CN103321447B - Method for repairing metal fluorocarbon paint outer wall coating defects - Google Patents

Method for repairing metal fluorocarbon paint outer wall coating defects Download PDF

Info

Publication number
CN103321447B
CN103321447B CN201310288567.9A CN201310288567A CN103321447B CN 103321447 B CN103321447 B CN 103321447B CN 201310288567 A CN201310288567 A CN 201310288567A CN 103321447 B CN103321447 B CN 103321447B
Authority
CN
China
Prior art keywords
coating
smooth
special
silk stocking
roller coating
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201310288567.9A
Other languages
Chinese (zh)
Other versions
CN103321447A (en
Inventor
李学平
鲁爱国
邱树林
鲁克
刘芳
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
WUHAN HAIDE-TIANWU NEW MATERIAL Co Ltd
Original Assignee
WUHAN HAIDE-TIANWU NEW MATERIAL Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by WUHAN HAIDE-TIANWU NEW MATERIAL Co Ltd filed Critical WUHAN HAIDE-TIANWU NEW MATERIAL Co Ltd
Priority to CN201310288567.9A priority Critical patent/CN103321447B/en
Publication of CN103321447A publication Critical patent/CN103321447A/en
Application granted granted Critical
Publication of CN103321447B publication Critical patent/CN103321447B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses a method for repairing metal fluorocarbon paint outer wall coating defects. The method includes the nine steps of surface processing, cutting seam manufacturing, batch puttying of a rough putty layer, batch puttying of a fine putty layer, polishing of putty layers, rolling coating of oil primer for fluorocarbon, rolling coating of true-color fluorocarbon finishing coat, rolling coating of coating varnish for the outer wall fluorocarbon and coloring seam by seam. A repair tool used for repairing the metal fluorocarbon paint outer wall coating defects is composed of a rolling drum and a silk stocking, after the rolling drum is soaked, the silk stocking is sleeved on the rolling drum, and then the repair tool is formed. The repair method is not limited by electric power and machinery, saves construction cost, is simple in procedures, convenient to operate and good in effect, protects the environment, and is capable of being used for a steel structure, a mortar wall and a concrete surface layer.

Description

A kind of method for repairing and mending of metal fluorocarbon coating exterior wall painting defect
Technical field
The present invention relates to construction exterior paint technical field, be specifically related to a kind of method for repairing and mending of metal fluorocarbon coating exterior wall painting defect.
Background technology
Metal fluorocarbon coating is a kind of exterior wall coating material of high-quality, and it can resist the adverse effect of ultraviolet, harsh weather, complex environment etc., can resist the osmosis of corrosive ions, and has overlength weatherability and corrosion resistance and excellent self-cleaning function.In engineer applied, designer usually utilizes metal fluorocarbon coating to reach the effect of Aluminium and plastic board curtain wall, adopts it to save construction costs.Thus, in practice of construction process, metal fluorocarbon coating is low with its cost, easy construction, the durable advantage such as self-cleaning attractive in appearance, there is obvious Social benefit and economic benefit.But in engineering practice, easily there is the mass defects such as hollowing, delamination, crack due to metal fluorocarbon coating surface, thus have a strong impact on elevation of building perception, directly impact is caused on workmanship, also have influence on the attractive in appearance of building.Particularly go out local mass defect, when needing to repair, also exist that construction organization inconvenience, scaffold installation difficulty are large, high pressure painting equipment connects that electricity is inconvenient, thinner to pollution of surrounding enviroment etc., inconvenience.
Summary of the invention
The object of the invention is for the problems referred to above, a kind of method for repairing and mending of metal fluorocarbon coating exterior wall painting defect is provided, the defect such as hollowing, delamination, crack that metal fluorocarbon coating coating surface easily occurs is repaired, keep the attractive in appearance of external wall.
For achieving the above object, the technical solution adopted in the present invention is:
A method for repairing and mending for metal fluorocarbon coating exterior wall painting defect, comprises the steps:
(1) surfacing
With the original basic unit of grinder buffing, point mends depressed area, the outstanding position of polishing; Sand paper completely grinds basal plane, bar negative and positive angle, correction windows sideline etc.;
(2) work is made in cutting
Cut cut-off rule or push up embedding glazing bar, filling up Pasteur's glue, extruding Pasteur glue, revises and paints;
(3) criticize and scrape thick putty layer
Batch scrape the thick putty of water-proof elastic, repair basal plane defects, smooth with 300# sand papering, dry too fast time atomized water spray maintenance, do twice altogether, before entering operation, 24 hours, interval, winter, appropriateness extended, and according to user's requirement, all or at least at the position of window frame, beam, post separately drew in the net to process;
When using common thick putty, label lower than 10mpa, and should not mix " gram row are built " special cracking resistant fiber that volume ratio is 0.1% in mortar;
(4) criticize and scrape fine and smooth sublayer
Batch to scrape the fine and smooth son of water-proof elastic, finishing basal plane defects, smooth with 300# sand papering, dry too fast time need wet curing, do twice altogether, before entering next procedure, 7 days, interval, winter, appropriateness extended;
Use the fine and smooth period of the day from 11 p.m. to 1 a.m, " gram row are built " special cracking resistant fiber that volume ratio is 0.1% should be mixed in floating mortar;
(5) polished putty layer
Criticize and scrape fluorine carbon type polished putty, smooth with 800# sand papering, do twice, before entering next procedure, 24 hours, interval, winter, appropriateness extended;
(6) the special oil primer of roller coating fluorine carbon
Use the special repair outfit that cylinder and silk stocking make, the special oil primer of roller coating fluorine carbon, infiltrate basic unit, formed without interface coating, priming paint forms cross-linked structure on basal plane, polishes smooth when grinding with 600# sand paper, before entering next procedure, 24 hours, interval, winter, appropriateness extended;
(7) the real look fluorine carbon finishing paint of roller coating
The real look fluorine carbon finishing paint of roller coating, provides tough and tensile diaphragm and fluorine carbon effect surface, does twice altogether, polish gently with sand paper after constructing for one time dry 3-4 hour, removing surface dirt, technique for grinding should adopt wet grinding, firmly will gently want evenly, sand paper requires 600 orders or 800 orders; During second time roller coating, ensureing, not under sagging prerequisite, coating to be rolled thick, to ensure surperficial levelling effect as far as possible;
(8) the special coating varnish of roller coating exterior wall
Keep even speed roller coating twice coating varnish, the bright and clean lucid and lively feel of coating surface is provided and has more resistant, weather-proof, discoloration-resistant performance;
(9) dividing joint colouring
Tear the face glue that dividing joint pastes off, be in line with one side sticker again on dividing joint both sides;
With Pasteur's glue by dividing joint colouring (twice), midfeather more than 1 hour, note keeping groove mark level and smooth, strain line is straight.
Wherein, described special repair outfit is made up of cylinder and silk stocking, after being soaked by cylinder, silk stocking is enclosed within cylinder, depending on the smooth fineness of metope, can increase the number of plies of silk stocking or select silk stocking hole size.
After partition seam has been painted, also need to check construction quality.
Construction requirement:
1. environmental requirement
Estimate that following environment is not constructed:
---ambient temperature will lower than+4 DEG C;
---ambient temperature will higher than+36 DEG C;
---humidity is higher than 85%;
---before surface drying, (about 2 hours) may rain.
2. user's requirement
Party A-subscriber's architectural drawing: plan view and elevation, identifies tie point, terminal and the interface conditions with other material.
The installation suggestion of party B-subscriber: just special procedure and the periphery situation that need pay special attention to.
C basal plane qualification test report: prove that basal plane meets or exceed the requirement of one-level basal plane regulation.
3. instrument prepares
Perching knife, batch cutter, No. 200-No. 600 sand paper, abrasive machine, polishing lumps of wood block, guiding ruler, filter cloth, cylinder, Electric portable drills.
According to construction ratio, finish paint: curing compound: thinner=2:1:1-1.5, compo, at every turn should more than 7kg, in case precipitation, evaporation, fully stirred once every 5 minutes, in order to avoid precipitation.
Filter with 100# filter cloth, site clearing.
Waste disposal after construction: because this product can pollute environment, my company takes method to be: regain after concentrating, and delivers to the recovery company that qualification can process chemical waste product and processes.
Beneficial effect
Method for repairing and mending step of the present invention is simple, easy to operate, executes engineering cost low, effective, and environmental protection, can be used for steel work, mortar body of wall and concrete surface layer.
Method for repairing and mending of the present invention by electric power, machinery restriction, does not save construction cost.
Accompanying drawing explanation
Fig. 1 is the flow chart of repair technology of the present invention.
Detailed description of the invention
Below in conjunction with accompanying drawing, the present invention will be described in detail, can be easier to be readily appreciated by one skilled in the art, thus make more explicit defining to protection scope of the present invention to make advantages and features of the invention.
As shown in Figure 1, a kind of method for repairing and mending of metal fluorocarbon coating exterior wall painting defect, comprises the steps:
(1) surfacing
With the original basic unit of grinder buffing, point mends depressed area, the outstanding position of polishing; Sand paper completely grinds basal plane, bar negative and positive angle, correction windows sideline etc.;
(2) work is made in cutting
Cut cut-off rule or push up embedding glazing bar, filling up Pasteur's glue, extruding Pasteur glue, revises and paints;
(3) criticize and scrape thick putty layer
Batch scrape the thick putty of water-proof elastic, repair basal plane defects, smooth with 300# sand papering, dry too fast time atomized water spray maintenance, do twice altogether, before entering operation, 24 hours, interval, winter, appropriateness extended, and according to user's requirement, all or at least at the position of window frame, beam, post separately drew in the net to process;
When using common thick putty, label lower than 10mpa, and should not mix " gram row are built " special cracking resistant fiber that volume ratio is 0.1% in mortar;
(4) criticize and scrape fine and smooth sublayer
Batch to scrape the fine and smooth son of water-proof elastic, finishing basal plane defects, smooth with 300# sand papering, dry too fast time need wet curing, do twice altogether, before entering next procedure, 7 days, interval, winter, appropriateness extended;
Use the fine and smooth period of the day from 11 p.m. to 1 a.m, " gram row are built " special cracking resistant fiber that volume ratio is 0.1% should be mixed in floating mortar;
(5) polished putty layer
Criticize and scrape fluorine carbon type polished putty, smooth with 800# sand papering, do twice, before entering next procedure, 24 hours, interval, winter, appropriateness extended;
(6) the special oil primer of roller coating fluorine carbon
Use the special repair outfit that cylinder and silk stocking make, the special oil primer of roller coating fluorine carbon, infiltrate basic unit, formed without interface coating, priming paint forms cross-linked structure on basal plane, polishes smooth when grinding with 600# sand paper, before entering next procedure, 24 hours, interval, winter, appropriateness extended;
(7) the real look fluorine carbon finishing paint of roller coating
The real look fluorine carbon finishing paint of roller coating, provides tough and tensile diaphragm and fluorine carbon effect surface, does twice altogether, polish gently with sand paper after constructing for one time dry 3-4 hour, removing surface dirt, technique for grinding should adopt wet grinding, firmly will gently want evenly, sand paper requires 600 orders or 800 orders; During second time roller coating, ensureing, not under sagging prerequisite, coating to be rolled thick, to ensure surperficial levelling effect as far as possible;
(8) the special coating varnish of roller coating exterior wall
Keep even speed roller coating twice coating varnish, the bright and clean lucid and lively feel of coating surface is provided and has more resistant, weather-proof, discoloration-resistant performance;
(9) dividing joint colouring
Tear the face glue that dividing joint pastes off, be in line with one side sticker again on dividing joint both sides;
With Pasteur's glue by dividing joint colouring (twice), midfeather more than 1 hour, note keeping groove mark level and smooth, strain line is straight.
Wherein, described special repair outfit is made up of cylinder and silk stocking, after being soaked by cylinder, silk stocking is enclosed within cylinder, depending on the smooth fineness of metope, can increase the number of plies of silk stocking or select silk stocking hole size.
After partition seam has been painted, also need to check construction quality.
Construction requirement:
1. environmental requirement
Estimate that following environment is not constructed:
---ambient temperature will lower than+4 DEG C;
---ambient temperature will higher than+36 DEG C;
---humidity is higher than 85%;
---before surface drying, (about 2 hours) may rain.
2. user's requirement
Party A-subscriber's architectural drawing: plan view and elevation, identifies tie point, terminal and the interface conditions with other material.
The installation suggestion of party B-subscriber: just special procedure and the periphery situation that need pay special attention to.
C basal plane qualification test report: prove that basal plane meets or exceed the requirement of one-level basal plane regulation.
3. instrument prepares
Perching knife, batch cutter, No. 200-No. 600 sand paper, abrasive machine, polishing lumps of wood block, guiding ruler, filter cloth, cylinder, Electric portable drills.
According to construction ratio, finish paint: curing compound: thinner=2:1:1-1.5, compo, at every turn should more than 7kg, in case precipitation, evaporation, fully stirred once every 5 minutes, in order to avoid precipitation.
Filter with 100# filter cloth, site clearing.
Waste disposal after construction: because this product can pollute environment, my company takes method to be: regain after concentrating, and delivers to the recovery company that qualification can process chemical waste product and processes.
Last it is noted that obviously, above-described embodiment is only for example of the present invention is clearly described, and the restriction not to embodiment.For those of ordinary skill in the field, can also make other changes in different forms on the basis of the above description.Here exhaustive without the need to also giving all embodiments.And thus the apparent change of amplifying out or variation be still among protection scope of the present invention.

Claims (3)

1. a method for repairing and mending for metal fluorocarbon coating exterior wall painting defect, is characterized in that, comprises the steps:
(1) surfacing
With the original basic unit of grinder buffing, point mends depressed area, the outstanding position of polishing; Sand paper completely grinds basal plane, bar negative and positive angle, correction windows sideline;
(2) work is made in cutting
Cut cut-off rule or push up embedding glazing bar, filling up Pasteur's glue, extruding Pasteur glue, revises and paints;
(3) criticize and scrape thick putty layer and criticize and scrape the thick putty of water-proof elastic, repair basal plane defects, with 300 #sand papering is smooth, dry too fast time atomized water spray maintenance, do twice altogether, before entering next procedure, 24 hours, interval, winter extends 5-10 hour, all or at least at the position of window frame, beam, post separately draws in the net process; When using common thick putty, label lower than 10MPa, and should not mix " gram row are built " special cracking resistant fiber that volume ratio is 0.1% in mortar;
(4) criticize and scrape fine and smooth sublayer
Criticize and scrape the fine and smooth son of water-proof elastic, finishing basal plane defects, with 300 #sand papering is smooth, dry too fast time need wet curing, do twice altogether, before entering next procedure, 7 days, interval, winter extends 2-3 days; Use the fine and smooth period of the day from 11 p.m. to 1 a.m, " gram row are built " special cracking resistant fiber that volume ratio is 0.1% should be mixed in floating mortar;
(5) polished putty layer
Criticize and scrape fluorine carbon type polished putty, with 800 #sand papering is smooth, does twice, before entering next procedure, and 24 hours, interval, winter extends 5-10 hour;
(6) the special oil primer of roller coating fluorine carbon
Use the special repair outfit that cylinder and silk stocking make, the special oil primer of roller coating fluorine carbon, infiltrate basic unit, formed without interface coating, priming paint forms cross-linked structure on basal plane, with 600 #sand papering is smooth, before entering next procedure, and 24 hours, interval, winter extends 5-10 hour;
(7) the real look fluorine carbon finishing paint of roller coating
Use the real look fluorine carbon finishing paint of special repair outfit roller coating, tough and tensile diaphragm and fluorine carbon effect surface are provided, do twice altogether, polish gently with sand paper after constructing for one time dry 3-4 hour, removing surface dirt, technique for grinding should adopt wet grinding, and firmly will gently want evenly, sand paper requires 600 orders or 800 orders; During second time roller coating, ensureing, not under sagging prerequisite, coating to be rolled thick, to ensure surperficial levelling effect as far as possible;
(8) the special coating varnish of roller coating exterior wall
Use special repair outfit to keep even speed roller coating twice coating varnish, the bright and clean lucid and lively feel of coating surface is provided and has more resistant, weather-proof, discoloration-resistant performance;
(9) dividing joint colouring
Tear the face glue that dividing joint pastes off, be in line with one side sticker again on dividing joint both sides; With Pasteur's glue by dividing joint colouring twice, midfeather more than 1 hour, note keeping groove mark level and smooth, strain line is straight.
2. method for repairing and mending according to claim 1, it is characterized in that: described in step (6), (7) and (8), special repair outfit is made up of cylinder and silk stocking, after cylinder is soaked, silk stocking are enclosed within cylinder, depending on the smooth fineness of metope, increase the number of plies of silk stocking or select silk stocking hole size.
3. method for repairing and mending according to claim 1, is characterized in that: coating used meets finish paint: curing compound: thinner=2: 1: 1-1.5, and compo is no more than 7kg at every turn, in case precipitation, evaporation, fully stirred once every 5 minutes, in order to avoid precipitation.
CN201310288567.9A 2013-07-10 2013-07-10 Method for repairing metal fluorocarbon paint outer wall coating defects Active CN103321447B (en)