CN103232822A - 一种含有有机膨润土的包装用胶粘剂及其制备方法 - Google Patents

一种含有有机膨润土的包装用胶粘剂及其制备方法 Download PDF

Info

Publication number
CN103232822A
CN103232822A CN2013101185744A CN201310118574A CN103232822A CN 103232822 A CN103232822 A CN 103232822A CN 2013101185744 A CN2013101185744 A CN 2013101185744A CN 201310118574 A CN201310118574 A CN 201310118574A CN 103232822 A CN103232822 A CN 103232822A
Authority
CN
China
Prior art keywords
parts
add
rubber
organobentonite
chloroprene rubber
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN2013101185744A
Other languages
English (en)
Other versions
CN103232822B (zh
Inventor
刘祥鹏
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Anhui Fenghuangsong Packaging Co ltd
Original Assignee
QINGYANG HUADING PACKAGING CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by QINGYANG HUADING PACKAGING CO Ltd filed Critical QINGYANG HUADING PACKAGING CO Ltd
Priority to CN201310118574.4A priority Critical patent/CN103232822B/zh
Publication of CN103232822A publication Critical patent/CN103232822A/zh
Application granted granted Critical
Publication of CN103232822B publication Critical patent/CN103232822B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种含有有机膨润土的包装用胶粘剂及其制备方法。其由下列重量份的原料组成:氯丁橡胶(CR244)25-30、环己烷55-65、甲苯120-150、醋酸乙酯20-30、三氯甲烷10-15、2402酚醛树脂20-30、古马隆树脂5-8、干酪素5-10、甲基三乙氧基硅烷2-3、N-甲基-2-吡咯烷酮0.2-0.4、4,4’-二苯基甲烷二异氰酸酯1-2、氯化石蜡3-5、司盘-800.25-0.35、丁腈橡胶(N220S)8-12、丁基橡胶(BBK232)5-10、活性氧化锌1-1.5、活性氧化镁2-3、硫磺0.5-1、有机膨润土3-5、石英粉2-4等。本发明胶粘剂具有优良的耐高、低温性、耐磨性,粘结强度高,耐水防潮,贮存稳定性好,环保性好,使用效果好且方便。

Description

一种含有有机膨润土的包装用胶粘剂及其制备方法
技术领域
本发明涉及一种胶粘剂,具体涉及一种含有有机膨润土的包装用胶粘剂及其制备方法。
背景技术
包装用胶粘剂是在包装行业快速发展的基础上产生并发展壮大的,包装用胶粘剂的性能、质量直接影响了包装效果和质量,目前包装用的胶粘剂普遍存在耐热性较差,耐寒性不佳,耐磨性差,贮存稳定性差等缺点。为了克服传统的胶粘剂的缺点,通过改进配方,从而生产出一种新型包装用胶粘剂。
发明内容
本发明的目的是提供一种耐温性好、耐磨性好、粘结强度高、贮存稳定性好的含有有机膨润土的包装用胶粘剂及其制备方法。
本发明采用的技术方案如下:
   一种含有有机膨润土的包装用胶粘剂,由下列重量份的原料组成:氯丁橡胶(CR244)25-30、环己烷55-65、甲苯120-150、醋酸乙酯20-30、三氯甲烷10-15、2402酚醛树脂20-30、古马隆树脂5-8、干酪素5-10、甲基三乙氧基硅烷2-3、N-甲基-2-吡咯烷酮 0.2-0.4、4,4’-二苯基甲烷二异氰酸酯1-2、氯化石蜡3-5、司盘-80 0.25-0.35、丁腈橡胶(N220S)8-12、丁基橡胶(BBK232)5-10、活性氧化锌1-1.5、活性氧化镁2-3、硫磺0.5-1、有机膨润土3-5、石英粉2-4、沉淀白炭黑3-4、防老剂NBC 1-2、防老剂ODA 0.5-1、促进剂ZDC 0.5-1.5、促进剂DM 0.5-1、抗氧剂1010 1-1.5、硬脂酸钡1-2、柠檬酸三乙酯 2-3、癸二酸二丁酯1-2、改性淀粉2-4。
    所述的改性淀粉以下方法制得:将木薯淀粉和双氧水按2-3:1的比例进行氧化得木薯氧化淀粉,向木薯氧化淀粉中2-3%的羧甲基纤维素、4-6%的木质素磺酸钠、2-3%的海藻酸钠、3-5%的草木灰,充分混合均匀,将其干燥至含水量5-8%,然后在140-160℃加热2-3h,产物经冷却、干燥、粉碎后研磨成粉末即可。
    一种含有有机膨润土的包装用胶粘剂的制备方法,包括以下步骤:
    (1)将环己烷加入反应釜中,加入活性氧化镁,搅拌混合10-15min,再连续加入称量好的2402酚醛树脂,搅拌3-4h至完全溶解,加入N-甲基-2-吡咯烷酮于25-28℃下搅拌反应6-10h,静置20-24h,过滤去除沉淀物,即得预反应液,待用;
    (2)将氯丁橡胶加入双螺杆挤出机中,升温至140-150℃,待其成为熔融状态时,加入有机膨润土,在400-600rpm的转速下熔融共混20-30min,然后挤出造粒,冷却至常温即得氯丁橡胶包覆有机膨润土粒子;
    (3)将上述制得的氯丁橡胶包覆有机膨润土粒子与氯化石蜡、丁腈橡胶、丁基橡胶、活性氧化锌、硫磺、石英粉、沉淀白炭黑、防老剂NBC、促进剂ZDC 、促进剂DM、抗氧剂1010、硬脂酸钡、柠檬酸三乙酯、癸二酸二丁酯送入炼胶机中在40-50℃下进行混炼,混炼3-5次,然后薄通6-8次下片,冷却至常温后剪成碎片;
    (4)取上述碎片加入甲苯、醋酸乙酯和三氯甲烷,充分搅拌均匀,使碎片全部溶解,再加入4,4’-二苯基甲烷二异氰酸酯、古马隆树脂、甲基三乙氧基硅烷和司盘-80,搅拌均匀反应4-6h;
    (5)在上述反应液中加入预反应液、防老剂ODA、干酪素和改性淀粉,搅拌1-2h即得成品。
    本发明的有益效果:
    本发明通过对工艺改进,利用氯丁橡胶包覆有机膨润土制粒,可以明显改善有机膨润土与橡胶的相容性,从而提高包装胶的弯曲、抗拉强度和耐磨性等性能。本发明利用2402酚醛树脂与活性氧化镁生成螯合树脂,可以提高氯丁胶粘剂的耐水性和耐热性,延长粘性保持时间。本发明通过对淀粉进行改性,可以进一步提高包装胶的粘接强度和耐水性,并具有成本低,效果优良的特点。本发明胶粘剂具有优良的耐高、低温性、耐磨性,粘结强度高,耐水防潮,贮存稳定性好,环保性好,使用效果好且方便。
具体实施方式
    下面结合具体实施例对本发明作进一步的说明。      
    一种含有有机膨润土的包装用胶粘剂,由下列重量份的原料组成:氯丁橡胶(CR244)28份、环己烷60份、甲苯140份、醋酸乙酯 30份、三氯甲烷15份、2402酚醛树脂 27份、古马隆树脂6份、干酪素8份、甲基三乙氧基硅烷2份、N-甲基-2-吡咯烷酮 0.3份、4,4’-二苯基甲烷二异氰酸酯1.5份、氯化石蜡4份、司盘-80 0.3份、丁腈橡胶(N220S)10份、丁基橡胶(BBK232)10份、活性氧化锌1.5份、活性氧化镁2.5份、硫磺0.7份、有机膨润土4份、石英粉4份、沉淀白炭黑3份、防老剂NBC 1份、防老剂ODA 0.8份、促进剂ZDC 1份、促进剂DM 0.5份、抗氧剂1010 1份、硬脂酸钡1.5份、柠檬酸三乙酯 2份、癸二酸二丁酯2份、改性淀粉2份。
    所述的改性淀粉以下方法制得:将木薯淀粉和双氧水按2.5:1的比例进行氧化得木薯氧化淀粉,向木薯氧化淀粉中3%的羧甲基纤维素、5%的木质素磺酸钠、3%的海藻酸钠、3%的草木灰,充分混合均匀,将其干燥至含水量7%,然后在160℃加热2h,产物经冷却、干燥、粉碎后研磨成粉末即可。
    一种含有有机膨润土的包装用胶粘剂的制备方法,包括以下步骤:
    (1)将环己烷加入反应釜中,加入活性氧化镁,搅拌混合10min,再连续加入称量好的2402酚醛树脂,搅拌3h至完全溶解,加入N-甲基-2-吡咯烷酮于26℃下搅拌反应8h,静置24h,过滤去除沉淀物,即得预反应液,待用;
    (2)将氯丁橡胶加入双螺杆挤出机中,升温至150℃,待其成为熔融状态时,加入有机膨润土,在500rpm的转速下熔融共混20min,然后挤出造粒,冷却至常温即得氯丁橡胶包覆有机膨润土粒子;
    (3)将上述制得的氯丁橡胶包覆有机膨润土粒子与氯化石蜡、丁腈橡胶、丁基橡胶、活性氧化锌、硫磺、石英粉、沉淀白炭黑、防老剂NBC、促进剂ZDC 、促进剂DM、抗氧剂1010、硬脂酸钡、柠檬酸三乙酯、癸二酸二丁酯送入炼胶机中在45℃下进行混炼,混炼4次,然后薄通6次下片,冷却至常温后剪成碎片;
    (4)取上述碎片加入甲苯、醋酸乙酯和三氯甲烷,充分搅拌均匀,使碎片全部溶解,再加入4,4’-二苯基甲烷二异氰酸酯、古马隆树脂、甲基三乙氧基硅烷和司盘-80,搅拌均匀反应5h;
(5)在上述反应液中加入预反应液、防老剂ODA、干酪素和改性淀粉,搅拌1h即得成品。
本实施例制得的胶黏剂的性能测试结果如下:
拉伸强度(MPa):44;
弯曲强度(MPa):65;
压缩强度(MPa):85;
抗拉强度(MPa):37;
剥离强度(N/cm):54;
剪切强度(MPa):28;
耐介质性能(在90℃溶液中浸3天后的剪切强度保持率/%):0#柴油98.8、蒸馏水99.7;
耐磨性(滑动摩擦磨损体积/mm3):3.78;
耐热老化性(80-100℃下7天后粘合强度/N/cm):36;
耐低温性:-30℃下7天不冻结;
耐久性:室内使用10-20年,室外3-5年;
 使用本发明粘结剂的纸箱泡在水中,48小时不脱胶,纸箱干燥后,粘合良好,质量不变。

Claims (3)

1.一种含有有机膨润土的包装用胶粘剂,其特征在于,由下列重量份的原料组成:氯丁橡胶(CR244)25-30、环己烷55-65、甲苯120-150、醋酸乙酯20-30、三氯甲烷10-15、2402酚醛树脂20-30、古马隆树脂5-8、干酪素5-10、甲基三乙氧基硅烷2-3、N-甲基-2-吡咯烷酮 0.2-0.4、4,4’-二苯基甲烷二异氰酸酯1-2、氯化石蜡3-5、司盘-80 0.25-0.35、丁腈橡胶(N220S)8-12、丁基橡胶(BBK232)5-10、活性氧化锌1-1.5、活性氧化镁2-3、硫磺0.5-1、有机膨润土3-5、石英粉2-4、沉淀白炭黑3-4、防老剂NBC 1-2、防老剂ODA 0.5-1、促进剂ZDC 0.5-1.5、促进剂DM 0.5-1、抗氧剂1010 1-1.5、硬脂酸钡1-2、柠檬酸三乙酯 2-3、癸二酸二丁酯1-2、改性淀粉2-4。
2.根据权利要求1所述的含有有机膨润土的包装用胶粘剂,其特征在于,所述的改性淀粉以下方法制得:将木薯淀粉和双氧水按2-3:1的比例进行氧化得木薯氧化淀粉,向木薯氧化淀粉中2-3%的羧甲基纤维素、4-6%的木质素磺酸钠、2-3%的海藻酸钠、3-5%的草木灰,充分混合均匀,将其干燥至含水量5-8%,然后在140-160℃加热2-3h,产物经冷却、干燥、粉碎后研磨成粉末即可。
3.一种如权利要求1所述的含有有机膨润土的包装用胶粘剂的制备方法,其特征在于包括以下步骤:
(1)将环己烷加入反应釜中,加入活性氧化镁,搅拌混合10-15min,再连续加入称量好的2402酚醛树脂,搅拌3-4h至完全溶解,加入N-甲基-2-吡咯烷酮于25-28℃下搅拌反应6-10h,静置20-24h,过滤去除沉淀物,即得预反应液,待用;
(2)将氯丁橡胶加入双螺杆挤出机中,升温至140-150℃,待其成为熔融状态时,加入有机膨润土,在400-600rpm的转速下熔融共混20-30min,然后挤出造粒,冷却至常温即得氯丁橡胶包覆有机膨润土粒子;
(3)将上述制得的氯丁橡胶包覆有机膨润土粒子与氯化石蜡、丁腈橡胶、丁基橡胶、活性氧化锌、硫磺、石英粉、沉淀白炭黑、防老剂NBC、促进剂ZDC 、促进剂DM、抗氧剂1010、硬脂酸钡、柠檬酸三乙酯、癸二酸二丁酯送入炼胶机中在40-50℃下进行混炼,混炼3-5次,然后薄通6-8次下片,冷却至常温后剪成碎片;
(4)取上述碎片加入甲苯、醋酸乙酯和三氯甲烷,充分搅拌均匀,使碎片全部溶解,再加入4,4’-二苯基甲烷二异氰酸酯、古马隆树脂、甲基三乙氧基硅烷和司盘-80,搅拌均匀反应4-6h;
(5)在上述反应液中加入预反应液、防老剂ODA、干酪素和改性淀粉,搅拌1-2h即得成品。
CN201310118574.4A 2013-04-07 2013-04-07 一种含有有机膨润土的包装用胶粘剂及其制备方法 Active CN103232822B (zh)