CN100562369C - 高铁泥化钼铅矿浮选方法 - Google Patents
高铁泥化钼铅矿浮选方法 Download PDFInfo
- Publication number
- CN100562369C CN100562369C CNB2007100502811A CN200710050281A CN100562369C CN 100562369 C CN100562369 C CN 100562369C CN B2007100502811 A CNB2007100502811 A CN B2007100502811A CN 200710050281 A CN200710050281 A CN 200710050281A CN 100562369 C CN100562369 C CN 100562369C
- Authority
- CN
- China
- Prior art keywords
- wulfenite
- agent
- kerosene
- aqueous solution
- copper sulphate
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Fee Related
Abstract
一种高铁泥化钼铅矿浮选方法,采用六偏磷酸钠作为散剂,氢氧化钠作矿浆pH调整剂,以硫化钠进行硫化脱铅,硫酸铜作活化剂,煤油作疏水剂,异戊基黄药作钼铅矿捕收剂,2号油作起泡剂。采用本发明能够有效将泥化严重、含铁高的钼铅矿进行浮选回收,在给矿钼品位为0.5~0.76%条件下,经过一次粗选两次扫选及四次精选,钼精矿品位可达13~16.8%,回收率达到71~76%。
Description
一、技术领域
本发明涉及一种矿物浮选方法,特别是一种高铁泥化钼铅矿浮选方法。
二、背景技术
中国专利申请NO.200610048650.9公开了一种用浮-重-浮联合流程回收彩钼铅矿的方法,以彩钼铅矿为原料,将矿石磨矿至矿物单体解离;首先用浮选设备和药剂将钼矿物与脉石矿物相分离,上浮产物为钼精矿产品;再用摇床将浮选尾矿中的钼矿物与脉石矿物进一步分离得重选钼精矿产品。当第一段磨矿不足以使钼矿物充分单体解离时,将摇床尾矿进一步磨矿,使钼矿物进一步单体解离,最后用浮选设备和药剂进一步分离得钼精矿产品;浮选药剂用硫化钠、丁基黄药、丁铵黑药和松油。该发明适用于以彩钼铅矿为主要目的矿物的钼矿物与脉石矿物的分离。但是该发明流程长且较为复杂,需多段磨矿,浮选前需要脱泥,而且钼矿物回收率不高,仅为65%,精矿质量也只有7.25%;另外,该工艺设备投资大,占地广,能耗较大。此外,对高铁、泥化、微细粒的钼铅矿无法回收。
三、发明内容
本发明的目的在于提供一种可以提高钼精矿品位和回收率,减少能耗的高铁泥化钼铅矿的浮选方法。
本发明采用以下技术方案达到上述目的:以六偏磷酸钠作为分散剂,氢氧化钠作矿浆pH调整剂,用硫化钠进行硫化脱铅,硫酸铜作活化剂,煤油作疏水剂,异戊基黄药作钼铅矿捕收剂。
浮选时矿浆pH值为9-10.5;浮选过程中,将矿石磨至矿物单体解离后,加入分散剂六偏磷酸钠至搅拌桶中,然后加氢氧化钠和硫化钠调节pH,再加硫酸铜活化钼矿物,最后加捕收剂煤油和异戊基黄药、起泡剂2号油进行捕收。
药剂用量(g/t)为:
六偏磷酸钠 粗选 50~80 精选20~50
硫化钠 粗选 6000~9000 精选1000~4000
硫酸铜 粗选 60~90 精选0~10
异戊基黄药 粗选 250~300 精选0~50
煤油 粗选 60~80 精选10~40
2号油 粗选 0~60 精选0~10
使用时,先配制成以下浓度(重量%):
氢氧化钠 10~20%水溶液
六偏磷酸钠 1~5%水溶液
硫化钠 10~20%水溶液
硫酸铜 1~5%水溶液
异戊基黄药 1~5%水溶液
煤油 直接原液添加
2号油 直接原液添加
当硫化钠用量为10000g/t,矿浆pH为10左右时,钼铅矿浮选指标好;添加六偏磷酸钠能够改善矿浆的分散性能,但用量过大时,则对钼铅矿有抑制作用;采用硫酸铜能够活化部分难浮钼铅矿,提高了钼的回收率;用异戊基黄药作钼铅矿捕收剂对提高钼精矿品位和回收率效果都比较好,添加煤油能够增强钼铅矿表面的疏水性,提高钼的回收率。
本发明的具体优点在于:
1、采用本发明能够对低品位高铁钼铅矿能够有效回收,并获得较高钼精矿品位和回收率。在给矿钼品位为0.5~0.67%条件下,经过一次粗选两次扫选及四次精选,钼精矿品位可达13~16.8%,回收率达到71~76%。
2、本发明占地面积少,流程简单,能耗低。
四、具体实施方式
下面以实施例对本发明作进一步详细描述:
实施例1
1.矿物原料:
贵州某矿,处理量为100吨/天,其矿石中钼含量为0.92%,铅3.9%、三氧化二铁含量达到29%,铁主要以褐铁矿形式存在,矿石泥化严重。物相分析表明钼主要是以钼铅矿(PbMoO4)形式存在,铅与钼的比值达到4.23(钼铅矿中钼与铅的比值为2.16),说明矿石的铅除了以钼铅矿形式存在外,还含有部分氧化铅,物相分析这部分氧化铅主要是白铅矿。
2.浮选药剂及操作步骤:
药剂制度:
用氢氧化钠调矿浆到pH 9-10.5、六偏磷酸钠100g/t,硫化钠10kg/t,硫酸铜67g/t,异戊基黄药用量330g/t,煤油100g/t,2号油60g/t。
使用时,先配制成以下浓度(重量%):
氢氧化钠 10%水溶液
六偏磷酸钠 1%水溶液
硫化钠 20%水溶液
硫酸铜 5%水溶液
异戊基黄药 5%水溶液
煤油 直接原液添加
2号油 直接原液添加
操作步骤:
先将矿石磨至矿物单体解离后,加入分散剂六偏磷酸钠至浮选机中,然后加氢氧化钠和硫化钠后再加硫酸铜活化钼矿物,最后加煤油和异戊基黄药及2号油进行捕收。
按上述工艺参数进行了一年100t/d工业扩大试验,表明采用以上工艺和药剂条件能够有效将泥化严重、含铁高的钼铅矿进行浮选回收。在给矿钼品位为0.67%条件下,经过一次粗选两次扫选及四次精选,浮选精矿钼品位为16.8%,回收率为达到76%。
实施例2
1.矿物原料
贵州某矿,矿石中钼含量为0.54%,铅2.63%、三氧化二铁含量达到17%,铁主要以褐铁矿形式存在,矿石泥化严重。钼主要是以钼铅矿(PbMoO4)形式存在,其他矿物除了有少量铜外,还有少量的锌矿,物相分析这两部分矿物均为氧化矿。
2.浮选药剂及操作步骤:
药剂制度:
用氢氧化钠调矿浆到pH 9.5、六偏磷酸钠300g/t,硫化钠8kg/t,硫酸铜120g/t,异戊基黄药用量210g/t,煤油80g/t,2号油70g/t。
使用时,先配制成以下浓度(重量%):
氢氧化钠 20%水溶液
六偏磷酸钠 5%水溶液
硫化钠 10%水溶液
硫酸铜 1%水溶液
异戊基黄药 1%水溶液
煤油 直接原液添加
2号油 直接原液添加
操作步骤同实施例1。
按照上述浮选工艺参数进行了八个月200t/d的工业试验,表明采用上述工艺和药剂条件能够有效将泥化严重、含铁高的钼铅矿进行浮选回收。在给矿钼品位为0.54%条件下,经过一次粗选两次扫选及四次精选,浮选精矿钼品位为13.65%,回收率为71.58%。
Claims (2)
1、一种高铁泥化钼铅矿浮选方法,其特征在于:
(1)采用六偏磷酸钠作分散剂,氢氧化钠作矿浆pH调整剂,以硫化钠进行硫化脱铅,硫酸铜作活化剂,煤油作疏水剂,异戊基黄药和煤油混合作钼铅矿捕收剂,2号油作起泡剂,
(2)浮选时矿浆pH值为9-10.5,
(3)浮选过程中,将矿石磨至矿物单体解离后,加入分散剂六偏磷酸钠至搅拌桶中,然后加氢氧化钠和硫化钠调节pH,再加硫酸铜活化钼矿物,最后加捕收剂煤油和异戊基黄药、起泡剂2号油进行捕收,
(4)药剂用量(g/t)为:
六偏磷酸钠 粗选 50~80 精选20~50
硫化钠 粗选 6000~9000 精选1000~4000
硫酸铜 粗选 60~90 精选0~10
异戊基黄药 粗选 250~300 精选0~50
煤油 粗选 60~80 精选10~40
2号油 粗选 60 精选10。
2、根据权利要求1所述的高铁泥化钼铅矿浮选方法,其特征在于使用时,先配制成以下浓度(重量%):
氢氧化钠 10~20%水溶液
六偏磷酸钠 1~5%水溶液
硫化钠 10~20%水溶液
硫酸铜 1~5%水溶液
异戊基黄药 1~5%水溶液
煤油 直接原液添加
2号油 直接原液添加。