CN103485205A - Shell fabric process of all cotton water soluble yarn figured cloth - Google Patents

Shell fabric process of all cotton water soluble yarn figured cloth Download PDF

Info

Publication number
CN103485205A
CN103485205A CN201310407548.3A CN201310407548A CN103485205A CN 103485205 A CN103485205 A CN 103485205A CN 201310407548 A CN201310407548 A CN 201310407548A CN 103485205 A CN103485205 A CN 103485205A
Authority
CN
China
Prior art keywords
water soluble
soluble yarn
yarn
cotton
minutes
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201310407548.3A
Other languages
Chinese (zh)
Other versions
CN103485205B (en
Inventor
达紫临
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nantong Sai Hui technology development Limited by Share Ltd
Original Assignee
NANTONG TIANYE GARMENT Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by NANTONG TIANYE GARMENT Co Ltd filed Critical NANTONG TIANYE GARMENT Co Ltd
Priority to CN201310407548.3A priority Critical patent/CN103485205B/en
Publication of CN103485205A publication Critical patent/CN103485205A/en
Application granted granted Critical
Publication of CN103485205B publication Critical patent/CN103485205B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses a shell fabric process of all cotton water soluble yarn figured cloth. The process comprises the following steps: preparation of raw materials; weaving process; dyeing process; post-finishing and sizing. The process disclosed by the invention is precise in weaving and uniform in dyeing, and the shell fabric prepared by using the process is fine and good dyeing and printing effects can be obtained.

Description

A kind of fabric technique of cotton water soluble yarn FIGURED CLOTH
Technical field
The present invention is specifically related to a kind of fabric technique of cotton water soluble yarn FIGURED CLOTH.
Background technology
The fabric technique of traditional cotton water soluble yarn FIGURED CLOTH there will be crack while weaving, and easily reels off raw silk from cocoons, and there will be the inhomogeneous phenomenon of dyeing during dyeing, the phenomenon that has the wrinkle bar produces, excessive concentration or too low, and the effect of dyeing is undesirable, thereby finished product is undesirable, can not reach people's requirement.
Summary of the invention
Goal of the invention: the invention provides a kind of fabric technique of cotton water soluble yarn FIGURED CLOTH, weave precision, even dyeing.
Technical scheme: a kind of fabric technique of cotton water soluble yarn FIGURED CLOTH: comprise the steps:
1) prepare raw material: prepare 21S cotton yarn and 80S water soluble yarn;
2) weaving process: on the machine that is 14 rev/mins at the large jacquard of single face and the normal temperature rotating speed of 30 cun 24G, colored type as requested draws pattern in computer, figure according to computerized version is arranged pin with 21S cotton yarn and 80S water soluble yarn, and both consumptions determine according to pattern;
3) dyeing: boil and wash 20 minutes with the clear water of 95 ℃, allow water soluble yarn fully dissolve; Pre-treatment adds anti wrinkling agent 3G/L, refining agent 1G/L, caustic soda 1G/L and H simultaneously 2o 25G/L, boil after washing 50 minutes and be warming up to 105 ℃ at the clear water of 98 ℃, then boil and wash 20min; Washing; Pickling 1G/L; Add except oxygenase 0.1G/L, each 1G/L of chelated dispersants and levelling agent washes 10 minutes under 40 ℃; Add dyestuff, dyeing 40-50 minute under 60 ℃; Rear arrangement, under 60 ℃, heat is washed 10 minutes; Washing; Pickling 0.5-1G/L; Under 90 ℃, according to different colours, carry out soaping for 1-2 time; Hot wash water is washed twice; Soft; Go out cloth;
4) arrange typing after: upper setting machine specification is 150 ℃ 20 yard/minute, upper overfeeding 25, and lower overfeeding-3, the frame ratio requires large 10cm, and lower machine ratio requires large 5cm, finished product after typing out.
As preferably, in described weaving process, 21S cotton yarn accounts for the 70-90% of total amount, and water soluble yarn accounts for the 10-30% of total amount.
Beneficial effect: the present invention weaves precision, even dyeing, and the fabric of producing is meticulous, and can obtain good dyeing and printing quality.
The specific embodiment
Below in conjunction with specific embodiment, the present invention will be described in detail.
Specific embodiment 1:
A kind of fabric technique of cotton water soluble yarn FIGURED CLOTH: comprise the steps:
1) prepare raw material: prepare 21S cotton yarn and 80S water soluble yarn;
2) weaving process: on the machine that is 14 rev/mins at the large jacquard of single face and the normal temperature rotating speed of 30 cun 24G, colored type as requested draws pattern in computer, figure according to computerized version is arranged pin with 21S cotton yarn and 80S water soluble yarn, and both consumptions determine according to pattern;
3) dyeing: boil and wash 20 minutes with the clear water of 95 ℃, allow water soluble yarn fully dissolve; Pre-treatment adds anti wrinkling agent 3G/L, refining agent 1G/L, caustic soda 1G/L and H simultaneously 2o 25G/L, boil after washing 50 minutes and be warming up to 105 ℃ at the clear water of 98 ℃, then boil and wash 20min; Washing; Pickling 1G/L; Add except oxygenase 0.1G/L, each 1G/L of chelated dispersants and levelling agent washes 10 minutes under 40 ℃; Add dyestuff, under 60 ℃, dyeing is 40 minutes; Rear arrangement, under 60 ℃, heat is washed 10 minutes; Washing; Pickling 0.5G/L; Under 90 ℃, carry out 1 time according to different colours and soap; Hot wash water is washed twice; Soft; Go out cloth;
4) arrange typing after: upper setting machine specification is 150 ℃ 20 yard/minute, upper overfeeding 25, and lower overfeeding-3, the frame ratio requires large 10cm, and lower machine ratio requires large 5cm, finished product after typing out.
Wherein, in weaving process, 21S cotton yarn accounts for 70% of total amount, and water soluble yarn accounts for 10% of total amount.
Specific embodiment 2:
A kind of fabric technique of cotton water soluble yarn FIGURED CLOTH: comprise the steps:
1) prepare raw material: prepare 21S cotton yarn and 80S water soluble yarn;
2) weaving process: on the machine that is 14 rev/mins at the large jacquard of single face and the normal temperature rotating speed of 30 cun 24G, colored type as requested draws pattern in computer, figure according to computerized version is arranged pin with 21S cotton yarn and 80S water soluble yarn, and both consumptions determine according to pattern;
3) dyeing: boil and wash 20 minutes with the clear water of 95 ℃, allow water soluble yarn fully dissolve; Pre-treatment adds anti wrinkling agent 3G/L, refining agent 1G/L, caustic soda 1G/L and H simultaneously 2o 25G/L, boil after washing 50 minutes and be warming up to 105 ℃ at the clear water of 98 ℃, then boil and wash 20min; Washing; Pickling 1G/L; Add except oxygenase 0.1G/L, each 1G/L of chelated dispersants and levelling agent washes 10 minutes under 40 ℃; Add dyestuff, under 60 ℃, dyeing is 50 minutes; Rear arrangement, under 60 ℃, heat is washed 10 minutes; Washing; Pickling 1G/L; Under 90 ℃, carry out 2 times according to different colours and soap; Hot wash water is washed twice; Soft; Go out cloth;
4) arrange typing after: upper setting machine specification is 150 ℃ 20 yard/minute, upper overfeeding 25, and lower overfeeding-3, the frame ratio requires large 10cm, and lower machine ratio requires large 5cm, finished product after typing out.
Wherein, in weaving process, 21S cotton yarn accounts for 90% of total amount, and water soluble yarn accounts for 30% of total amount.
Specific embodiment 3:
A kind of fabric technique of cotton water soluble yarn FIGURED CLOTH: comprise the steps:
1) prepare raw material: prepare 21S cotton yarn and 80S water soluble yarn;
2) weaving process: on the machine that is 14 rev/mins at the large jacquard of single face and the normal temperature rotating speed of 30 cun 24G, colored type as requested draws pattern in computer, figure according to computerized version is arranged pin with 21S cotton yarn and 80S water soluble yarn, and both consumptions determine according to pattern;
3) dyeing: boil and wash 20 minutes with the clear water of 95 ℃, allow water soluble yarn fully dissolve; Pre-treatment adds anti wrinkling agent 3G/L, refining agent 1G/L, caustic soda 1G/L and H simultaneously 2o 25G/L, boil after washing 50 minutes and be warming up to 105 ℃ at the clear water of 98 ℃, then boil and wash 20min; Washing; Pickling 1G/L; Add except oxygenase 0.1G/L, each 1G/L of chelated dispersants and levelling agent washes 10 minutes under 40 ℃; Add dyestuff, under 60 ℃, dyeing is 45 minutes; Rear arrangement, under 60 ℃, heat is washed 10 minutes; Washing; Pickling 0.8G/L; Under 90 ℃, carry out 2 times according to different colours and soap; Hot wash water is washed twice; Soft; Go out cloth;
4) arrange typing after: upper setting machine specification is 150 ℃ 20 yard/minute, upper overfeeding 25, and lower overfeeding-3, the frame ratio requires large 10cm, and lower machine ratio requires large 5cm, finished product after typing out.
Wherein, in weaving process, 21S cotton yarn accounts for 80% of total amount, and water soluble yarn accounts for 20% of total amount.

Claims (2)

1. the fabric technique of a cotton water soluble yarn FIGURED CLOTH, is characterized in that: comprise the steps:
1) prepare raw material: prepare 21S cotton yarn and 80S water soluble yarn;
2) weaving process: on the machine that is 14 rev/mins at the large jacquard of single face and the normal temperature rotating speed of 30 cun 24G, colored type as requested draws pattern in computer, figure according to computerized version is arranged pin with 21S cotton yarn and 80S water soluble yarn, and both consumptions determine according to pattern;
3) dyeing: boil and wash 20 minutes with the clear water of 95 ℃, allow water soluble yarn fully dissolve; Pre-treatment adds anti wrinkling agent 3G/L, refining agent 1G/L, caustic soda 1G/L and H simultaneously 2o 25G/L, boil after washing 50 minutes and be warming up to 105 ℃ at the clear water of 98 ℃, then boil and wash 20min; Washing; Pickling 1G/L; Add except oxygenase 0.1G/L, each 1G/L of chelated dispersants and levelling agent washes 10 minutes under 40 ℃; Add dyestuff, dyeing 40-50 minute under 60 ℃; Rear arrangement, under 60 ℃, heat is washed 10 minutes; Washing; Pickling 0.5-1G/L; Under 90 ℃, according to different colours, carry out soaping for 1-2 time; Hot wash water is washed twice; Soft; Go out cloth;
4) arrange typing after: upper setting machine specification is 150 ℃ 20 yard/minute, upper overfeeding 25, and lower overfeeding-3, the frame ratio requires large 10cm, and lower machine ratio requires large 5cm, finished product after typing out.
2. the fabric technique of cotton water soluble yarn FIGURED CLOTH as claimed in claim 1, it is characterized in that: in described weaving process, 21S cotton yarn accounts for the 70-90% of total amount, and water soluble yarn accounts for the 10-30% of total amount.
CN201310407548.3A 2013-09-10 2013-09-10 Shell fabric process of all cotton water soluble yarn figured cloth Active CN103485205B (en)