CN101870573A CN201010214279A CN201010214279A CN101870573A CN 101870573 A CN101870573 A CN 101870573A CN 201010214279 A CN201010214279 A CN 201010214279A CN 201010214279 A CN201010214279 A CN 201010214279A CN 101870573 A CN101870573 A CN 101870573A
Authority
CN
China
Prior art keywords
acrylic acid
waterproof mortar
acid modified
modified waterproof
quartz sand
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201010214279A
Other languages
Chinese (zh)
Inventor
张永进
张毅
张宜萍
辛春华
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
SHANGHAI INSURING POLYMER MATERIALS CO Ltd
Original Assignee
SHANGHAI INSURING POLYMER MATERIALS CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by SHANGHAI INSURING POLYMER MATERIALS CO Ltd filed Critical SHANGHAI INSURING POLYMER MATERIALS CO Ltd
Priority to CN201010214279A priority Critical patent/CN101870573A/en
Publication of CN101870573A publication Critical patent/CN101870573A/en
Pending legal-status Critical Current

Links

Classifications

    • CCHEMISTRY; METALLURGY
    • C04CEMENTS; CONCRETE; ARTIFICIAL STONE; CERAMICS; REFRACTORIES
    • C04BLIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE; CERAMICS; REFRACTORIES; TREATMENT OF NATURAL STONE
    • C04B28/00Compositions of mortars, concrete or artificial stone, containing inorganic binders or the reaction product of an inorganic and an organic binder, e.g. polycarboxylate cements
    • C04B28/02Compositions of mortars, concrete or artificial stone, containing inorganic binders or the reaction product of an inorganic and an organic binder, e.g. polycarboxylate cements containing hydraulic cements other than calcium sulfates
    • CCHEMISTRY; METALLURGY
    • C04CEMENTS; CONCRETE; ARTIFICIAL STONE; CERAMICS; REFRACTORIES
    • C04BLIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE; CERAMICS; REFRACTORIES; TREATMENT OF NATURAL STONE
    • C04B2111/00Mortars, concrete or artificial stone or mixtures to prepare them, characterised by specific function, property or use
    • C04B2111/20Resistance against chemical, physical or biological attack
    • C04B2111/27Water resistance, i.e. waterproof or water-repellent materials
    • YGENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y02TECHNOLOGIES OR APPLICATIONS FOR MITIGATION OR ADAPTATION AGAINST CLIMATE CHANGE
    • Y02WCLIMATE CHANGE MITIGATION TECHNOLOGIES RELATED TO WASTEWATER TREATMENT OR WASTE MANAGEMENT
    • Y02W30/00Technologies for solid waste management
    • Y02W30/50Reuse, recycling or recovery technologies
    • Y02W30/91Use of waste materials as fillers for mortars or concrete

Landscapes

  • Chemical & Material Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Ceramic Engineering (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Inorganic Chemistry (AREA)
  • Materials Engineering (AREA)
  • Structural Engineering (AREA)
  • Organic Chemistry (AREA)
  • Curing Cements, Concrete, And Artificial Stone (AREA)

Abstract

The invention relates to acrylic acid modified waterproof mortar comprising cement, quartz sands, pulverized fuel ash, triple superphosphate powder, acrylic acid redispersable rubber powder, a water-repellent agent, a deforming agent and other auxiliary agents. The waterproof mortar with compact structure is obtained by adopting the acrylic acid redispersable rubber powder which has excellent ageing-resistant property and water-resistant property and good quartz sand graduation through formulation design and optimization, not only has good waterproof and impervious property, but also has excellent ageing-resistant property and excellent physical property.

Description

Acrylic acid modified waterproof mortar
Technical field
The present invention relates to a kind of building water-proof mortar material, relate in particular to a kind of polymer modification waterproof mortar for building.
Background technology
Traditional building water-proof material is mostly based on flexible materials, as various waterproof rolls and waterproof paint etc.They form watertight insulation by paving or coating in the building substrate surface.Yet because the compatibility problem of flexible waterproof material and matrix make that its ageing-resistant performance is relatively poor, and cost is higher.Waterproof mortar be a kind of be raw material by cement, sandstone, mix a small amount of admixture and macromolecular material therein,, reduce porosity by adjusting proportioning, increase method such as closely knit performance between each starting material interface, formulated a kind of sand-cement slurry class water-proof material with certain impervious ability.It is bigger that this type of water-proof material can be widely used in structural rigidity, and building deformation is less, and the engineering lower to impervious requirement because this kind water-proof material cost is lower, has good prospects for application.
200910074498.5 1 kinds of environment-friendly type waterproof polymer mortars of patent disclose a kind of waterproof mortar, described waterproof mortar is made up of cement, quartz sand, flyash, plastic of poly vinyl acetate redispersable latex powder, Vinyl Acetate Copolymer tertiary ethylene carbonate redispersable latex powder, water reducer, defoamer, polyacrylic fibre, has good anti-permeability performance and workability.
Existing waterproof polymer mortar, though have good anti-permeability performance, it does not have good aging properties, and its weak point is arranged in actual applications, so its performance remains further perfect.
Summary of the invention
The purpose of this invention is to provide a kind of acrylic acid modified waterproof mortar with premium properties, this mortar has good anti-folding, compressive property, excellent anti-permeability performance and ageing-resistant performance.Waterproof mortar of the present invention consists of:
Cement 42-50
Quartz sand 35-40
Flyash 5-15
Coarse whiting 5-15
Re-dispersible glue powder 2.5-3.5
Ether of cellulose 0.02-0.05
Hydrophober 0.1-0.2
Modification boron-moisten soil 0.2-0.3
Defoamer 0.2-0.3
Water reducer 0.15-0.3
Polypropylene fibre 0.1-0.2
Further, above-mentioned cement is ordinary portland cement, preferred 425 ash concretes.
Above-mentioned quartz sand is preferably two kinds of gratings in 30-50,40-70,50-100, the 70-140 order quartz sand.
Above-mentioned coarse whiting is preferably 200 purpose coarse whitings.
Above-mentioned re-dispersible glue powder is preferably the vinylformic acid rubber powder.
Above-mentioned ether of cellulose is preferably viscosity at the methyl cellulose ether below 10000.
Above-mentioned hydrophober is preferably the hydrophober of organosilicon type.
Above-mentioned defoamer is preferably the modified siloxane defoamer.
Above-mentioned water reducer is preferably carboxylic acid water reducing agent.
It is 6mm that above-mentioned polypropylene fibre is preferably specification.
Acrylic acid modified waterproof mortar of the present invention, with cement is main gelatinous material, adopt the modification of vinylformic acid re-dispersible glue powder, add the quartz sand of different gradation, coarse whiting, hydrophober and the cooperation of other auxiliary agent form, because the vinylformic acid re-dispersible glue powder is compared EVA rubber powder commonly used, excellent in water resistance energy and ageing-resistant performance are arranged, can guarantee that resulting waterproof mortar has good bonding strength and ageing-resistant performance, by optimizing its addition, waterproof mortar solidifies back vinylformic acid rubber powder can form the successive rete therein, cooperate other filler and grating quartz sand, can be so that closely knit waterproof layer has good endurance quality and waterproof impervious characteristic, in addition, owing to adopted high performance cement and good grating quartz sand, can guarantee that by adjusting the prescription composition waterproof mortar of the present invention has excellent anti-folding, physicalies such as resistance to compression.
Embodiment
Embodiment 1
A kind of raw material composition and mass fraction thereof of acrylic acid modified waterproof mortar are as shown in table 1:
Table 1 raw material is formed and mass fraction
Material name Model Weight
Ordinary portland cement ??425 ??42
Quartz sand The 30-50 order ??20
Orpiment sand The 50-100 order ??20
Flyash The II level ??15
Coarse whiting 200 orders ??5
Re-dispersible glue powder ??695P ??3.5
Ether of cellulose ??HK8000 ??0.02
Hydrophober ??69051 ??0.2
The modification boron-moisten soil ??- ??0.2
Defoamer ??P210 ??0.3
Water reducer ??CPC-1 ??0.15
Polypropylene fibre ??PP6 ??0.2
The preparation method of above-mentioned waterproof mortar is: according to proportioning raw materials, various raw materials are added in the mixed/stirred bucket successively, reinforced principle is for adding raw materials such as the big cement of consumption, quartz sand earlier, and the back adds raw materials such as the less re-dispersible glue powder of consumption, ether of cellulose, mixes stand-by.
Above-mentioned waterproof mortar using method is: the powder for preparing is joined mix in the agitation vat, be metered into the water of 18-21%, stir, ageing can be used after 5 minutes, can evenly be coated to the building substrate surface that needs to want waterproof by instruments such as spatulas, dry solidification obtains waterproof layer.This waterproof mortar excellent property has good aging properties and anti-permeability performance, and its specific performance index such as following table 2 are as showing:
Table 2 waterproof mortar performance index
Figure BSA00000193425300031
Annotate: the performance test methods in the table is with reference to JC/T984-2005 polymer cement waterproof mortar.
Embodiment 2
A kind of raw material composition and mass fraction thereof of acrylic acid modified waterproof mortar are as shown in table 3:
Table 3 raw material is formed and mass fraction
Material name Model Weight
Ordinary portland cement ??425 ??45
Quartz sand The 40-70 order ??18
Material name Model Weight
Quartz sand The 70-140 order ??20
Flyash The II level ??6
Coarse whiting 200 orders ??15
Re-dispersible glue powder ??695P ??3
Ether of cellulose ??MC7000PF ??0.04
Hydrophober ??P750 ??0.1
The modification boron-moisten soil ??- ??0.2
Defoamer ??P210 ??0.25
Water reducer ??F10 ??0.2
Polypropylene fibre ??PP6 ??0.2
Above-mentioned waterproof mortar preparation method and using method be with implementing just 1, its specific performance index such as following table 4 as show:
Table 4 waterproof mortar performance index
Figure BSA00000193425300041
Annotate: the performance test methods in the table is with reference to JC/T984-2005 polymer cement waterproof mortar.
Embodiment 3
A kind of raw material composition and mass fraction thereof of acrylic acid modified waterproof mortar are as shown in table 5:
Table 5 raw material is formed and mass fraction
Material name Model Weight
Ordinary portland cement ??425 ??50
Quartz sand The 40-70 order ??20
Quartz sand The 50-100 order ??15
Flyash The II level ??5
Coarse whiting 200 orders ??7
Re-dispersible glue powder ??695P ??2.5
Ether of cellulose ??MC7000PF ??0.05
Hydrophober ??69051 ??0.2
The modification boron-moisten soil ??- ??0.2
Defoamer ??RE2971 ??0.2
Water reducer ??F10 ??0.3
Polypropylene fibre ??PP6 ??0.1
Above-mentioned waterproof mortar preparation method and using method are with embodiment 1, and its specific performance index such as following table 6 are as showing:
Table 6 waterproof mortar performance index
Figure BSA00000193425300051
Annotate: the performance test methods in the table is with reference to JC/T984-2005 polymer cement waterproof mortar.

Claims (10)

1. an acrylic acid modified waterproof mortar is characterized in that, and is composed as follows in the raw material of weight part:
Cement 42-50;
Quartz sand 35-40;
Flyash 5-15;
Coarse whiting 5-15;
Re-dispersible glue powder 2.5-3.5;
Ether of cellulose 0.02-0.05;
Hydrophober 0.1-0.2;
Modification boron-moisten soil 0.2-0.3;
Defoamer 0.2-0.3;
Water reducer 0.15-0.3;
Polypropylene fibre 0.1-0.2.
2. acrylic acid modified waterproof mortar as claimed in claim 1 is characterized in that, described cement is ordinary portland cement.
3. acrylic acid modified waterproof mortar as claimed in claim 1 is characterized in that, described quartz sand is two kinds of gratings in 30-50,40-70,50-100, the 70-140 order quartz sand.
4. acrylic acid modified waterproof mortar as claimed in claim 1 is characterized in that, described re-dispersible glue powder is the vinylformic acid rubber powder.
5. acrylic acid modified waterproof mortar as claimed in claim 1 is characterized in that, described ether of cellulose is that viscosity is at the methyl cellulose ether below 10000.
6. acrylic acid modified waterproof mortar as claimed in claim 1 is characterized in that, described hydrophober is organosilicon moisture repellent.
7. acrylic acid modified waterproof mortar as claimed in claim 1 is characterized in that, described defoamer is the modified siloxane defoamer.
8. acrylic acid modified waterproof mortar as claimed in claim 1 is characterized in that, described coarse whiting is 200 purpose coarse whitings.
9. acrylic acid modified waterproof mortar as claimed in claim 1 is characterized in that, described polypropylene fibre specification is 6mm.
10. acrylic acid modified waterproof mortar as claimed in claim 1 is characterized in that, described water reducer is a carboxylic acid water reducing agent.
CN201010214279A 2010-06-29 2010-06-29 Acrylic acid modified waterproof mortar Pending CN101870573A (en)

Priority Applications (1)

Application Number Priority Date Filing Date Title
CN201010214279A CN101870573A (en) 2010-06-29 2010-06-29 Acrylic acid modified waterproof mortar

Applications Claiming Priority (1)

Application Number Priority Date Filing Date Title
CN201010214279A CN101870573A (en) 2010-06-29 2010-06-29 Acrylic acid modified waterproof mortar

Publications (1)

Publication Number Publication Date
CN101870573A true CN101870573A (en) 2010-10-27

Family

ID=42995680

Family Applications (1)

Application Number Title Priority Date Filing Date
CN201010214279A Pending CN101870573A (en) 2010-06-29 2010-06-29 Acrylic acid modified waterproof mortar

Country Status (1)

Country Link
CN (1) CN101870573A (en)

Cited By (26)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN102249629A (en) * 2011-06-10 2011-11-23 上海三瑞高分子材料有限公司 Acrylate emulsion modified cement-base repair mortar
CN102605867A (en) * 2012-03-08 2012-07-25 上海天补建筑科技有限公司 External wall insulation structure through foaming cement board and construction method thereof
CN102619310A (en) * 2012-03-08 2012-08-01 上海天补建筑科技有限公司 Coating system dedicated for outer wall reflecting and heat-insulating paint and construction method of coating system
CN103058591A (en) * 2012-12-26 2013-04-24 上海天补建筑科技有限公司 Protective coloring material used for concrete surfaces and preparation method thereof
CN103058619A (en) * 2013-01-17 2013-04-24 同济大学 Mineral powder-doped polymer waterproof mortar and using method thereof
CN103253922A (en) * 2013-04-18 2013-08-21 池州版筑科技有限公司 Bentonite binder of light batten for building partition
CN103304202A (en) * 2013-06-25 2013-09-18 江苏蓝圈新材料有限公司 Polymer waterproof mortar
CN103964763A (en) * 2014-04-04 2014-08-06 黄裕兵 Preparation method of modified cement mortar
CN104140231A (en) * 2014-08-08 2014-11-12 鳄鱼制漆(上海)有限公司 Environment-friendly waterproof mortar
CN104478349A (en) * 2014-11-08 2015-04-01 辽宁省建设科学研究院 Early strength high wear-resisting self-leveling mortar used for ground repairing and preparation method thereof
CN104724990A (en) * 2015-03-09 2015-06-24 东莞市万科建筑技术研究有限公司 Mortar for splicing mounting of light partition boards and splicing mounting process
CN105130303A (en) * 2015-08-24 2015-12-09 安徽芜湖飞琪水泥制品有限公司 Heat-resistant cement column and preparation method therefor
CN105130304A (en) * 2015-08-24 2015-12-09 安徽芜湖飞琪水泥制品有限公司 Cement column with high anti-permeability and preparation method therefor
CN105198297A (en) * 2015-09-30 2015-12-30 安徽坤隆新型建材有限公司 Low-shrinkage mortar for aerated bricks
CN105314948A (en) * 2015-11-30 2016-02-10 上海宝田新型建材有限公司 Preparation method of polymer waterproof mortar
CN105503067A (en) * 2015-11-30 2016-04-20 上海宝田新型建材有限公司 Polymer-cement based waterproof mortar and application thereof
CN105503066A (en) * 2015-11-30 2016-04-20 上海宝田新型建材有限公司 Polymer waterproof mortar and application thereof
CN105924113A (en) * 2016-04-18 2016-09-07 盐城工学院 Self-heat insulation aerated concrete building block and mortar for construction of building blocks
WO2017071722A1 (en) * 2015-10-29 2017-05-04 Knauf Gips Kg Mineral sealing mortar
CN107200535A (en) * 2017-07-24 2017-09-26 四川君璜建材有限公司 A kind of environmental protection resists dry and cracked light partition board bonding agent and preparation method thereof
CN107311533A (en) * 2017-06-28 2017-11-03 佛山市涂无忧建材有限公司 A kind of waterproof and the high Polymer Mortar of adhesion strength and preparation method thereof
CN107619223A (en) * 2017-09-29 2018-01-23 佛山市涂无忧建材有限公司 A kind of waterproof mortar with anti-slipping property energy and preparation method thereof
CN108383477A (en) * 2018-05-03 2018-08-10 福建汇达建筑工程有限公司 A kind of modified cement-based waterproof mortar and preparation method thereof
CN109456005A (en) * 2018-12-17 2019-03-12 派丽(上海)管理有限公司 A kind of Polymer cement materials
CN109455996A (en) * 2018-11-05 2019-03-12 富思特新材料科技发展股份有限公司 A kind of danger external wall insulation grouting and reinforcing mortar
CN110577410A (en) * 2019-06-18 2019-12-17 佛山市涂无忧建材有限公司 Cement-based waterproof filling material

Citations (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN101560084A (en) * 2009-06-02 2009-10-21 河北科技大学 Environmental-friendly waterproof polymer mortar
CN101723638A (en) * 2009-12-14 2010-06-09 上海英硕聚合物材料有限公司 Wall facing mortar

Patent Citations (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN101560084A (en) * 2009-06-02 2009-10-21 河北科技大学 Environmental-friendly waterproof polymer mortar
CN101723638A (en) * 2009-12-14 2010-06-09 上海英硕聚合物材料有限公司 Wall facing mortar

Cited By (33)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN102249629A (en) * 2011-06-10 2011-11-23 上海三瑞高分子材料有限公司 Acrylate emulsion modified cement-base repair mortar
CN102605867A (en) * 2012-03-08 2012-07-25 上海天补建筑科技有限公司 External wall insulation structure through foaming cement board and construction method thereof
CN102619310A (en) * 2012-03-08 2012-08-01 上海天补建筑科技有限公司 Coating system dedicated for outer wall reflecting and heat-insulating paint and construction method of coating system
CN102605867B (en) * 2012-03-08 2014-09-10 上海天补建筑科技有限公司 External wall insulation structure through foaming cement board and construction method thereof
CN103058591A (en) * 2012-12-26 2013-04-24 上海天补建筑科技有限公司 Protective coloring material used for concrete surfaces and preparation method thereof
CN103058591B (en) * 2012-12-26 2014-09-24 上海天补建筑科技有限公司 Protective coloring material used for concrete surfaces and preparation method thereof
CN103058619A (en) * 2013-01-17 2013-04-24 同济大学 Mineral powder-doped polymer waterproof mortar and using method thereof
CN103253922B (en) * 2013-04-18 2016-04-20 池州版筑科技有限公司 A kind of light lath for building partition wall bentonite adhesive
CN103253922A (en) * 2013-04-18 2013-08-21 池州版筑科技有限公司 Bentonite binder of light batten for building partition
CN103304202A (en) * 2013-06-25 2013-09-18 江苏蓝圈新材料有限公司 Polymer waterproof mortar
CN103964763A (en) * 2014-04-04 2014-08-06 黄裕兵 Preparation method of modified cement mortar
CN104140231A (en) * 2014-08-08 2014-11-12 鳄鱼制漆(上海)有限公司 Environment-friendly waterproof mortar
CN104478349B (en) * 2014-11-08 2017-11-07 辽宁省建设科学研究院 A kind of early strong high abrasion gravity flowing levelling mortar repaired for ground and preparation method thereof
CN104478349A (en) * 2014-11-08 2015-04-01 辽宁省建设科学研究院 Early strength high wear-resisting self-leveling mortar used for ground repairing and preparation method thereof
CN104724990A (en) * 2015-03-09 2015-06-24 东莞市万科建筑技术研究有限公司 Mortar for splicing mounting of light partition boards and splicing mounting process
CN105130304A (en) * 2015-08-24 2015-12-09 安徽芜湖飞琪水泥制品有限公司 Cement column with high anti-permeability and preparation method therefor
CN105130304B (en) * 2015-08-24 2019-02-05 安徽芜湖飞琪水泥制品有限公司 Impervious cement column and preparation method thereof
CN105130303A (en) * 2015-08-24 2015-12-09 安徽芜湖飞琪水泥制品有限公司 Heat-resistant cement column and preparation method therefor
CN105198297A (en) * 2015-09-30 2015-12-30 安徽坤隆新型建材有限公司 Low-shrinkage mortar for aerated bricks
WO2017071722A1 (en) * 2015-10-29 2017-05-04 Knauf Gips Kg Mineral sealing mortar
CN105314948A (en) * 2015-11-30 2016-02-10 上海宝田新型建材有限公司 Preparation method of polymer waterproof mortar
CN105503067A (en) * 2015-11-30 2016-04-20 上海宝田新型建材有限公司 Polymer-cement based waterproof mortar and application thereof
CN105503066A (en) * 2015-11-30 2016-04-20 上海宝田新型建材有限公司 Polymer waterproof mortar and application thereof
CN105924113A (en) * 2016-04-18 2016-09-07 盐城工学院 Self-heat insulation aerated concrete building block and mortar for construction of building blocks
CN107311533A (en) * 2017-06-28 2017-11-03 佛山市涂无忧建材有限公司 A kind of waterproof and the high Polymer Mortar of adhesion strength and preparation method thereof
CN107200535A (en) * 2017-07-24 2017-09-26 四川君璜建材有限公司 A kind of environmental protection resists dry and cracked light partition board bonding agent and preparation method thereof
CN107619223A (en) * 2017-09-29 2018-01-23 佛山市涂无忧建材有限公司 A kind of waterproof mortar with anti-slipping property energy and preparation method thereof
CN108383477A (en) * 2018-05-03 2018-08-10 福建汇达建筑工程有限公司 A kind of modified cement-based waterproof mortar and preparation method thereof
CN108383477B (en) * 2018-05-03 2019-06-07 福建汇达建筑工程有限公司 A kind of modified cement-based waterproof mortar and preparation method thereof
CN109455996A (en) * 2018-11-05 2019-03-12 富思特新材料科技发展股份有限公司 A kind of danger external wall insulation grouting and reinforcing mortar
CN109456005A (en) * 2018-12-17 2019-03-12 派丽(上海)管理有限公司 A kind of Polymer cement materials
CN109456005B (en) * 2018-12-17 2022-03-22 西卡(上海)管理有限公司 Polymer cement waterproof mortar
CN110577410A (en) * 2019-06-18 2019-12-17 佛山市涂无忧建材有限公司 Cement-based waterproof filling material

Similar Documents

Publication Publication Date Title
CN101870573A (en) Acrylic acid modified waterproof mortar
CN104945997A (en) External wall flexible waterproof putty powder and preparation method thereof
CN103332901A (en) Anti-cracking waterproof mortar
CN102491709B (en) Cement-based polymer water-proof mortar and preparation method thereof
JP5590492B2 (en) Cement-containing polymer-based waterproofing agent and method for producing the same
CN109439054B (en) Putty powder and putty slurry for plastering-free machine, and preparation method and application thereof
CN112341878B (en) Polymer cement waterproof coating, roof waterproof layer and preparation method thereof
CN101269936B (en) Interface mortar
CN107162502A (en) A kind of fiber reinforced type polymer cement waterproof paint
CN103342525A (en) Waterproof and decorative dry powder mortar and coating process for same
CN101508539B (en) Polymer glue powder and method of use thereof
CN105906265A (en) Waterproof flexible cement-based dry-mixed overlay repairing mortar
CN108751843A (en) Backwater pressure water-repellent paint impervious for back side leak stopping and preparation method thereof
CN108046687B (en) Graphene modified cement-based waterproof coating
CN103224366A (en) Monocomponent polymer cement waterproof slurry containing slurry microcrystalline powder
CN102503321A (en) Cement base self-leveling for cushion layer
CN108298915A (en) A kind of exterior wall Crack-resistance Front Mortar and preparation method thereof containing fiberglass recycled fiber
CN101386505A (en) Dry powder mortar adhesive agent and preparation method thereof
CN109574591B (en) Leveling mortar with waterproof function
CN107619232A (en) Tile style waterproofing and thermal insulation of roofing adhesive mortar and preparation method thereof
CN103058608B (en) Monocomponent elastic waterproof putty and construction method thereof
CN101343158A (en) Liquid fine-expansion pumping agent
CN105272074A (en) Preparation method of energy-saving environment-friendly highly anti-seepage water-proof mortar
CN107540318A (en) A kind of cement base water-proof plugging material
CN108264270B (en) Environment-friendly slurry for paving metal floor tiles

Legal Events

Date Code Title Description
C06 Publication
PB01 Publication
C10 Entry into substantive examination
SE01 Entry into force of request for substantive examination
C02 Deemed withdrawal of patent application after publication (patent law 2001)
WD01 Invention patent application deemed withdrawn after publication

Application publication date: 20101027