A kind of environment-friendly type is strengthened the production method of bamboo and wood products
The ㈠ technical field: the present invention relates to furniture and architectural constructional materials manufacturing technology, especially a kind of environment-friendly type is strengthened the production method of bamboo and wood products.
The ㈡ background technology: traditional furniture, woodwork palpus employing redwood, pear wood, camphorwood, Chinese toon wood etc. are strong but pliable in texture, density big, the high-quality timber of good stability is made, and general low-grade timber can not be used to manufacture furniture etc.Existing bamboo and wood products is yielding, damage by worms, be subjected to deliquescence, and the holding time is limited, need to paint after the processing of general bamboo wood, but existing paint staining poor permeability, fugitive color, come off, damaged in collision.
The ㈢ summary of the invention: purpose of the present invention will solve conventional method processing bamboo and wood products exactly, furniture is yielding, damage by worms, be subjected to deliquescence, the holding time is limited, paint fugitive color, come off, damaged in collision, and need high-quality timber to make, the problem that cost is high provides a kind of a kind of environment-friendly type of the high-grade furniture of common wood and bamboo making, goods that can adopt to strengthen the production method of bamboo and wood products.
Concrete scheme of the present invention is: at first carry out bamboo wood processing and forming, it is characterized in that: the bamboo and wood products that processes is put into baking oven heat to 70-90 ℃, constant temperature 5-7 hour → put into pressure pan to vacuumize → inject C01-1 alkyd edible vegetable oil submergence woodwork, soak 2 hours → taking-up and put into baking oven inner control temperature at 80-90 ℃ of curing 3-4 hour → taking-up sanding and polishing → finished product to the pressure pan inner high voltage.
Pressure among the present invention when pressure pan injects C01-1 alkyd edible vegetable oil is not less than 3 atmospheric pressure.
In pressure pan, inject C01-1 alkyd edible vegetable oil among the present invention and mix a certain amount of oiliness pigment simultaneously, before injecting COH alkyd edible vegetable oil is fully mixed with the oiliness pigment.
The inventive method is easy and simple to handle, draws materials extensively, not only can use high-quality timber, can also use common low-grade timber such as bamboo, paulownia wood, poplar, willow wood to make high-grade furniture and decorative architecture bamboo and wood products.Adopt products C OH alkyd edible vegetable oil infiltration that the inventive method makes wherein, enhanced products can be exempted from paint, fire prevention, moistureproofly, anti-damages by worms, anti-aging, color tunable, and the original bamboo wood grain after showing signs of anger is constant, can forever preserve.
The ㈣ description of drawings:
Accompanying drawing is the structural representation of pressure pan of the present invention.
The ㈤ specific embodiment:
Example 1: take the inventive method to make one environment-friendly type reinforced wood chair, flow process is as follows:
It is some that ⒈ gets poplar, and the carpenter is made into the log chair;
⒉ puts into baking oven with the log chair and heats to 70 ℃, constant temperature 6 hours;
Log chair after ⒊ will heat is put into pressure pan from the baking oven taking-up and is vacuumized.Described pressure pan structure is referring to accompanying drawing, and it has tank body 1 and seal cover 2, and seal cover 2 is provided with vacuum valve 3 and irritates fuel tap door 5 and Pressure gauge 4, and vacuum valve 3 is irritated fuel tap door 5 by the external hydraulic pump 7 of pipeline by the external vavuum pump 6 of pipeline.
⒋ injects C01-1 alkyd edible vegetable oil by hydraulic pump 7 to pressure pan inner high voltage (3 and above atmospheric pressure), and submergence log chair soaked 2 hours.
⒌ takes out chair and puts into baking oven inner control temperature 80 ℃ of curing 3 hours.
⒍ takes out the chair sanding and polishing can make an environment-friendly type reinforcement chair.
Example 2: it is as follows to adopt environment-friendly type of the inventive method making to strengthen bamboo screen flow process:
It is some that ⒈ gets bamboo chip, and the carpenter is made into the bamboo chip screen;
⒉ puts into baking oven with the bamboo chip screen and heats to 80 ℃, constant temperature 5 hours;
Bamboo chip screen after ⒊ will heat is put into pressure pan from the baking oven taking-up and is vacuumized.Described pressure pan structure is with example 1.
⒋ injects C01-1 alkyd edible vegetable oil by hydraulic pump 7 to pressure pan inner high voltage (3 and above atmospheric pressure), and submergence bamboo chip screen soaked 2 hours.
⒌ takes out screen and puts into baking oven inner control temperature 86 ℃ of curing 3.5 hours.
⒍ takes out the screen sanding and polishing can make an environment-friendly type reinforcement screen.
Example 3: it is as follows to adopt environment-friendly type of the inventive method making to strengthen red wooden tea table flow process:
It is some that ⒈ gets willow wood, and the carpenter is made into the log tea table;
⒉ puts into baking oven with the log tea table and heats to 90 ℃, constant temperature 7 hours;
Log tea table after ⒊ will heat is put into pressure pan from the baking oven taking-up and is vacuumized.Described pressure pan structure is with example 1.
⒋ gets COH alkyd edible vegetable oil, red oiliness pigment, add the red oiliness pigment ratio allotment of 0.5 gram (general 1 kilogram of COH alkyd edible vegetable oil adds 0-1 gram oiliness pigment ratio to be grasped, and selects color, determines depth ratio according to user's request) in 1 kilogram of COH alkyd edible vegetable oil.Fully mix, inject C01-1 alkyd edible vegetable oil and red oiliness pigment mixed liquor by hydraulic pump 7 to pressure pan inner high voltage (3 and above atmospheric pressure) again, submergence log tea table soaked 2 hours.
⒌ takes out tea table and puts into baking oven inner control temperature 90 ℃ of curing 4 hours.
⒍ takes out the tea table sanding and polishing can make an environment-friendly type reinforcement tea table.