.4 prepare burden: prepare burden and to carry out in pond with slurry, be provided with propeller in pond with slurry, wood pulp and auxiliary material can be made fully to merge, concentration with slurry is 3-3.5wt%, batching sequence is dyeing, applying glue, reinforcement finally add fibre bundle, wherein
Dyeing: at room temperature dye, to wood pulp meter, dye dosage is 0-1wt%, and color-fixing agent is 0-1wt%;
To wood pulp meter, other auxiliary materials (i.e. sizing agent, determine agent and reinforcing agent) consumption is 0.2-3.0wt%, and all auxiliary material liquid must by 200 mesh screen before entering pond with slurry;
Fibre bundle: to wood pulp meter, fibre bundle consumption is 1-10wt%;
1.2 pulp flows: flow apperach comprises consistencyregulator, flow control valve, fan pump and slurry-stablizing case, the slurry of step 1.1.4 gained is diluted to 0.06-0.20wt% from 3.0-3.5wt% by flow apperach, sends into copy paper system with constant concentration, constant slurry amount, stably fluidised form;
1.3 paper makings: carry out in two cylinder multi-cylinder paper machine;
1.3.1 sheet forming: select following current to overflow paddle cylinder, online concentration 0.06-0.2wt%;
1.3.2 squeeze: squeezing is gentle, goes out to squeeze moisture 60-65wt%;
1.3.3 dry: to use many drying cylinders (being no less than 3 drying cylinders) dry, control surface temperature of drier curve, gently dried guarantees that page two sides difference is little: according to paper feed direction, the surface temperature of first drying cylinder 80 ~ 85 DEG C, from second drying cylinder, the surface temperature of each drying cylinder raises gradually until the drying cylinder at middle part reaches maximum surface temperature 100 ~ 105 DEG C, after this surface temperature of each drying cylinder reduces gradually, until last surface temperature of drier 95 DEG C, paper moisture is become to be 3-6wt%;
1.3.4 cooling cylinder: use 2 cooling cylinders to carry out ornamenting to paper, makes paper level and smooth, paper formation.
1.3.5 coil paper: be copied into product and send next part process as a roll;
2. top sizing
Sizing agent is water-soluble substances, and preferably sizing agent is starch, PVA or synthetic latex.Applying glue concentration is 4-6wt%, and resin added is one side 0.3-0.5g/m 2, top sizing idiographic flow: glue application solution is prepared, unreel, two-sided applying glue, oven dry, rolling; Preferably, applying glue concentration is 5wt%, and resin added is one side 0.4g/m 2.
3. complete part
Roll product is processed into sheet product.
3.1 cutting systems: carry out in paper cutter, idiographic flow comprise unreel, trimming, cut paper, paper feeding, stacking.
3.2 selections: reject defective products.
3.3 packagings: pack by specification.
3.4 packings: packaged paper clamping plate are packed.
3.5 product warehousing.
The main feature of the preparation method of antique artistic paper of the present invention adds fibre bundle in slurry, the method adding fibre bundle is adopted to make paper more distinct brilliant, and these fibre bundles present Rejoice sensation through making beating, in excellent paper pulp, drop into fibre bundle can make antique artistic paper have the high-quality performance of modern art paper, makes again the graceful bearing which are added rough ancient paper somewhat.In addition, the present invention selects two following currents paddle cylinder that overflows to have larger shaping area as Kothen sheet former feature, can low concentration online to be ferreted out formation of sheet even, there is good physical property.Because antique artistic paper adds fibre bundle, it and paper fibre adhesion are poor, and easy hair and powder dropping during printing, so the present invention carries out top sizing to antique artistic paper.Therefore antique artistic paper of the present invention can be used in the packaging, business card etc. of printing ancient books books and periodicals, picture album, local and special products.
Accompanying drawing explanation
Fig. 1 is papermaking partial process view;
Fig. 2 is top sizing and completes partial process view.
Detailed description of the invention
Below provide a specific embodiment of the present invention thus more fully the present invention be described, but this and do not mean that the restriction of the scope to claimed claim of the present invention.
Embodiment 1
A manufacture method for antique artistic paper, it comprises: papermaking part, top sizing and complete part, wherein
1. papermaking part
1.1 get the raw materials ready
1.1.1 auxiliary material liquid prepares: auxiliary material comprises dyestuff, color-fixing agent, sizing agent, determines agent and reinforcing agent, accurately take auxiliary material and dissolve stand-by in the dissolvers of specifying completely, and wherein dyestuff must be incubated stored for future use with 90-95 DEG C of hot water dissolving;
1.1.2 the preparation of fibre bundle: the raw material of fibre bundle is be selected from not steam fresh material (i.e. screening reject) in sulfate pulp-making factory in boil house; According to different shape requirement, select dogstail, needlebush, leaf wood or bast fiber do not steam fresh material as raw material; The concrete preparation flow of fibre bundle is: 1. break into pieces; 2. pull an oar: adopt small-sized beater process, beating consistency 1-2wt%, the maximum fibre bundle of making beating terminal point control by no more than 20 fibrous; 3. wash: carry out in beater; 4. dewater for subsequent use: adopt centrifugal dehydrator dehydration, after dehydration, measure fibre bundle mass dryness fraction, so that metering drops into; Preferably, the colourity in order to improve fibre bundle make more eye-catching step 3. and step 4. between add staining procedure and the washing step after dyeing; Fibre bundle mass dryness fraction: 23-30wt% (fibre bundle in suspension, still has large water gaging to be present in the middle of fibre bundle, i.e. fibre bundle mass dryness fraction=dry fibre bundle weight/(dry fibre bundle weight+water weight) in water after processed)
1.1.3 the preparation of wood pulp: select masson pine, this wood pulp comprises softwood pulp and hardwood pulp, softwood pulp is 1:1 with the operating weight ratio of hardwood pulp, accurately take wood pulp and carry out fibration in hydrabrusher, then deliver on 1# and store stock tank, lower storage stock tank is put into when pulling an oar, again with being pumped into conical refiner, slurry after process is delivered on 2# and is store stock tank, utilize slurry position transfer valve to put into lower storage stock tank and carry out second time defibrination, so through repeatedly defibrination circulation until send storage stock tank 2# on stand-by after meeting the requirements of beating degree (22-24 ° of SR), wood pulp refining concentration is 3.5-4.0wt%,
1.1.4 prepare burden: prepare burden and to carry out in pond with slurry, be provided with propeller in pond with slurry, wood pulp and auxiliary material can be made fully to merge, concentration with slurry is 3-3.5wt%, batching sequence is dyeing, applying glue, reinforcement finally add fibre bundle, the slurry prepared is delivered to 1# and destroies forebay and arrive 2# again to destroy forebay stand-by, wherein
Dyeing: at room temperature dye, to wood pulp meter, dye dosage is 0-1wt%, and color-fixing agent is 0-1wt%;
To wood pulp meter, other auxiliary materials (i.e. sizing agent, determine agent and reinforcing agent) consumption is 0.2-3.0wt%, and all auxiliary material liquid must by 200 mesh screen before entering pond with slurry;
Fibre bundle: to wood pulp meter, fibre bundle consumption is 1-10wt%;
1.2 pulp flows: flow apperach comprises consistencyregulator, flow control valve, fan pump and slurry-stablizing case, wherein:
1.2.1 consistencyregulator: 2# copied the pulp dilution of forebay and be stabilized in 1.5wt%;
1.2.2 flow control valve: the slurry of steady concentration is sent in fan pump by setting constant magnitude;
1.2.3 fan pump: by the concentration 0.06-0.20wt% needed for the pulp dilution of constant flow rate to paper sheet formation net;
1.2.4 slurry-stablizing case: the impulsive force eliminating fan pump powerful delivers to paper sheet formation net to starch stream stably;
1.3 paper makings: carry out in two cylinder multi-cylinder paper machine;
1.3.1 sheet forming: select following current to overflow paddle cylinder, online concentration 0.06-0.2wt%;
1.3.2 squeeze: squeezing is gentle, goes out to squeeze moisture 60-65wt%;
1.3.3 dry: to use many drying cylinders (being no less than 3 drying cylinders) dry, control surface temperature of drier curve, gently dried guarantees that page two sides difference is little: according to paper feed direction, the surface temperature of first drying cylinder 80 ~ 85 DEG C, from second drying cylinder, the surface temperature of each drying cylinder raises gradually until the drying cylinder at middle part reaches maximum surface temperature 100 ~ 105 DEG C, after this surface temperature of each drying cylinder reduces gradually, until last surface temperature of drier 95 DEG C, paper moisture is become to be 3-6wt%;
1.3.4 cooling cylinder: use 2 cooling cylinders to carry out ornamenting to paper, makes paper level and smooth, paper formation.
1.3.5 coil paper: be copied into product and send next part process as a roll;
2. top sizing
Sizing agent is starch.Applying glue concentration is 4wt%, and resin added is one side 0.3g/m 2, top sizing idiographic flow: glue application solution is prepared, unreel, two-sided applying glue, oven dry, rolling;
3. complete part
Roll product is processed into sheet product.
3.1 cutting systems: carry out in paper cutter, idiographic flow comprise unreel, trimming, cut paper, paper feeding, stacking.
3.2 selections: reject defective products.
3.3 packagings: pack by specification.
3.4 packings: packaged paper clamping plate are packed.
3.5 product warehousing.
Embodiment 2
Other parts are with embodiment 1, and difference is: in top sizing part, sizing agent is PVA.Applying glue concentration is 5wt%, and resin added is one side 0.4g/m 2.
Embodiment 3
Other parts are with embodiment 1, and difference is: in top sizing part, sizing agent is synthetic latex.Applying glue concentration is 6wt%, and resin added is one side 0.5g/m 2.

Claims (4)

1. a manufacture method for antique artistic paper, it comprises: papermaking part, top sizing and complete part, wherein
1. papermaking part
1.1 get the raw materials ready
1.1.1 auxiliary material liquid prepares: auxiliary material comprises dyestuff, color-fixing agent, sizing agent, determines agent and reinforcing agent, accurately take auxiliary material and dissolve stand-by in the dissolvers of specifying completely, and wherein dyestuff must be incubated stored for future use with 90-95 DEG C of hot water dissolving;
1.1.2 the preparation of fibre bundle: the raw material of fibre bundle is be selected from not steam fresh material in sulfate pulp-making factory in boil house; According to different shape requirement, select dogstail, needlebush, leaf wood or bast fiber do not steam fresh material as raw material; The concrete preparation flow of fibre bundle is: 1. break into pieces; 2. pull an oar: adopt small-sized beater process, beating consistency 1-2wt%, the maximum fibre bundle of making beating terminal point control by no more than 20 fibrous; 3. wash: carry out in beater; 4. dewater for subsequent use: adopt centrifugal dehydrator dehydration, after dehydration, measure fibre bundle mass dryness fraction, so that metering drops into; Fibre bundle mass dryness fraction: 23-30wt%;
1.1.3 the preparation of wood pulp: select masson pine, this wood pulp comprises softwood pulp and hardwood pulp, softwood pulp is 1:1 with the operating weight ratio of hardwood pulp, by conical refiner process after hydrabrusher fibration, beating degree is 22-24 ° of SR, and wood pulp refining concentration is 3.5-4.0wt%;
1.1.4 prepare burden: prepare burden and to carry out in pond with slurry, be provided with propeller in pond with slurry, wood pulp and auxiliary material can be made fully to merge, concentration with slurry is 3-3.5wt%, batching sequence is the fibre bundle that dyeing, applying glue, reinforcement finally add step 1.1.2 and obtain, wherein
Dyeing: at room temperature dye, to wood pulp meter, dye dosage is 0-1wt%, and color-fixing agent is 0-1wt%;
To wood pulp meter, other supplementary product consumptions removed beyond dyestuff and color-fixing agent are 0.2-3.0%, and all auxiliary material liquid must by 200 mesh screen before entering pond with slurry;
Fibre bundle: to wood pulp meter, fibre bundle consumption is 1-10wt%;
1.2 pulp flows: flow apperach comprises consistencyregulator, flow control valve, fan pump and slurry-stablizing case, the slurry of step 1.1.4 gained is diluted to 0.06-0.20wt% from 3.0-3.5wt% by flow apperach, sends into copy paper system with constant concentration, constant slurry amount, stably fluidised form;
1.3 paper makings: carry out in two cylinder multi-cylinder paper machine;
1.3.1 sheet forming: select following current to overflow paddle cylinder, online concentration 0.06-0.2wt%;
1.3.2 squeeze: squeezing is gentle, goes out to squeeze moisture 60-65wt%;
1.3.3 dry: to use many drying cylinders, namely 3 cylinder drieds are no less than, control surface temperature of drier curve, gently dried guarantees that page two sides difference is little: according to paper feed direction, the surface temperature of first drying cylinder 80 ~ 85 DEG C, from second drying cylinder, the surface temperature of each drying cylinder raises gradually until the drying cylinder at middle part reaches maximum surface temperature 100 ~ 105 DEG C, after this surface temperature of each drying cylinder reduces gradually, until last surface temperature of drier 95 DEG C, becomes paper moisture to be 3-6wt%;
1.3.4 cooling cylinder: use 2 cooling cylinders to carry out ornamenting to paper, makes paper level and smooth, paper formation;
1.3.5 coil paper: be copied into product and send next part process as a roll;
2. top sizing
Sizing agent is water-soluble substances, and applying glue concentration is 4-6wt%, and resin added is one side 0.3-0.5g/m 2, top sizing idiographic flow: glue application solution is prepared, unreel, two-sided applying glue, oven dry, rolling;
3. complete part
Roll product is processed into sheet product;
3.1 cutting systems: carry out in paper cutter, idiographic flow comprise unreel, trimming, cut paper, paper feeding, stacking;
3.2 selections: reject defective products;
3.3 packagings: pack by specification;
3.4 packings: packaged paper clamping plate are packed;
3.5 product warehousing.
2. the manufacture method of antique artistic paper according to claim 1, the colourity wherein in order to improve fibre bundle make more eye-catching step in step 1.1.2 3. and step 4. between add staining procedure and the washing step after dyeing.
3. the manufacture method of antique artistic paper according to claim 1, wherein in top sizing, sizing agent is starch, PVA or synthetic latex.
4. the manufacture method of antique artistic paper according to claim 3, wherein in top sizing, applying glue concentration is 5wt%, and resin added is one side 0.4g/m 2.
CN201310751596.4A 2013-12-31 2013-12-31 A kind of manufacture method of antique artistic paper Active CN103741558B (en)