CN102134772B - Positioning strip leisure fabric and production process thereof - Google Patents

Positioning strip leisure fabric and production process thereof Download PDF

Info

Publication number
CN102134772B
CN102134772B CN201110071730.7A CN201110071730A CN102134772B CN 102134772 B CN102134772 B CN 102134772B CN 201110071730 A CN201110071730 A CN 201110071730A CN 102134772 B CN102134772 B CN 102134772B
Authority
CN
China
Prior art keywords
raw material
yarn
yarns
dyeing
positioning strip
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN201110071730.7A
Other languages
Chinese (zh)
Other versions
CN102134772A (en
Inventor
胡平友
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
SHAOXING YUEFA TEXTILE CO Ltd
Original Assignee
SHAOXING YUEFA TEXTILE CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by SHAOXING YUEFA TEXTILE CO Ltd filed Critical SHAOXING YUEFA TEXTILE CO Ltd
Priority to CN201110071730.7A priority Critical patent/CN102134772B/en
Publication of CN102134772A publication Critical patent/CN102134772A/en
Application granted granted Critical
Publication of CN102134772B publication Critical patent/CN102134772B/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention provides a positioning strip leisure fabric and a production process thereof, and belongs to the technical field of textile fabrics. The positioning strip leisure fabric comprises a fabric body part and a positioning strip part, wherein the warp yarns of the fabric body part are prepared from a raw material A, a raw material B and a raw material C; the raw material A is low-temperature cationic viscose yarns; the raw material B is super-bright proportional color slub yarns; the raw material C is deep navy blue yarns and deep sapphire blue yarns; the warp yarns of the positioning strip part are prepared from a raw material D and a raw material E; the raw material D is reddish brown network yarns, multi-color metallic network yarns and wine red yarns; the raw material E is sky blue network yarns, multi-color metallic network yarns and deep navy blue yarns; the weft yarns of the fabric body part are prepared from a raw material F and a raw material G; the raw material F is low-temperature cationic viscose yarns; the raw material G is bright draw textured yarns (DTY) and super-bright proportional color slub yarns; and the weft yarns of the positioning strip part are prepared from the same raw materials as the weft yarns of the fabric body part. The positioning strip leisure fabric has soft handfeel, strong hair feel, a unique style and high quality.

Description

Positioning strip leisure fabric
Technical field
The invention provides a kind of positioning strip leisure fabric and production technology thereof, belong to weaving face fabric technical field.
Background technology
Along with scientific and technological development and living standard improve, people require more to pay close attention to fabric comfortableness, Overseas Textile Industry market is also more and more high to the requirement of textiles, and weaving face fabric is progressively to superior, leisureization future development, and the leisure fabric that floridity is comfortable will become the fashion of society.The coming five years, the general trend of textile product development be ecology, fashion, comfortable, healthy, functional, be conducive to environmental protection, and environment harmonious development; The direction of carry out have no water or little water processing, strengthening resource circulation utilization, adhere to sustainable development; Apply raw material and the high-tech means of various diversification combination tencel materials and environmental protection type dye auxiliary agent, carry out autonomous innovation, implement " Scientific Outlook on Development ", " taking a new road to industrialization ", realize structural adjustment and the industrial upgrading of textile industry.Therefore develop properties and international fashion of synchronizeing, comfortable, healthy, functional product and be the directive selecting properly of city's textile industry tool now.
Summary of the invention
The invention provides a kind of soft, the feel of wool strong, unique style and high-quality positioning strip leisure fabric and production technology thereof.
For achieving the above object, the technical solution adopted in the present invention is:
A kind of positioning strip leisure fabric, comprises body part and positioning strip part, and the warp thread of described body part adopts A raw material, B raw material, C raw material; Wherein A raw material is the sticky yarn of 14.7tex × 2 low temperature sun, B raw material be 14.7tex × 2 superbright light positive than color yarn slub yarn, C raw material is that radical is than the dark purplish blue look silk of 100D/36F, the dark royalblue silk of 100D/36F for 1:1; The warp thread of positioning strip part adopts D raw material, E raw material; Wherein D raw material is the reddish brown network yarn of 100D/36F, 100D illusion-colour paillette network yarn, the red silk of 150D/48F nine that radical ratio is 1:1:1, and E raw material is that radical is than the sky blue network yarn of 100D/36F, 100D illusion-colour paillette network yarn, the dark purplish blue look silk of 150D/48F that are 1:1:1; The weft yarn of body part adopts F raw material, G raw material, and wherein F raw material is the sticky yarn of 14.7tex × 2 low temperature sun, and G raw material is that radical is than having light DIY, 18.5tex superbright light positive than color yarn slub yarn for the 108D/36F of 1:1; The weft yarn raw material of positioning strip part is identical with the weft yarn raw material of body part.
The sticky yarn of described low temperature sun is made up of low temperature CATION DTY, triangle profile CATION DTY, fine denier viscose, and between low temperature CATION DTY, triangle profile CATION DTY, fine denier viscose, blending ratio when dry weight is 45%:20%:35%.
Described body part adopts 2/2 twill-weave, and positioning strip part adopts figured texture weave.
A production technology for positioning strip leisure fabric, comprises the following steps,
(1) warp thread → winder → double twisting → sizing → warping → gait → denting;
(2) weft yarn → winder → double twisting → sizing → rewinding;
(3) each the warp thread after above-mentioned manufacturing procedure raw material is woven into grey cloth together with the each raw material of weft yarn;
(4) grey cloth check → blank cloth coiling → kiering → pre-setting → dyeing and finishing → calendering → filling steaming → check → clot;
In two steps, first, with cation dyes, disperse dye one-bath dyeing, dyeing temperature is 120-130 ℃, then uses REACTIVE DYES two-bath dyeing in dyeing in described dyeing and finishing process;
Stentering forming in dyeing and finishing process, temperature is 150-165 ℃, and the sizing speed of a motor vehicle is 45-55 m/min.
In two steps, first, with cation dyes, disperse dye one-bath dyeing, dyeing temperature is 125 ℃, then uses REACTIVE DYES two-bath dyeing in dyeing in described dyeing and finishing process;
Stentering forming in dyeing and finishing process, temperature is 160 ℃, and the sizing speed of a motor vehicle is 50 ms/min.
In described dyeing and finishing process, before dyeing, adopt soda ash and enzyme to carry out rear arrangement to grey cloth, to be wherein used for regulating pH value be 7-9 to soda ash; The temperature of rear arrangement is 60-80 ℃, and the time is 30 minutes; Enzyme is any one or the multiple mixture in amylase, composite fibre enzyme, protease, esterase.Grey cloth adds in order to remove preceding working procedure the component that produce or add man-hour before dyeing, as slurry, and wax, iron rust etc., these components can have a strong impact on the dyeing processing of postorder, therefore will carry out soft soda ash and enzyme processing.
When described REACTIVE DYES dyes, be used in conjunction with salt-free dyeing crosslinking agent.In order to reduce water and other auxiliary agent use amount, in reactive dyeing, use salt-free dyeing crosslinking agent.In dyeing course, crosslinking agent and dyestuff and fiber form crosslinked covalent bond, to improve utilization rate and the dyefastness of dyestuff.Traditional crosslinking agent is to contain benzaldehyde compound, containing noxious material, seldom uses at present.Salt-free dyeing crosslinking agent mainly contains active vinyl-compound, polyisocyanates, Cyanuric Chloride and derivative thereof.
Described weaving process, upper gate width is 180 centimetres; Body part adopts 2/2 twill-weave, and positioning strip part adopts figured texture weave.
C raw material in described warp thread, the twist between its each component when double twisting is 6T/cmS; D raw material in warp thread, the twist between its each component when double twisting is 6T/cmS; E raw material in warp thread, the twist between its each component when double twisting is 6T/cmS; G raw material in weft yarn, the twist between its each component when double twisting is 6T/cmS.
The present invention has adopted novel sun to glue yarn (containing low temperature, the section of triangle profile CATION), superbright light positive than color yarn ring, plurality of color silk, the plurality of raw materials combinations such as paillette silk, add figured texture weave, form the novel unique positioning strip product of style, be aided with the improvement of weaving with dyeing and printing process, form soft, the feel of wool is strong, the distinguished Novel leisure fabric of flower type.Product is applicable to making single-piece Western-style clothes, suit fabric, has very high market acceptance, and market prospects are wide.
The present invention has improved scientific and technological content and the economic value added of product greatly, and then greatly improves woven quality and class.
Adopt feel, comfortableness, gas permeability and the woven complexity of suitable thread count to cloth cover most important.The present invention has adopted the raw material of medium-coarse, larger thread count: finished product, through 326/10 centimetres of close 432/10 centimetres, finished product filling density, has reached soft, the effect that resilience is good.
Positioning strip of the present invention is apart from selvedge 16-20 centimetre, and the width of positioning strip is 5-8 centimetre, and the colored type of positioning strip is different from body weavy grain.Cloth is as dull and stereotyped or comparatively succinct dark fringe, and location barriness type is obviously outstanding, and weavy grain is slightly rough.
The key technical indexes of positioning strip leisure fabric of the present invention is as follows:
Color fastness to water (variable color, staining) >=3-4 level;
Acid and alkali resistance PERSPIRATION COLOR FASTNESS: variable color >=4 grade, staining >=3-4 level;
Colour fastness to rubbing: unlubricated friction >=4 grade, wet rubbing >=3 grades;
Washing size changing rate: warp-wise >=-5.0%, broadwise >=-3.0%;
Fabric ultimate strength; Warp-wise >=300N, broadwise >=300N.
The specific embodiment
Embodiment 1
Positioning strip leisure fabric of the present invention, comprises body part and positioning strip part.The warp thread of body part adopts A raw material, B raw material, C raw material; Wherein A raw material is the sticky yarn of 14.7tex × 2 low temperature sun, B raw material be 14.7tex × 2 superbright light positive than color yarn slub yarn, C raw material is that radical is than the dark purplish blue look silk of 100D/36F, the dark royalblue silk of 100D/36F for 1:1.The warp thread of positioning strip part adopts D raw material, E raw material; Wherein D raw material is the reddish brown network yarn of 100D/36F, 100D illusion-colour paillette network yarn, the red silk of 150D/48F nine that radical ratio is 1:1:1, and E raw material is that radical is than the sky blue network yarn of 100D/36F, 100D illusion-colour paillette network yarn, the dark purplish blue look silk of 150D/48F that are 1:1:1.The weft yarn of body part adopts F raw material, G raw material, and wherein F raw material is the sticky yarn of 14.7tex × 2 low temperature sun, and G raw material is that radical is than having light DIY, 18.5tex superbright light positive than color yarn slub yarn for the 108D/36F of 1:1.The weft yarn raw material of positioning strip part is identical with the weft yarn raw material of body part.
The sticky yarn of above-mentioned low temperature sun is by low temperature CATION DTY, triangle profile CATION DTY, fine denier viscose composition, and between low temperature CATION DTY, triangle profile CATION DTY, fine denier viscose, blending ratio when dry weight is 45%:20%:35%.
Body part adopts 2/2 twill-weave, and positioning strip part adopts figured texture weave.
The technique of producing this positioning strip leisure fabric, comprises the following steps,
(1) warp thread → winder → double twisting → sizing → warping → gait → denting;
(2) weft yarn → winder → double twisting → sizing → rewinding;
(3) each the warp thread after above-mentioned manufacturing procedure raw material is woven into grey cloth together with the each raw material of weft yarn;
(4) grey cloth check → blank cloth coiling → kiering → pre-setting → dyeing and finishing → calendering → filling steaming → check → clot.
Wherein, in dyeing and finishing process, before dyeing, adopt soda ash and enzyme to carry out rear arrangement to grey cloth.It is 7 that soda ash is used for regulating pH value; The temperature of rear arrangement is 60 ℃, and the time is 30 minutes; Enzyme is amylase.
In two steps, first, with cation dyes, disperse dye one-bath dyeing, dyeing temperature is 125 ℃, then uses REACTIVE DYES two-bath dyeing in dyeing in dyeing and finishing process; When REACTIVE DYES dyes, be used in conjunction with salt-free dyeing crosslinking agent, salt-free dyeing crosslinking agent is Cyanuric Chloride.
Stentering forming in dyeing and finishing process, temperature is 160 ℃, and the sizing speed of a motor vehicle is 50 ms/min.
Weaving process, upper gate width is 180 centimetres; Body part adopts 2/2 twill-weave, and positioning strip part adopts figured texture weave.
C raw material in warp thread, the twist between its each component when double twisting is 6T/cmS; D raw material in warp thread, the twist between its each component when double twisting is 6T/cmS; E raw material in warp thread, the twist between its each component when double twisting is 6T/cmS; G raw material in weft yarn, the twist between its each component when double twisting is 6T/cmS.
Embodiment 2
Positioning strip leisure fabric of the present invention, comprises body part and positioning strip part.The warp thread of body part adopts A raw material, B raw material, C raw material; Wherein A raw material is the sticky yarn of 14.7tex × 2 low temperature sun, B raw material be 14.7tex × 2 superbright light positive than color yarn slub yarn, C raw material is that radical is than the dark purplish blue look silk of 100D/36F, the dark royalblue silk of 100D/36F for 1:1.The warp thread of positioning strip part adopts D raw material, E raw material; Wherein D raw material is the reddish brown network yarn of 100D/36F, 100D illusion-colour paillette network yarn, the red silk of 150D/48F nine that radical ratio is 1:1:1, and E raw material is that radical is than the sky blue network yarn of 100D/36F, 100D illusion-colour paillette network yarn, the dark purplish blue look silk of 150D/48F that are 1:1:1.The weft yarn of body part adopts F raw material, G raw material, and wherein F raw material is the sticky yarn of 14.7tex × 2 low temperature sun, and G raw material is that radical is than having light DIY, 18.5tex superbright light positive than color yarn slub yarn for the 108D/36F of 1:1.The weft yarn raw material of positioning strip part is identical with the weft yarn raw material of body part.
The sticky yarn of above-mentioned low temperature sun is by low temperature CATION DTY, triangle profile CATION DTY, fine denier viscose composition, and between low temperature CATION DTY, triangle profile CATION DTY, fine denier viscose, blending ratio when dry weight is 45%:20%:35%.
Body part adopts 2/2 twill-weave, and positioning strip part adopts figured texture weave.
The technique of producing this positioning strip leisure fabric, comprises the following steps,
(1) warp thread → winder → double twisting → sizing → warping → gait → denting;
(2) weft yarn → winder → double twisting → sizing → rewinding;
(3) each the warp thread after above-mentioned manufacturing procedure raw material is woven into grey cloth together with the each raw material of weft yarn;
(4) grey cloth check → blank cloth coiling → kiering → pre-setting → dyeing and finishing → calendering → filling steaming → check → clot.
Wherein, in dyeing and finishing process, before dyeing, adopt soda ash and enzyme to carry out rear arrangement to grey cloth.It is 8 that soda ash is used for regulating pH value; The temperature of rear arrangement is 80 ℃, and the time is 30 minutes; Enzyme is composite fibre enzyme.
In two steps, first, with cation dyes, disperse dye one-bath dyeing, dyeing temperature is 125 ℃, then uses REACTIVE DYES two-bath dyeing in dyeing in dyeing and finishing process; When REACTIVE DYES dyes, be used in conjunction with salt-free dyeing crosslinking agent.Salt-free dyeing crosslinking agent is polyisocyanates.
Stentering forming in dyeing and finishing process, temperature is 160 ℃, and the sizing speed of a motor vehicle is 50 ms/min.
Weaving process, upper gate width is 180 centimetres; Body part adopts 2/2 twill-weave, and positioning strip part adopts figured texture weave.
C raw material in warp thread, the twist between its each component when double twisting is 6T/cmS; D raw material in warp thread, the twist between its each component when double twisting is 6T/cmS; E raw material in warp thread, the twist between its each component when double twisting is 6T/cmS; G raw material in weft yarn, the twist between its each component when double twisting is 6T/cmS.
Embodiment 3
Positioning strip leisure fabric of the present invention, comprises body part and positioning strip part.The warp thread of body part adopts A raw material, B raw material, C raw material; Wherein A raw material is the sticky yarn of 14.7tex × 2 low temperature sun, B raw material be 14.7tex × 2 superbright light positive than color yarn slub yarn, C raw material is that radical is than the dark purplish blue look silk of 100D/36F, the dark royalblue silk of 100D/36F for 1:1.The warp thread of positioning strip part adopts D raw material, E raw material; Wherein D raw material is the reddish brown network yarn of 100D/36F, 100D illusion-colour paillette network yarn, the red silk of 150D/48F nine that radical ratio is 1:1:1, and E raw material is that radical is than the sky blue network yarn of 100D/36F, 100D illusion-colour paillette network yarn, the dark purplish blue look silk of 150D/48F that are 1:1:1.The weft yarn of body part adopts F raw material, G raw material, and wherein F raw material is the sticky yarn of 14.7tex × 2 low temperature sun, and G raw material is that radical is than having light DIY, 18.5tex superbright light positive than color yarn slub yarn for the 108D/36F of 1:1.The weft yarn raw material of positioning strip part is identical with the weft yarn raw material of body part.
The sticky yarn of above-mentioned low temperature sun is by low temperature CATION DTY, triangle profile CATION DTY, fine denier viscose composition, and between low temperature CATION DTY, triangle profile CATION DTY, fine denier viscose, blending ratio when dry weight is 45%:20%:35%.
Body part adopts 2/2 twill-weave, and positioning strip part adopts figured texture weave.
The technique of producing this positioning strip leisure fabric, comprises the following steps,
(1) warp thread → winder → double twisting → sizing → warping → gait → denting;
(2) weft yarn → winder → double twisting → sizing → rewinding;
(3) each the warp thread after above-mentioned manufacturing procedure raw material is woven into grey cloth together with the each raw material of weft yarn;
(4) grey cloth check → blank cloth coiling → kiering → pre-setting → dyeing and finishing → calendering → filling steaming → check → clot.
Wherein, in dyeing and finishing process, before dyeing, adopt soda ash and enzyme to carry out rear arrangement to grey cloth.It is 9 that soda ash is used for regulating pH value; The temperature of rear arrangement is 70 ℃, and the time is 30 minutes; Enzyme is protease.
In two steps, first, with cation dyes, disperse dye one-bath dyeing, dyeing temperature is 120 ℃, then uses REACTIVE DYES two-bath dyeing in dyeing in dyeing and finishing process; When REACTIVE DYES dyes, be used in conjunction with salt-free dyeing crosslinking agent.Salt-free dyeing crosslinking agent is active vinyl-compound.
Stentering forming in dyeing and finishing process, temperature is 150 ℃, and the sizing speed of a motor vehicle is 45 ms/min.
Weaving process, upper gate width is 180 centimetres; Body part adopts 2/2 twill-weave, and positioning strip part adopts figured texture weave.
C raw material in warp thread, the twist between its each component when double twisting is 6T/cmS; D raw material in warp thread, the twist between its each component when double twisting is 6T/cmS; E raw material in warp thread, the twist between its each component when double twisting is 6T/cmS; G raw material in weft yarn, the twist between its each component when double twisting is 6T/cmS.
Embodiment 4
Positioning strip leisure fabric of the present invention, comprises body part and positioning strip part.The warp thread of body part adopts A raw material, B raw material, C raw material; Wherein A raw material is the sticky yarn of 14.7tex × 2 low temperature sun, B raw material be 14.7tex × 2 superbright light positive than color yarn slub yarn, C raw material is that radical is than the dark purplish blue look silk of 100D/36F, the dark royalblue silk of 100D/36F for 1:1.The warp thread of positioning strip part adopts D raw material, E raw material; Wherein D raw material is the reddish brown network yarn of 100D/36F, 100D illusion-colour paillette network yarn, the red silk of 150D/48F nine that radical ratio is 1:1:1, and E raw material is that radical is than the sky blue network yarn of 100D/36F, 100D illusion-colour paillette network yarn, the dark purplish blue look silk of 150D/48F that are 1:1:1.The weft yarn of body part adopts F raw material, G raw material, and wherein F raw material is the sticky yarn of 14.7tex × 2 low temperature sun, and G raw material is that radical is than having light DIY, 18.5tex superbright light positive than color yarn slub yarn for the 108D/36F of 1:1.The weft yarn raw material of positioning strip part is identical with the weft yarn raw material of body part.
The sticky yarn of above-mentioned low temperature sun is by low temperature CATION DTY, triangle profile CATION DTY, fine denier viscose composition, and between low temperature CATION DTY, triangle profile CATION DTY, fine denier viscose, blending ratio when dry weight is 45%:20%:35%.
Body part adopts 2/2 twill-weave, and positioning strip part adopts figured texture weave.
The technique of producing this positioning strip leisure fabric, comprises the following steps,
(1) warp thread → winder → double twisting → sizing → warping → gait → denting;
(2) weft yarn → winder → double twisting → sizing → rewinding;
(3) each the warp thread after above-mentioned manufacturing procedure raw material is woven into grey cloth together with the each raw material of weft yarn;
(4) grey cloth check → blank cloth coiling → kiering → pre-setting → dyeing and finishing → calendering → filling steaming → check → clot.
Wherein, in dyeing and finishing process, before dyeing, adopt soda ash and enzyme to carry out rear arrangement to grey cloth.It is 8 that soda ash is used for regulating pH value; The temperature of rear arrangement is 60 ℃, and the time is 30 minutes; Enzyme is the mixture of amylase and protease.
In two steps, first, with cation dyes, disperse dye one-bath dyeing, dyeing temperature is 130 ℃, then uses REACTIVE DYES two-bath dyeing in dyeing in dyeing and finishing process; When REACTIVE DYES dyes, be used in conjunction with salt-free dyeing crosslinking agent.Salt-free dyeing crosslinking agent is Cyanuric Chloride.
Stentering forming in dyeing and finishing process, temperature is 165 ℃, and the sizing speed of a motor vehicle is 55 ms/min.
Weaving process, upper gate width is 180 centimetres; Body part adopts 2/2 twill-weave, and positioning strip part adopts figured texture weave.
C raw material in warp thread, the twist between its each component when double twisting is 6T/cmS; D raw material in warp thread, the twist between its each component when double twisting is 6T/cmS; E raw material in warp thread, the twist between its each component when double twisting is 6T/cmS; G raw material in weft yarn, the twist between its each component when double twisting is 6T/cmS.
Above-described embodiment is only for the inventive concept of the present invention of explaining, but not restriction to rights protection of the present invention, allly utilizes this design to carry out the change of unsubstantiality to the present invention, all should fall into protection scope of the present invention.

Claims (2)

1. a positioning strip leisure fabric, comprises body part and positioning strip part, it is characterized in that: the warp thread of described body part adopts A raw material, B raw material, C raw material; Wherein A raw material is the sticky yarn of 14.7tex × 2 low temperature sun, B raw material be 14.7tex × 2 superbright light positive than color yarn slub yarn, C raw material is that radical is than the dark purplish blue look silk of 100D/36F, the dark royalblue silk of 100D/36F for 1:1; The warp thread of positioning strip part adopts D raw material, E raw material; Wherein D raw material is the reddish brown network yarn of 100D/36F, 100D illusion-colour paillette network yarn, the red silk of 150D/48F nine that radical ratio is 1:1:1, and E raw material is that radical is than the sky blue network yarn of 100D/36F, 100D illusion-colour paillette network yarn, the dark purplish blue look silk of 150D/48F that are 1:1:1; The weft yarn of body part adopts F raw material, G raw material, and wherein F raw material is the sticky yarn of 14.7tex × 2 low temperature sun, and G raw material is that radical is than having light DIY, 18.5tex superbright light positive than color yarn slub yarn for the 108D/36F of 1:1; The weft yarn raw material of positioning strip part is identical with the weft yarn raw material of body part;
Its production technology comprises the following steps:
(1) warp thread → winder → double twisting → sizing → warping → gait → denting;
(2) weft yarn → winder → double twisting → sizing → rewinding;
(3) each the warp thread after above-mentioned manufacturing procedure raw material is woven into grey cloth together with the each raw material of weft yarn;
(4) grey cloth check → blank cloth coiling → kiering → pre-setting → dyeing and finishing → calendering → filling steaming → check → clot;
In two steps, first, with cation dyes, disperse dye one-bath dyeing, dyeing temperature is 120-130 ℃, then uses REACTIVE DYES two-bath dyeing in dyeing in described dyeing and finishing process;
Stentering forming in dyeing and finishing process, temperature is 150-165 ℃, and the sizing speed of a motor vehicle is 45-55 m/min;
In described dyeing and finishing process, before dyeing, adopt soda ash and enzyme to carry out rear arrangement to grey cloth, to be wherein used for regulating pH value be 7-9 to soda ash; The temperature of rear arrangement is 60-80 ℃, and the time is 30 minutes; Enzyme is any one or the multiple mixture in amylase, composite fibre enzyme, protease, esterase;
The sticky yarn of described low temperature sun is made up of low temperature CATION DTY, triangle profile CATION DTY, fine denier viscose, and between low temperature CATION DTY, triangle profile CATION DTY, fine denier viscose, blending ratio when dry weight is 45%:20%:35%;
C raw material in described warp thread, the twist between its each component when double twisting is 6T/cmS; D raw material in warp thread, the twist between its each component when double twisting is 6T/cmS; E raw material in warp thread, the twist between its each component when double twisting is 6T/cmS; G raw material in weft yarn, the twist between its each component when double twisting is 6T/cmS;
Described weaving process, upper gate width is 180 centimetres; Body part adopts 2/2 twill-weave, and positioning strip part adopts figured texture weave.
2. positioning strip leisure fabric as claimed in claim 1, is characterized in that: when described REACTIVE DYES dyes, be used in conjunction with salt-free dyeing crosslinking agent.
CN201110071730.7A 2011-03-24 2011-03-24 Positioning strip leisure fabric and production process thereof Expired - Fee Related CN102134772B (en)