CN103526499A - Dry-type presetting production method of spandex fabric - Google Patents
Dry-type presetting production method of spandex fabric Download PDFInfo
- Publication number
- CN103526499A CN103526499A CN201310482711.2A CN201310482711A CN103526499A CN 103526499 A CN103526499 A CN 103526499A CN 201310482711 A CN201310482711 A CN 201310482711A CN 103526499 A CN103526499 A CN 103526499A
- Authority
- CN
- China
- Prior art keywords
- fabric
- speed
- dry
- setting
- technological requirement
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention relates to the technical field of fabric processing, particularly a dry-type presetting production method of a spandex fabric. The presetting is dry-type presetting. The method is implemented by sending the spandex fabric into a drying oven machine at the speed of 18-25 m/min to carry out presetting treatment, wherein the temperature of the drying oven is set at 190-195 DEG C, the air quantity is 90-95%, the door width is 5-7 cm greater than the door width of the technological requirement, and the gram weight of the lower machine is 5-10 g/m<2> smaller than the gram weight of the technological requirement. The technique enhances the productivity by 50%, and effectively improves the production speed; the fabric feed speed of the traditional squeezing mode is usually only 15 m/min or so, and the fabric feed speed of the dry-type presetting mode can reach 25 m/min; and thus, the cost of more than 500 yuan can be saved per ton of fabric, thereby ensuring the quality stability of the finished product on the premise of enhancing the production speed.
Description
Technical field
The present invention relates to fabric processing technology field, be specifically related to spandex cloth dry type pre-setting production method.
Background technology
Nowadays, the production cost of textile industry is more and more higher, and interests are more and more lower, owing to bleachinging and dyeing rear dressing floor shaping process output, has bottleneck, thereby makes original predetermined production capacity can not meet the demand of plan completely.As everyone knows, first three joint baking oven of pre-setting is the effect of drying substantially, and rear several joints just play desired effects, and therefore how to allow grey cloth not dry directly entering predetermined state is the key that improves speed of production.At present, existing spandex cloth fabric first passes through hopper conventionally, then through squezzing, enters baking oven, and adopts above-mentioned this mode, can consume a large amount of heat energy, and 1 ton of fabric will consume 1 ton of water conventionally, and the speed of service of setting machine is slow, inefficiency.
Summary of the invention
The object of this invention is to provide simple process, simple to operate, production capacity lifting, effectively enhance productivity, and the spandex cloth dry type pre-setting production method reducing production costs.
In order to solve the existing problem of background technology, the present invention is by the following technical solutions: spandex cloth dry type pre-setting production method, concrete operations are as follows: the spandex cloth fabric in drying regime is entered to pre-setting in baking oven machine with the speed of 18~25m/min and process, wherein, baking oven set temperature is 190~195 ℃, air quantity is 90~95%, and door width is set as technological requirement door width and adds 5~7cm control, and lower machine grammes per square metre is that technological requirement grammes per square metre subtracts 5-10g/m
2control.
The present invention has following beneficial effect: spandex cloth dry type pre-setting production method of the present invention, wherein, pre-setting is dry type pre-setting, has omitted former technique spandex cloth first by hopper, spandex cloth is soaked to the operation of floating squezzing.The present invention adopts after above-mentioned technique, its production capacity has promoted 50%, and effectively improved speed of production, the mode of tradition employing squezzing is entered cloth speed and is conventionally only had 15m/min, and adopt dry the entering cloth speed and can reaching 25 m/min of mode that determine, cloth fabric per ton is cost-saved is more than 500 yuan, can guarantee the quality stability of finished product when improving speed of production.In addition, the present invention have simple process, simple to operate, improved production efficiency and reduced the features such as production cost.
The specific embodiment
Below the present invention will be further described in detail.
Embodiment mono-:
Take 30S+70D as example, spandex cloth dry type pre-setting production method, concrete operations are as follows: spandex cloth fabric is entered to pre-setting in baking oven machine with the speed of 18m/min and process, wherein, baking oven set temperature is 190 ℃, and air quantity is 90%, technological requirement door width is 180cm, and technological requirement grammes per square metre is 240 g/m
2,, therefore, in the present embodiment, a door width is set as technological requirement door width and adds 5cm, i.e. 185cm, and lower machine grammes per square metre is that technological requirement grammes per square metre subtracts 5g/m
2, i.e. 235 g/m
2; But traditional technological operation is as follows: spandex cloth fabric is entered to pre-setting in baking oven machine with the speed of 12m/min and process, wherein, baking oven set temperature is 195 ℃, and air quantity is 95%, and a door width is set as 189cm, and lower machine grammes per square metre is 238g/m
2.Dry type pre-setting promotes 50% compared with traditional handicraft production capacity, and traditional technique needs squezzing to produce in addition, will roll bleeding agent and improve stability when consuming water, further increases production cost.The consumption that dry type pre-setting has been cancelled water and bleeding agent does not affect again the quality of finished product.
Embodiment bis-:
Take 30S+40D as example, spandex cloth dry type pre-setting production method, described pre-setting is dry type pre-setting, concrete operations are as follows: spandex cloth fabric is entered to pre-setting in baking oven machine with the speed of 22m/min and process, wherein, baking oven set temperature is 193 ℃, and air quantity is 93%, technological requirement door width is 180cm, and technological requirement grammes per square metre is 240 g/m
2, therefore, in the present embodiment, a door width is set as technological requirement door width and adds 6cm, i.e. 186 cm, and lower machine grammes per square metre is that technological requirement grammes per square metre subtracts 7g/m
2, i.e. 233 g/m
2; But traditional technological operation is as follows: spandex cloth fabric is entered to pre-setting in baking oven machine with the speed of 15m/min and process, wherein, baking oven set temperature is 195 ℃, and air quantity is 95%, and a door width is set as 202cm, and lower machine grammes per square metre is 210g/m
2.Dry type pre-setting promotes 46.7% compared with traditional handicraft production capacity.
Embodiment tri-:
Take 30S+20D as example, spandex cloth dry type pre-setting production method, described pre-setting is dry type pre-setting, concrete operations are as follows: spandex cloth fabric is entered to pre-setting in baking oven machine with the speed of 25m/min and process, wherein, baking oven set temperature is 195 ℃, and air quantity is 95%, technological requirement door width is 180cm, and technological requirement grammes per square metre is 240 g/m
2, therefore, in the present embodiment, a door width is set as technological requirement door width and adds 7cm, i.e. 187cm, and lower machine grammes per square metre is that technological requirement grammes per square metre subtracts 10g/m
2, i.e. 230 g/m
2; But traditional technological operation is as follows: spandex cloth fabric is entered to pre-setting in baking oven machine with the speed of 17m/min and process, wherein, baking oven set temperature is 195 ℃, and air quantity is 95%, and a door width is set as 212cm, and lower machine grammes per square metre is 190g/m
2.Dry type pre-setting promotes 47% compared with traditional handicraft production capacity.
Finally explanation is, above embodiment is only unrestricted in order to technical scheme of the present invention to be described, other modifications that those of ordinary skills make technical scheme of the present invention or be equal to replacement, only otherwise depart from the spirit and scope of technical solution of the present invention, all should be encompassed in the middle of claim scope of the present invention.
Claims (1)
1. spandex cloth dry type pre-setting production method, it is characterized in that, concrete operations are as follows: described spandex cloth is in drying regime, speed with 18~25m/min enters pre-setting processing in baking oven machine, wherein, the baking oven set temperature of described baking oven machine is 190~195 ℃, and air quantity is 90~95%, the door width of described spandex cloth is set as technological requirement door width and adds 5~7cm, and lower machine grammes per square metre is that technological requirement grammes per square metre subtracts 5~10g/m
2.