CN102876132B - 一种紫外光固化的喷墨油墨组合物及其制备方法 - Google Patents

一种紫外光固化的喷墨油墨组合物及其制备方法 Download PDF

Info

Publication number
CN102876132B
CN102876132B CN201210384307.7A CN201210384307A CN102876132B CN 102876132 B CN102876132 B CN 102876132B CN 201210384307 A CN201210384307 A CN 201210384307A CN 102876132 B CN102876132 B CN 102876132B
Authority
CN
China
Prior art keywords
ultraviolet
ink composition
ultraviolet light
preparation
inkjet ink
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201210384307.7A
Other languages
English (en)
Other versions
CN102876132A (zh
Inventor
高延敏
代仕梅
杜才刚
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Zhenjiang Hengchang Color Technology Co. Ltd.
Original Assignee
Jiangsu University of Science and Technology
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Jiangsu University of Science and Technology filed Critical Jiangsu University of Science and Technology
Priority to CN201210384307.7A priority Critical patent/CN102876132B/zh
Publication of CN102876132A publication Critical patent/CN102876132A/zh
Application granted granted Critical
Publication of CN102876132B publication Critical patent/CN102876132B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种紫外光固化的喷墨油墨组合物,它包含如下重量百分比的组分:1,6-己二醇二丙烯酸酯15~45%;丙烯酸羟乙酯10~20%;异冰片丙烯酸酯20~40%;紫外光促进剂1~10%;光引发剂11735%;三苯胺1~10%。本发明还公开了上述紫外光固化的喷墨油墨组合物的制备方法。本发明的紫外光固化的喷墨油墨组合物与现有技术相比,具有的优势如下:附着力1级;固化时间为10~25秒;漆膜的机械强度好,按照GB/T 17200标准进行测试,漆膜拉伸强度为50~80N。

Description

一种紫外光固化的喷墨油墨组合物及其制备方法
技术领域
本发明属于油墨领域,涉及一种紫外光固化的喷墨油墨组合物及其制备方法。
背景技术
近年来,随着现代计算机软硬件技术、电子技术、彩色数字图像技术、物理光学技术等科技成果的发展,计算机直接制版技术(CTP),简化了复杂的制版工艺过程,减少了制版中胶片输出、显影、定影和晒版等中间环节,也减少了含银,对苯二酚等对人体和环境危害较大的废液排放及制版过程中紫外光对人体的伤害和对空气的污染,与这种技术配合的就是印刷油墨技术的进步。
传统意义上的印刷流程是个技术含量相当复杂和繁琐的过程,而且对印刷品的幅面、材质有着严格的限制和要求,短版印刷、快速印刷和印刷试销的成本也居高不下。数字出现,简化了印刷过程,数字技术无论是图像制作的精度和色彩,还是制作成本和工艺,以及短版印刷、快速印刷、季节性促销品的制作,数字化的无版印刷技术在印刷领域发挥着独特的优势。
采用最先进的APR数字喷头技术和配合印刷油墨,可以直接将文字,图案在材料上进行印刷,使生产过程更加简便,色彩更加艳丽和真实,图像更加清晰,使得包装印刷向大幅面、小批量、高产出、个性化发展。
在数字化印刷过程中,油墨好坏,直接影响了印刷效果,目前,所使用的油墨,尚存在固化速度慢,附着力差的缺陷。
UV固化喷墨油墨是一种粘度极低的材料,粘度过高,容易出现塞孔的现象,因此,其所使用的材料一般为单体,然而,单体在极短的时间内固化,所形成的聚合物膜,分子量都不高,影响了印刷品的质量,因此,需要在极短的时间内,形成大分子量的物质。
发明内容
本发明所要解决的技术问题,是提供一种紫外光固化的喷墨油墨组合物。
本发明还要解决的技术问题,是提供上述组合物的制备方法。
为解决上述技术问题,本发明采用的技术方案如下:
一种紫外光固化的喷墨油墨组合物,它包含如下重量百分比的组分:
其中,所述的紫外光促进剂,结构式如下:
上述紫外光促进剂按如下方法制备得到:将对二苯胺与丙烯酸酰氯反应而得到的产物,在反应投料的摩尔比为1:2.2,反应温度为80℃,反应的时间为9小时,反应所用的催化剂为三苯胺,催化剂用量为二苯胺和丙烯酰氯总质量的1%。
上述紫外光固化的喷墨油墨组合物的制备方法,将配方量的1,6-己二醇二丙烯酸酯、丙烯酸羟乙酯、异冰片丙烯酸酯、紫外光促进剂和光引发剂1173在避光下,搅拌混匀,即得。
上述紫外光固化的喷墨油墨组合物的使用方法,印刷的方法是喷涂的,紫外光固化,固化的能量为80-100mj/cm2
有益的效果:本发明的紫外光固化的喷墨油墨组合物与现有技术相比,具有的优势如下:
1.附着力1级;
2.固化时间为10~25秒。
3.漆膜的机械强度好,按照GB/T17200标准进行测试,漆膜拉伸强度为50~80N。
具体实施方式
根据下述实施例,可以更好地理解本发明。然而,本领域的技术人员容易理解,实施例所描述的内容仅用于说明本发明,而不应当也不会限制权利要求书中所详细描述的本发明。
以下实施例所用的紫外光促进剂,结构式如下:
紫外光促进剂的具体制备方法:将对二苯胺与丙烯酸酰氯反应而得到的产物,在反应投料的摩尔比为1:2.2,反应温度为80℃,反应的时间为9小时,反应所用的催化剂为三苯胺,催化剂用量为二苯胺和丙烯酰氯总质量的1%。
实施例1:
一种紫外光固化的喷墨油墨组合物,它包含如下重量百分比的组分:
制备方法:将配方量的1,6-己二醇二丙烯酸酯、丙烯酸羟乙酯、异冰片丙烯酸酯、紫外光促进剂和光引发剂1173在避光下,搅拌混匀,即得。
效果:
●附着力1级。
●固化时间为25秒。
●漆膜的机械强度好,按照GB/T17200标准进行测试,漆膜拉伸强度为50N。
实施例2:
一种紫外光固化的喷墨油墨组合物,它包含如下重量百分比的组分:
制备方法:将配方量的1,6-己二醇二丙烯酸酯、丙烯酸羟乙酯、异冰片丙烯酸酯、紫外光促进剂和光引发剂1173在避光下,搅拌混匀,即得。
效果:
●附着力2级。
●固化时间为10秒。
●漆膜的机械强度好,按照GB/T17200标准进行测试,漆膜拉伸强度为55N。
实施例3:
一种紫外光固化的喷墨油墨组合物,它包含如下重量百分比的组分:
制备方法:将配方量的1,6-己二醇二丙烯酸酯、丙烯酸羟乙酯、异冰片丙烯酸酯、紫外光促进剂和光引发剂1173在避光下,搅拌混匀,即得。
效果:
●附着力1级。
●固化时间为15秒。
●漆膜的机械强度好,按照GB/T17200标准进行测试,漆膜拉伸强度为80N。
实施例4:
一种紫外光固化的喷墨油墨组合物,它包含如下重量百分比的组分:
制备方法:将配方量的1,6-己二醇二丙烯酸酯、丙烯酸羟乙酯、异冰片丙烯酸酯、紫外光促进剂和光引发剂1173在避光下,搅拌混匀,即得。
效果:
●附着力1级。
●固化时间为25秒。
●漆膜的机械强度好,按照GB/T17200标准进行测试,漆膜拉伸强度为60N。
实施例5:
一种紫外光固化的喷墨油墨组合物,它包含如下重量百分比的组分:
制备方法:将配方量的1,6-己二醇二丙烯酸酯、丙烯酸羟乙酯、异冰片丙烯酸酯、紫外光促进剂和光引发剂1173在避光下,搅拌混匀,即得。
效果:
●附着力1级。
●固化时间为30秒。
●漆膜的机械强度好,按照GB/T17200标准进行测试,漆膜拉伸强度为75N。

Claims (3)

1.一种紫外光固化的喷墨油墨组合物,其特征在于,它包含如下重量百分比的组分:
所述的紫外光促进剂,结构式如下:
2.根据权利要求1所述的紫外光固化的喷墨油墨组合物,其特征在于,所述的紫外光促进剂按如下方法制备得到:将对苯二胺与丙烯酰氯反应而得到的产物,在反应投料的摩尔比为1:2.2,反应温度为80℃,反应的时间为9小时,反应所用的催化剂为三苯胺,催化剂用量为苯二胺和丙烯酰氯总质量的1%。
3.权利要求1所述的紫外光固化的喷墨油墨组合物的使用方法,其特征在于,印刷的方法是喷涂的,紫外光固化,固化的能量为80-100mJ/cm2
CN201210384307.7A 2012-10-11 2012-10-11 一种紫外光固化的喷墨油墨组合物及其制备方法 Active CN102876132B (zh)