CN102191119A - 润滑脱模剂及其制备方法 - Google Patents

润滑脱模剂及其制备方法 Download PDF

Info

Publication number
CN102191119A
CN102191119A CN2011100967497A CN201110096749A CN102191119A CN 102191119 A CN102191119 A CN 102191119A CN 2011100967497 A CN2011100967497 A CN 2011100967497A CN 201110096749 A CN201110096749 A CN 201110096749A CN 102191119 A CN102191119 A CN 102191119A
Authority
CN
China
Prior art keywords
releasing agent
release agent
preparation
lubricant
casting
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN2011100967497A
Other languages
English (en)
Other versions
CN102191119B (zh
Inventor
孙兰凤
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Tianjin Zhongchuan lubrication Polytron Technologies Inc
Original Assignee
TIANJIN ANLOOP ENVIRONMENTAL PROTECTION TECHNOLOGY DEVELOPMENT Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by TIANJIN ANLOOP ENVIRONMENTAL PROTECTION TECHNOLOGY DEVELOPMENT Co Ltd filed Critical TIANJIN ANLOOP ENVIRONMENTAL PROTECTION TECHNOLOGY DEVELOPMENT Co Ltd
Priority to CN 201110096749 priority Critical patent/CN102191119B/zh
Publication of CN102191119A publication Critical patent/CN102191119A/zh
Application granted granted Critical
Publication of CN102191119B publication Critical patent/CN102191119B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明涉及一种润滑脱模剂及其制备方法,其组成成分为:增粘剂20-30%、分散剂5-6%、溶剂40-70%、有机膨润土0.1-1%、胶体石墨2-7%,制备方法为:依次混合后即得润滑脱模剂。本发明制备的润滑脱模剂主要用于钢水浇铸中的脱模润滑剂,本脱模剂能降低铸件表面粗糙度,有效地防止铸件粘砂、夹砂、砂眼等缺陷,具有提高铸件表面光洁度和模具清理简单方便的效果。

Description

润滑脱模剂及其制备方法
技术领域
本发明属于润滑油领域,尤其是一种润滑脱模剂及其制备方法。
背景技术
脱模剂应当具有较大的抗拉强度,使它在与模压树脂经常接触时不容易磨光,特别是在树脂中有磨砂矿物填料或玻璃纤维增强料时尤其如此。脱模剂具有耐化学性,以便在与不同树脂的化学成份(特别是苯乙烯和胺类)接触时不被溶解。脱模剂还应具有耐热及应力性能,不易分解或磨损,脱模剂应粘合到模具上而不转移到被加工的制件上,以便不妨碍喷漆或其他二次加工操作。
脱模剂化学原理
1.极性化学键与模具表面通过相互作用形成具有再生力的吸附型薄膜;
2.聚硅氧烷中的硅氧键可视为弱偶极子(Si+-O-),当脱模剂在模具表面铺展成单子取向排列时,分子采取特有的伸展链构型;
3.自由表面被烷基以密集堆积方式覆盖,脱模能力随烷基密度而递增;但当烷占有较大空间位阻时,伸展构型受到限制,脱模能力又会降低;
4.脱模剂分子量大小和粘度也与脱模能力相关,分子量小时,铺展性好,但耐热能力差。
常用的脱模剂有无机物、有机物以及高聚物三类。
无机脱模剂,如滑石粉、云母粉以及陶土、白粘土等为主要组分配置的复合物,主要用作橡胶加工中胶片、半成品防粘用隔离剂。
有机脱模剂包括脂肪酸皂(钾皂、钠皂、铵皂、锌皂等)、脂肪酸、石蜡、甘油、凡士林等。
第三类高聚物脱模剂是高聚物,包括硅油、聚乙二醇、低分子量聚乙烯等,它们的脱模剂效率和热稳定性比有机物脱模剂好得多。
脱模剂通常有粉状、半固体和液体之分,粉状和半固体可像蜡脂一样用毛刷或手涂于模具表面。液体可用喷雾或毛刷等工具涂于模具表面,从而形成隔离膜。液体脱模剂以喷涂为佳。
国际工业发达国家多采用金属喷雾罐灌装的脱模剂,由于金属喷雾罐密封性能较好,可避免脱模剂氧化或混入杂质,能保证脱模剂出厂时的纯洁性,大型的注塑设备安装在室内,环境温度变化小,对喷雾脱模剂的使用无影响,但对模压成形的模具温度要予以考虑,要选热稳定性能好的脱模剂,一般要求脱模剂的热分解温度要高于成型的模具温度,不然会发生炭化结诟现象。高档制品和需要二次加工(如喷漆和印刷)要选用适合于二次加工的脱模剂。为防止环境污染,要选用不易燃烧,气味和毒性小的脱模剂。在脱模剂选用中,经济性是不可忽视的重要因素,质量差的脱模剂会使产品表面产生龟裂皱纹,影响产品外观和模具使用寿命,并带来环境污染。选择高质量的喷雾脱模剂,价格较高,但综合经济效益高。
发明内容
本发明的目的在于克服现有技术的不足之处,提供一种能降低铸件表面粗糙度、提高铸件表面光洁度的润滑脱模剂及其制备方法。
本发明是通过以下技术方案实现目的的:
一种润滑脱模剂,其组成成分及重量百分比如下:
Figure BDA0000055914650000021
而且,所述增粘剂为:(-CH2-CH2-)m-(-CH2-CH(CH3)-)n
而且,所述分散剂为:
Figure BDA0000055914650000022
而且,所述溶剂为异构烷烃。
一种润滑脱模剂的方法,制备方法的步骤如下:
(1)投入溶剂、增粘剂,缓慢搅拌升温到50-70℃,恒温30-40分钟;
(2)依次加入有机膨润土升温到40℃搅拌均匀,在40-60℃恒温30-40分钟;
(3)投入胶体石墨搅拌混合,30-45分钟,即制备出润滑脱模剂。
本发明的优点和有益效果为:
1、本发明制备的润滑脱模剂主要用于钢水浇铸中的脱模润滑剂,本脱模剂能降低铸件表面粗糙度,有效地防止铸件粘砂、夹砂、砂眼等缺陷,具有提高铸件表面光洁度和模具清理简单方便的效果。
2、本发明提供的脱模剂具有耐热性,受热不发生炭化分解,化学性能稳定,不与成型产品发生化学反应,不影响塑料的二次加工性能。
3、本脱模剂不腐蚀模具,不污染制品,气味和毒性小;外观光滑美观、易涂布,生产效率高。
具体实施方式
下面结合实施例,对本发明进一步说明,下述实施例是说明性的,不是限定性的,不能以下述实施例来限定本发明的保护范围。
本发明中润滑脱模剂润滑剂的组成及重量百分比为:
Figure BDA0000055914650000023
Figure BDA0000055914650000031
溶剂的首选是异构烷烃溶剂,而在异构烷烃溶剂中选择美孚\ISOPAR L的效果较好,其他常用溶剂稀释剂参考如下:1、二氯甲烷:CH2Cl2、沸点39.75、相对密度1.326、闪点无,表面张力28.12mN/m,化学稳定,290度不氧化或裂解,溶解能力强,不燃烧;高浓度蒸汽引起中毒,引起温室效应。2、石油醚:是石油的低沸点馏分,为低级烷烃混合物,按沸点不同分为30-60℃,60-90℃,90-120℃三类,沸点低,挥发性高,毒性与低级烷烃相似。3、120#汽油:C4-C11的烷烃、烯烃、环烷烃和芳香烃组成的混合物,主要成分为戊烷、己烷、庚烷、辛烷组成,挥发性大,刺激性气味,大量吸入影响神经。4、石脑油:煤焦油轻油馏分所得芳香族烃类混合物,沸点120-200℃,由甲苯、乙苯等组成,避火,影响神经。5、庚烷:C7H16,沸点98.4℃,化学稳定,闪点-4℃,表面张力19.6mN/m,低毒性。6、二甲苯:C8H10,异构体,馏程140℃左右,密度0.86左右,高闪点易燃,低毒,对皮肤有影响。
实施例1
一种润滑脱模剂,组成成分及重量百分比如下:
Figure BDA0000055914650000032
一种润滑脱模剂的制备方法,步骤如下:
(1)投入增粘剂,缓慢搅拌升温到60℃,恒温30-40分钟;
(2)依次加入分散剂、有机膨润土混合剂,在50℃恒温30-40分钟;
(3)投入胶体石墨混合液30-45分钟,即制备出润滑脱模剂。
其中:增粘剂为
Figure BDA0000055914650000033
m为7到9之间,n为5-7之间。
分散剂为:
Figure BDA0000055914650000034
n为5-7之间。
溶剂为:异构烷烃主要是C8~C14异构烷烃,常用于润滑剂。
主要技术指标:
  性能   指标
  密度g/cm3(%)≤   1.4
  悬浮性24h(%)≥   98
  发气量ml/g≤   14
  高温抗开裂级<   1
  石墨含量≮   35

Claims (5)

1.一种润滑脱模剂,其特征在于:其组成成分及重量百分比如下:
Figure FDA0000055914640000011
2.根据权利要求1所述的润滑脱模剂,其特征在于:所述增粘剂为:(-CH2-CH2-)m-(-CH2-CH(CH3)-)n
3.根据权利要求1所述的润滑脱模剂,其特征在于:所述分散剂为:
4.根据权利要求1所述的润滑脱模剂,其特征在于:所述溶剂为异构烷烃。
5.一种制备如权利要求1所述的润滑脱模剂的方法,其特征在于:制备方法的步骤如下:
(1)投入溶剂、增粘剂,缓慢搅拌升温到50-70℃,恒温30-40分钟;
(2)依次加入有机膨润土升温到40℃搅拌均匀,在40-60℃恒温30-40分钟;
(3)投入胶体石墨搅拌混合,30-45分钟,即制备出润滑脱模剂。
CN 201110096749 2011-04-18 2011-04-18 润滑脱模剂及其制备方法 Expired - Fee Related CN102191119B (zh)