CN1030143C - Mastic neoprene water-proof paint and preparation technology - Google Patents
Mastic neoprene water-proof paint and preparation technology Download PDFInfo
- Publication number
- CN1030143C CN1030143C CN 93116690 CN93116690A CN1030143C CN 1030143 C CN1030143 C CN 1030143C CN 93116690 CN93116690 CN 93116690 CN 93116690 A CN93116690 A CN 93116690A CN 1030143 C CN1030143 C CN 1030143C
- Authority
- CN
- China
- Prior art keywords
- water
- pitch
- neoprene
- waterproof paint
- mastic
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Fee Related
Abstract
The present invention relates to waterproof paint and a production technology thereof, particularly to mastic neoprene waterproof paint used for preventing moisture and resisting leakage in building engineering, and the production technology thereof. The mastic neoprene waterproof paint is mainly composed of 60<#> petroleum asphalt, PVA (17-88 type), an emulsifying agent TOT (or NOT), a neoprene adhesive, fillers, water, etc. The technology process of the production technology comprises three processes such as petroleum asphalt fusion, emulsion preparation and finished product preparation. The technology process is fully closed and does not generate the three wastes. The waterproof paint is widely used for roofs, floors, basements, reservoirs, storehouses and various water conservancy facilities. The product has the advantages of high adhesive strength, elastic film layer, corrosion resistance, ageing resistance, long use period and low price.
Description
The present invention relates to a kind of water-proof material and production technique, particularly a kind of mastic neoprene water-proof paint and production technique that is used for construction work protection against the tide, anti-leakage.
As everyone knows, water-proof material is requisite a kind of important materials in the construction work, and its quality good job directly has influence on the quality of completion of works, need coated with water blocking material as roof, flooring, vault, warehouse, pond and water conservancy projects etc., reach the purpose of waterproof, protection against the tide, antiseep.What use in the prior art is traditional petroleum pitch water-proof material, exist easy embrittlement under easy trickling, the low temperature under the high temperature, play drum, be full of cracks, seepage easily, the waterproof effect instability, need carry out heat construction, problem such as labour intensity is big during construction, but cheap because of it, construction cost is low, be widely used always.The various asphalt modification water-proof materials and other water-proof materials that come next, as high-concentrated water-soluble water-proof coating (application number 90106875.6), high efficient water-proof painting material (application number 91108189.5) and waterproof paint (application number 89104899.5), these waterproof paints, it is many wherein to exist material component, the problem of processed complex, the raw material that has is toxic, the smell is awful, as triphen ethylphenol, propylene dichloride, influence the healthy of people, the raw material that has is in short supply, price is high, and as tung oil, vinylformic acid, thereby difficulty or ease are promoted the use of.
The object of the present invention is to provide a kind of have excellent protection against the tide, the mastic neoprene water-proof paint and the production technique of anti-leakage performance, overcome the deficiencies in the prior art part, it can carry out cold construction under humidity, dust atmosphere, the rete cohesive force is strong, high resilience, fast drying, no change in bubble.
Technical scheme of the present invention is as follows:
1, prescription: mastic neoprene water-proof paint, it is mixed with by 60# petroleum pitch, neoprene latex, polyvinyl alcohol (17-88), quaternary ammonium salt asphalt emulsifier TOT, filler and water, and its proportion of composing (weight ratio) is 60# petroleum pitch 53-56%, neoprene latex 4-8%, polyvinyl alcohol (17-88) 2-4%, quaternary ammonium salt asphalt emulsifier TOT0.3-0.6%, filler 1-2% and water 32-37%.
2, production technique: technology comprises the fusing of (1) petroleum pitch, to heat fusion in the petroleum pitch input fusing case, when temperature rises to 120-140 ℃, be fused into liquid, flow into then in the high-temperature cabinet (dewatering box), when containing water in the pitch, continue to be heated to 140-160 ℃, water evaporates is removed, be incubated to 120-130 ℃, rubber mill pours in the pitch hopper stand-by when starting, (2) emulsion preparation adds tap water and is heated to 100 ℃ in the hot well tank, flows into then in the stirred pot that adds polyvinyl alcohol (17-88) in advance, stirred 10-15 minute, polyvinyl alcohol all dissolves, and adds quaternary ammonium salt asphalt emulsifier TOT and filler then, continues to stir 5-10 minute to all dissolving mixing emulsification, be pressed into then in the insulation jar, be incubated 70-80 ℃, treat to be pressed in the emulsion hopper when rubber mill starts the preparation of (3) finished product, start rubber mill, rotating speed is 2900 rev/mins, opens pitch hopper and emulsion hopper, and pitch and emulsion flow in the rubber mill simultaneously and grind, fineness reaches the micron to 2-5, feed liquid after the grinding flows into the finished product pond, is cooled to 50-30 ℃, under agitation adds neoprene latex, treat to mix fully till the emulsification, the discharging can gets product.
Filler is U-Ramin MC, silicon-dioxide or water-ground limestone.
In the production process, heating system is by Oil Guide stove, header box, low level case, water-and-oil separator, strainer and carry thermal conductance oil sealing stopped pipe road to form resistant to elevated temperatures Oil Guide in the Oil Guide stove.
Fig. 1 is the technological process of production synoptic diagram of the technology of the present invention.
Below in conjunction with embodiment the present invention is specified.(table 1 is seen the literary composition back)
Operating procedure:
Pour into resistant to elevated temperatures Oil Guide in the Oil Guide stove, come high temperature oil in the process furnace by coal gas or electricity, temperature reaches 250-300 ℃, thermal conductance oil is delivered on the working face that needs heating with the high pressure transfer pump then, carry out coil pipe type and add thermal material, cooling after heat Oil Guide returns, and forms circulating pipeline and send heat.
(1) petroleum pitch fusing, take by weighing in the 60# petroleum pitch input fusing case and heat fusion, when temperature rises to 120-140 ℃, be fused into liquid, flow into then in the high-temperature cabinet (dewatering box), when containing water in the pitch, continue to be heated to 140-160 ℃, the water evaporation is removed, be incubated to 120-130 ℃, rubber mill pours in the pitch hopper stand-by when starting, (2) emulsion preparation, to be heated to 100 ℃ in the quantitative tap water adding hot well tank, flow in the stirred pot that adds quantitative polyvinyl alcohol (17-88 type) in advance then, stirred 10-15 minute, polyvinyl alcohol all dissolves, add quaternary ammonium salt asphalt emulsifier TOT and the filler that takes by weighing then, continue stirring extremely all dissolving mixing emulsification in 5-10 minute, be pressed into then in the insulation jar, be incubated 70-80 ℃, treat to be pressed into again in the emulsion hopper when rubber mill starts, (3) finished product preparation is started rubber mill, 2900 rev/mins of rotating speeds, open pitch hopper and emulsion hopper, pitch and emulsion flow in the rubber mill simultaneously and grind, and fineness reaches the 2-5 micron, under agitation add the neoprene latex that takes by weighing, till complete mixing emulsification, the discharging can gets product.
In sample test performance data such as the table 2.(table 2 is seen the literary composition back)
The present invention compared with prior art has following advantage:
1, water-repellent paint provided by the invention does not at high temperature trickle, not embrittlement under the low temperature, moistureproof anti-leakage performance excellence.
2, simple, the raw material of present technique technology is easy to get, and the industrial and commercial shop of vague generalization is on sale, and low price, cost are low, easily promote the use of.
3, adhesion strength height, the rete high resilience, corrosion-resistant, ageing-resistant, life cycle is long.
4, suitable cold construction, machine spray, artificial brushing all can.
5, technological process of production Totally-enclosed-type, safety and sanitation, the no three wastes produce.
(notes) 1, chemical plant, neoprene latex Qingdao produce
2, the 17 finger polymerization degree are that 1700,88 finger alcoholysis degrees are 88% in the polyvinyl alcohol (17-88), and Beijing Organic Chemical Plant produces.
3, quaternary ammonium salt asphalt emulsifier TOT, trade name 1831, specification are active matter content 35% aqueous solution, outward appearance is light yellow, thick liquid, low temperature is paste, and oil chemistry factory in Daliang City's produces.
Table 1
Component weight ratio % embodiment 1
60# asphalt 55 53 56 54
Polyvinyl alcohol (17-88) 3423
Quaternary ammonium salt asphalt emulsifier TOT 0.5 0.6 0.3 0.5
Filler (U-Ramin MC) (water-ground limestone) (silicon-dioxide) (U-Ramin MC)
2 2 1 2
Neoprene latex 5845
Water surplus surplus surplus surplus
Table 2
Test event result
Outward appearance black thick liquid
Solids content (%) is more than 56
Cohesive strength (Mpa) Eight characters modulus method is more than 16.9
Viscosity (Cp)>850
Low temperature flexibility-30 ℃ does not split
110 ℃ of thermotolerances are non-foaming, do not trickle
Extensibility (M/N) 16.4
Frost resistance+20 ℃ water logging 24 hours
Not crack initiation, embrittlement not
-20 ℃ 24 hours
One cloth two is coated with, and two cloth four are coated with (kg/cm)
Upstream face anti-leakage pressure 18,21
Be lower than international standard more than hundred times by 8 of national Drinking Water matter standards
10 oxious component chemical examinations
500W
45 ℃ of waterproof layer no changes of ultraviolet ray
240 hours
Claims (3)
1, a kind of mastic neoprene water-proof paint, its feature exists, be mixed with by 60# petroleum pitch, neoprene latex, polyvinyl alcohol (17-88), quaternary ammonium salt asphalt emulsifier TOT, filler and water in it, its proportion of composing (weight ratio) is: 60# petroleum pitch 53-56%, neoprene latex 4-8%, polyvinyl alcohol (17-88) 2-4%, quaternary ammonium salt asphalt emulsifier TOT0.3-0.6%, filler 1-2% and water 32-37%.
2, waterproof paint according to claim 1 is characterized in that, filler is U-Ramin MC, silicon-dioxide or water-ground limestone.
3, the production technique of the described waterproof paint of a kind of claim 1, it is characterized in that technology comprises: the fusing of (1) petroleum pitch, to heat fusion in the petroleum pitch input fusing case, when temperature rises to 120-140 ℃, be fused into liquid, flow into then in the high-temperature cabinet (dewatering box), when containing water in the pitch, continue to be heated to 140-160 ℃, water evaporates is removed, be incubated to 120-130 ℃, pour in the pitch hopper stand-by when rubber mill starts, (2) emulsion preparation, tap water added be heated to 100 ℃ in the hot well tank, flow into then and add in the polyvinyl alcohol stirred pot in advance, stirring/10-15 minute, polyvinyl alcohol all dissolves, add quaternary ammonium salt asphalt emulsifier TOT and filler then, continue to stir 5-10 minute to all dissolving mixing emulsification, be pressed into then in the insulation jar, be incubated 70-80 ℃, treat to be pressed in the emulsion hopper when rubber mill starts, (3) finished product preparation, start rubber mill, rotating speed is 2900 rev/mins, opens pitch hopper and emulsion hopper, pitch and emulsion flow in the rubber mill simultaneously and grind, fineness reaches the 2-5 micron, feed liquid after the grinding flows into the finished product pond, is cooled to 50-30 ℃, under agitation adds neoprene latex, treat to mix fully till the emulsification, the discharging can gets product.