CN103056140B - 一种在玻璃上胶粘配件后的清胶方法 - Google Patents

一种在玻璃上胶粘配件后的清胶方法 Download PDF

Info

Publication number
CN103056140B
CN103056140B CN201210553228.4A CN201210553228A CN103056140B CN 103056140 B CN103056140 B CN 103056140B CN 201210553228 A CN201210553228 A CN 201210553228A CN 103056140 B CN103056140 B CN 103056140B
Authority
CN
China
Prior art keywords
glass
glue
accessory
gel resin
conformable region
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201210553228.4A
Other languages
English (en)
Other versions
CN103056140A (zh
Inventor
黄奖华
李珍
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Xiuning Qiyun Urban Construction Investment Co.,Ltd.
Original Assignee
HUANGSHAN CHINA DISPLAY TECHNOLOGY CO LTD
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by HUANGSHAN CHINA DISPLAY TECHNOLOGY CO LTD filed Critical HUANGSHAN CHINA DISPLAY TECHNOLOGY CO LTD
Priority to CN201210553228.4A priority Critical patent/CN103056140B/zh
Publication of CN103056140A publication Critical patent/CN103056140A/zh
Application granted granted Critical
Publication of CN103056140B publication Critical patent/CN103056140B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

一种在玻璃上胶粘配件后的清胶方法,包括以下步骤:(1)在玻璃与配件贴合区外沿设置可剥胶;(2)烘烤可剥胶:将玻璃放入60~170℃的容器中烘烤10~15分钟取出;(3)在贴合区,用UV胶粘合配件和玻璃;(4)固化UV胶;(5)待UV胶固化,撕下可剥胶,即可清除落在贴合区外沿的残余胶水。本发明可清除胶水残余,方便快捷,有效提高生产效率,同时,避免采用尖锐物刮除固化后的胶水时刮伤产品,降低产品报废率。可广泛应用于玻璃粘合清胶领域。

Description

一种在玻璃上胶粘配件后的清胶方法
技术领域
本发明涉及一种在玻璃上胶粘配件后的清胶方法。
背景技术
近年来,随着触摸屏在消费性电子产品中的广泛应用,人们对触摸屏的需求量也越来越大,这就要求生产厂家要在原有的生产基础上不断地提升产能,同时提高产品的良率。在触摸屏的生产过程中,要将钢化玻璃(外形尺寸大于ITO玻璃)与ITO玻璃通过UV胶水贴合在一起,然后再进行固化及扩散的处理。但是在处理的过程中,会有一部分的UV胶水溢出而流到钢化玻璃的四周表面上,导致了产品的外观不良,导致后续要添加一项员工刮胶擦胶的工序,这严重影响了产品的生产效率,如刮胶手法不当,还会影响到产品的良率。
发明内容
本发明的目的是提供一种在玻璃上胶粘配件后的清胶方法,解决现有玻璃产品生产过程中采用UV胶粘合固化后清理不方便的问题。
本发明解决其技术问题所采用的技术方案是:一种在玻璃上胶粘配件后的清胶方法,包括以下步骤:
(1)在玻璃与配件贴合区外沿设置可剥胶;
(2)烘烤可剥胶:将玻璃放入60~170℃的容器中烘烤10~15分钟取出;
(3)在贴合区,用UV胶粘合配件和玻璃;
(4)固化UV胶;
(5)待UV胶固化,撕下可剥胶,即可清除落在非贴合区的残余胶水。
优选的,所述的可剥胶通过丝印的方式设置在贴合区外沿。
优选的,步骤2中所述的烘烤分为3个阶段,3个阶段的温度依次为170℃,140℃,60℃,三个阶段的时间依次为3分钟,5分钟和5分钟。
为使玻璃表面清洁,在步骤3和步骤4之间还需要将玻璃贴合面与配件贴合面进行清洁处理。
为使UV胶扩散均匀,在步骤4和步骤5之间还增加了将贴合后的玻璃放在75℃至85℃的加热平台上使UV胶扩散均匀。
优选的,所述的可剥胶的厚度为20um~100um。
本发明的有益效果:通过在非粘合区设置可剥胶,使得产品粘结后的胶水残余直接落在可剥胶上,粘结完成后只需将可剥胶撕下,即可清除胶水残余,方便快捷,有效提高生产效率,同时,避免采用尖锐物刮除固化后的胶水时刮伤产品,降低产品报废率。
具体实施方式
实施例1:一种触摸屏贴合后的清胶方法,所述的触摸屏包括钢化玻璃层和粘合在钢化玻璃层上的导电玻璃层,所述的清胶方法包括以下步骤:(1)在钢化玻璃与配件贴合区外沿丝印可剥胶;可剥胶的厚度为20um~100um。
(2)烘烤可剥胶:将钢化玻璃放入60~170℃的容器中烘烤10~15分钟取出;
(3)将钢化玻璃贴合面与导电玻璃贴合面进行清洁处理;
(4)在贴合区,用UV胶粘合钢化玻璃层和导电玻璃层;
(5)将贴合后的触摸屏放在75℃至85℃的加热平台上使UV胶扩散均匀。
(6)固化UV胶:用光照射UV胶使其固化;
(7)待UV胶固化,撕下可剥胶,即可清除落在贴合区外沿的残余胶水。
其中步骤2中所述的烘烤分为3个阶段,3个阶段的温度依次为170℃,140℃,60℃,三个阶段的时间依次为3分钟,5分钟和5分钟。
实施例2:一种液晶显示屏贴合后的清胶方法,所述的液晶显示屏包括第一导电玻璃和第二导电玻璃,所述的清胶方法包括以下步骤:(1)在第一导电玻璃与第二导电玻璃贴合区的外沿丝印可剥胶;可剥胶的厚度为20um~100um。
(2)烘烤可剥胶:将第一导电玻璃体放入60~170℃的容器中烘烤10~15分钟取出;
(3)将第一导电玻璃贴合面与第二导电玻璃贴合面进行清洁处理;
(4)将第二导电玻璃放入第一导电玻璃的贴合区,用UV胶粘合;
(5)将贴合后的玻璃放在75℃至85℃的加热平台上使UV胶扩散均匀。
(6)固化UV胶:用光照射UV胶使其固化;
(7)待UV胶固化,撕下可剥胶,即可清除落在贴合区外沿的残余胶水。
其中步骤2中所述的烘烤分为3个阶段,3个阶段的温度依次为170℃,140℃,60℃,三个阶段的时间依次为3分钟,5分钟和5分钟。

Claims (4)

1.一种在玻璃上胶粘配件后的清胶方法,包括以下步骤:
(1)在玻璃与配件贴合区外沿设置可剥胶;
(2)烘烤可剥胶:将玻璃放入60~170℃的容器中烘烤10~15分钟取出;
(3)在贴合区,用UV胶粘合配件和玻璃;
(4)固化UV胶;
(5)待UV胶固化,撕下可剥胶,即可清除落在贴合区外沿的残余胶水;
所述的可剥胶通过丝印的方式设置在贴合区外沿;
所述步骤2中所述的烘烤分为3个阶段,3个阶段的温度依次为170℃,140℃,60℃,三个阶段的时间依次为3分钟,5分钟和5分钟。
2.如权利要求1所述的在玻璃上胶粘配件后的清胶方法,其特征在于:在步骤3和步骤4之间还需要将玻璃贴合面与配件贴合面进行清洁处理。
3.如权利要求1所述的在玻璃上胶粘配件后的清胶方法,其特征在于:在步骤4和步骤5之间还增加了将贴合后的玻璃放在75℃至85℃的加热平台上使UV胶扩散均匀。
4.如权利要求1至3中任一项所述的在玻璃上胶粘配件后的清胶方法,其特征在于:所述的可剥胶的厚度为20um~100um。
CN201210553228.4A 2012-12-18 2012-12-18 一种在玻璃上胶粘配件后的清胶方法 Active CN103056140B (zh)