CN102371206B - 一种处理含碳铅锌多金属复杂硫化矿的工艺 - Google Patents

一种处理含碳铅锌多金属复杂硫化矿的工艺 Download PDF

Info

Publication number
CN102371206B
CN102371206B CN 201010258035 CN201010258035A CN102371206B CN 102371206 B CN102371206 B CN 102371206B CN 201010258035 CN201010258035 CN 201010258035 CN 201010258035 A CN201010258035 A CN 201010258035A CN 102371206 B CN102371206 B CN 102371206B
Authority
CN
China
Prior art keywords
zinc
concentrate
lead
flotation
metal complex
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN 201010258035
Other languages
English (en)
Other versions
CN102371206A (zh
Inventor
宋永胜
李文娟
周桂英
屈伟
刘爽
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
GRINM Resources and Environment Technology Co Ltd
Original Assignee
Beijing General Research Institute for Non Ferrous Metals
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Beijing General Research Institute for Non Ferrous Metals filed Critical Beijing General Research Institute for Non Ferrous Metals
Priority to CN 201010258035 priority Critical patent/CN102371206B/zh
Publication of CN102371206A publication Critical patent/CN102371206A/zh
Application granted granted Critical
Publication of CN102371206B publication Critical patent/CN102371206B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明涉及一种处理含碳铅锌多金属复杂硫化矿的工艺。该工艺采用浮选-重选联合流程处理含碳铅锌多金属复杂硫化矿,即将原矿磨至一定粒度,先利用浮选法得到含碳铅锌混合精矿,然后再利用比重差采用重选法将浮选混合精矿进行分选,重选前脱药,然后先将比重比较大的铅回收,得到合格的铅精矿,重选中矿为锌精矿,重选尾矿碳。利用该工艺设备简单,得到很高的技术指标,可为企业带来很好的经济效益。

Description

一种处理含碳铅锌多金属复杂硫化矿的工艺
技术领域
本发明涉及一种处理含碳铅锌多金属复杂硫化矿的工艺。本发明所指的铅锌是指方铅矿和易浮闪锌矿。
背景技术
含有方铅矿和易浮闪锌矿的多金属硫化矿的分离非常困难,国内外分选这类矿石常采用优先浮选方铅矿再选闪锌矿的工艺,个别极易难选的矿石直接混选得到铅、锌混合精矿,但混合精矿比单独的精矿经济效益差。当矿石中存在碳时,矿石的分选就更加困难,得到的精矿很难达到冶炼的要求。
在现有含碳多金属硫化矿的处理工艺中,也有的采用煤油等弱捕收剂先将碳浮选脱除,再进行其它矿物分选。该法的弱点是在浮碳时,不可避免地要损失有价金属。
本发明提供一种处理含碳铅锌多金属复杂硫化矿的工艺,采用浮选-重选联合工艺,充分回收该矿种的有价元素。
发明内容
本发明的目的是提供一种处理含碳铅锌多金属复杂硫化矿的工艺,利用该工艺可得到合格的铅精矿和锌精矿,且操作简单。
本发明的目的可以通过以下措施来实现:
该工艺的特点是利用浮选-重选联合流程处理含碳的铅锌多金属复杂硫化矿,即将原矿磨至一定粒度,先利用浮选法得到含碳的铅锌混合精矿,然后再利用方铅矿、闪锌矿和碳的比重差采用重选法将浮选混合精矿进行分选。重选前对混合精矿脱药,将比重比较大的方铅矿回收,得到合格的铅精矿,中矿为锌精矿,尾矿为碳。
(1)采用浮选得到含碳的铅锌混合精矿;
(2)浮选入选粒度为-74μm60-90%;
(3)浮选矿浆浓度为25-30%;
(4)浮选药剂为O-异丙基-N-乙基硫逐氨基甲酸酯、黄原酸钠、二乙氨基二硫代甲酸钠、二丁基二硫代磷酸铵或其中两种配合使用(配比为1∶1),
药剂用量为30-75g/t,时间为12-15分钟;
(5)利用重选将浮选混合精矿进行分选;
(6)重选前脱药,脱药搅拌时间为20-35min;
(7)重选的矿浆调浆浓度为10-15%;
(8)、重选精矿为铅精矿,重选中矿为锌精矿,重选尾矿为碳。
本发明的优点是:利用该工艺设备简单,得到很高的技术指标,可为企业带来很好的经济效益。
附图说明
图1为本发明提供的处理含碳铅锌多金属复杂硫化矿的工艺流程示意图。
图2为采用传统优先选铅再选锌工艺的流程示意图,用于与本发明对比。
图3为采用先用煤油浮选脱碳、再选铅锌工艺的流程示意图,用于与本发明对比。
具体实施方式
实施例1
某含碳铅锌多金属复杂硫化矿,矿石是以有用矿物方铅矿和闪锌矿为主的矿石。除有益元素构成的这些有用矿物外,矿石中还存在有大量的脉石矿物石英、长石和粘土矿物等。
矿石中铅含量为3.5%,锌2.8%,含碳为3%。
利用本发明方法,即将原矿磨至-74μm65%,利用O-异丙基-N-乙基硫逐氨基甲酸酯+乙基黄原酸钠(配比为1∶1)进行浮选,药剂总用量为55g/t,浮选矿浆浓度为30%,混合浮选的浮选时间为14分钟,得到的混合精矿利用摇床进行重选,重选前脱药搅拌25分钟,重选浓度为15%。重选精矿为铅精矿,重选中矿为锌精矿,重选摇床尾矿为碳。见图1,试验结果见表1。
采用传统优先选铅再选锌工艺,见图2,磨矿细度为-74μm 65%,实验结果见表1,用于与本发明对比。
采用传统先用煤油浮选脱碳、再选铅锌工艺流程,见图3,磨矿细度为-74μm 65%,实验结果见表1,用于与本发明对比。
实施例2
矿石来源同实施例1。
利用本发明方法,即将原矿磨至-74μm70%,利用O-异丙基-N-乙基硫逐氨基甲酸酯进行浮选,药剂用量为55g/t,浮选矿浆浓度为25%,混合浮选的浮选时间为14分钟,得到的混合精矿利用摇床进行重选,重选前脱药搅拌20分钟,重选浓度为10%。重选精矿为铅精矿,重选中矿为锌精矿,重选摇床尾矿为碳。试验结果见表1。
表1不同工艺结果
从表1可以看出,无论是实施例1还是实施例2,利用本发明提供的工艺可以得到达到冶炼要求的铅精矿和锌精矿,且两种矿物的回收率均很高。
采用传统优先选铅再选锌工艺,得不到合格的铅精矿且锌精矿的回收率非常低。
采用传统先浮选脱碳、再选铅锌工艺流程,碳中损失了大量的有价金属,且得不到合格的铅精矿,锌精矿的回收率也极低。
从上面的分析可知,利用本发明提供的浮选-重选联合流程处理含碳的铅锌复杂多金属硫化矿具有明显的优越性。

Claims (3)

1.一种处理含碳铅锌多金属复杂硫化矿的工艺,其特征在于,它是利用浮选-重选联合工艺流程处理含碳的铅锌多金属复杂硫化矿,原矿中铅锌矿是指方铅矿和易浮闪锌矿,其包括:
将原矿磨至-74μm占60-90%,先利用浮选法得到含碳的铅锌混合精矿;
然后再利用方铅矿、闪锌矿和碳的比重差采用重选法将浮选法得到含碳的铅锌混合精矿进行分选;
重选前对混合精矿脱药,将比重比较大的方铅矿回收,得到合格的铅精矿,中矿为锌精矿,尾矿为碳。
2.根据权利要求1所述的一种处理含碳铅锌多金属复杂硫化矿的工艺,其特征在于,所述的浮选是:
(1)浮选入选粒度为-74μm占60-90%;
(2)浮选矿浆浓度为25-30%(重量百分比);
(3)浮选药剂为0-异丙基-N-乙基硫逐氨基甲酸酯、黄原酸钠、二乙氨基二硫代甲酸钠或二丁基二硫代磷酸铵中的一种,或其中两种以重量比1∶1配合使用,药剂用量为30-75g/t,时间为12-15分钟。
3.根据权利要求1或2所述的一种处理含碳铅锌多金属复杂硫化矿的工艺,其特征在于,所述的重选是:
(1)重选所用的设备为摇床或螺旋溜槽;
(2)重选的矿浆调浆浓度为10-15%(重量百分比);
(3)重选精矿为铅精矿,重选中矿为锌精矿,重选尾矿为碳。
CN 201010258035 2010-08-19 2010-08-19 一种处理含碳铅锌多金属复杂硫化矿的工艺 Expired - Fee Related CN102371206B (zh)