WO2025127084A1 - ゴム組成物及びポリフェニレンエーテルの使用方法 - Google Patents

ゴム組成物及びポリフェニレンエーテルの使用方法 Download PDF

Info

Publication number
WO2025127084A1
WO2025127084A1 PCT/JP2024/043903 JP2024043903W WO2025127084A1 WO 2025127084 A1 WO2025127084 A1 WO 2025127084A1 JP 2024043903 W JP2024043903 W JP 2024043903W WO 2025127084 A1 WO2025127084 A1 WO 2025127084A1
Authority
WO
WIPO (PCT)
Prior art keywords
polyphenylene ether
rubber composition
mass
carbon atoms
parts
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
PCT/JP2024/043903
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
洋之 市野
雄大 田中
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Asahi Kasei Corp
Asahi Chemical Industry Co Ltd
Original Assignee
Asahi Kasei Corp
Asahi Chemical Industry Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Asahi Kasei Corp, Asahi Chemical Industry Co Ltd filed Critical Asahi Kasei Corp
Priority to KR1020267015277A priority Critical patent/KR20260088604A/ko
Priority to CN202480073655.3A priority patent/CN122270518A/zh
Priority to JP2025563547A priority patent/JPWO2025127084A1/ja
Publication of WO2025127084A1 publication Critical patent/WO2025127084A1/ja
Anticipated expiration legal-status Critical
Pending legal-status Critical Current

Links

Classifications

    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B60—VEHICLES IN GENERAL
    • B60C—VEHICLE TYRES; TYRE INFLATION; TYRE CHANGING; CONNECTING VALVES TO INFLATABLE ELASTIC BODIES IN GENERAL; DEVICES OR ARRANGEMENTS RELATED TO TYRES
    • B60C1/00—Tyres characterised by the chemical composition or the physical arrangement or mixture of the composition
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J3/00—Processes of treating or compounding macromolecular substances
    • C08J3/24—Crosslinking, e.g. vulcanising, of macromolecules
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K3/00—Use of inorganic substances as compounding ingredients
    • C08K3/02—Elements
    • C08K3/06—Sulfur
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K3/00—Use of inorganic substances as compounding ingredients
    • C08K3/34—Silicon-containing compounds
    • C08K3/36—Silica
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L71/00—Compositions of polyethers obtained by reactions forming an ether link in the main chain; Compositions of derivatives of such polymers
    • C08L71/08—Polyethers derived from hydroxy compounds or from their metallic derivatives
    • C08L71/10—Polyethers derived from hydroxy compounds or from their metallic derivatives from phenols
    • C08L71/12—Polyphenylene oxides
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L9/00—Compositions of homopolymers or copolymers of conjugated diene hydrocarbons

Definitions

  • the present invention relates to a rubber composition and a method for using polyphenylene ether.
  • Rubber compositions have conventionally been widely used in the field of industrial parts, such as automobile components, tire components, packings, gaskets, sealing materials, vibration-proof rubber, vibration-isolating rubber, vibration-damping materials, shoe outsoles, shoe midsoles, and the like.
  • a tire tread as a tire component is required to have a higher level of reduced rolling resistance (fuel economy) and improved steering stability on wet road surfaces (wet grip performance).
  • fuel economy and wet grip performance are generally in a trade-off relationship, and it is not easy to achieve both.
  • Patent Document 1 discloses a rubber composition containing a rubber component and a farnesene resin in a specific ratio, and describes that the rubber composition has good ice grip performance and abrasion resistance, and has little change in hardness.
  • Patent Document 1 shows an improvement in tire grip, it is not sufficient, and there is no mention of fuel economy. Therefore, further improvements are desired from the viewpoint of obtaining a rubber composition with an excellent balance of properties.
  • the present invention was made in consideration of the above problems, and aims to provide a rubber composition that combines high levels of processability, fuel efficiency, wet grip properties, and ice grip properties.
  • the polyphenylene ether (A) contains a repeating unit derived from a phenol represented by the following formula (1) and a repeating unit derived from a phenol represented by the following formula (2):
  • the rubber composition according to [1] characterized in that, relative to a total of 100 mol% of the repeating units of the following formulas (1) and (2), a content ratio of the repeating unit derived from phenol of the following formula (1) is 31 mol% or more and 100 mol%, and a content ratio of the repeating unit derived from phenol of the following formula (2) is more than 0 mol% and 69 mol% or less.
  • R 13 is a saturated or unsaturated hydrocarbon group having 15 carbon atoms which may be substituted, and R 11 and R 12 are each independently any one of a hydrogen atom, a linear saturated hydrocarbon group having 1 to 12 carbon atoms, and a substituent represented by the following formula (3):
  • R 31 each independently represents a linear alkyl group having 1 to 8 carbon atoms which may be substituted, or atoms contained in two R 31 are bonded to each other to form a cyclic alkyl group having 1 to 8 carbon atoms
  • R 32 each independently represents an alkylene group having 1 to 8 carbon atoms which may be substituted
  • b each independently represents 0 or 1
  • R 33 each represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms which may be substituted, or a phenyl group which may be substituted.
  • each R 21 is independently an optionally substituted saturated hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted ary
  • a method for using a polyphenylene ether comprising using a polyphenylene ether having a glass transition temperature of ⁇ 100° C. or higher and lower than 0° C. as measured by differential scanning calorimetry (DSC) as a raw material for a tire composition.
  • a method for producing vulcanized rubber comprising the steps of: A step of mixing a diene-based elastomer (B) with a polyphenylene ether (A) having a glass transition temperature measured by differential scanning calorimetry (DSC) of ⁇ 100° C. or higher and lower than 0° C. to obtain a rubber composition; and vulcanizing the rubber composition,
  • the polyphenylene ether (A) has an unsaturated hydrocarbon group in a side chain
  • a method for producing a vulcanized rubber comprising crosslinking the diene elastomer (B) and the polyphenylene ether (A).
  • a rubber composition can be obtained which achieves high levels of processability, fuel economy, wet grip performance and ice grip performance all at the same time. Furthermore, the present invention can provide a new method for using polyphenylene ether.
  • the present embodiment an embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail.
  • the following embodiment is an example for explaining the present invention, and the present invention is not limited to only this embodiment.
  • the present invention can be practiced by appropriately modifying it within the scope of its gist.
  • the rubber composition of the present embodiment contains a polyphenylene ether (A) and a diene-based elastomer (B).
  • the rubber composition of the present embodiment contains polyphenylene ether, and the polyphenylene ether has a glass transition temperature measured by DSC of -100°C or higher and lower than 0°C.
  • the compatibility between the polyphenylene ether and the diene elastomer is estimated from the high tan ⁇ of the rubber composition of the present embodiment. If the compatibility is good, the high tan ⁇ of the rubber composition of the present embodiment is not significantly lower than the high tan ⁇ of a rubber composition to which the polyphenylene ether is not added.
  • the polyphenylene ether (A) may be used alone or in combination of two or more kinds.
  • the glass transition temperature measured by DSC for example, it is possible to lower the glass transition temperature by performing molecular design that weakens the interactions between polymer chains and makes the polymer chains easier to move.
  • the measuring device for measuring the differential scanning calorimetry is not particularly limited, and a commercially available device can be used.
  • a commercially available device can be used.
  • the "DSC250" manufactured by TA Instruments can be used as the differential scanning calorimetry device.
  • the polyphenylene ether (A) contains a repeating unit derived from phenol of the following formula (1).
  • a polyphenylene ether containing a repeating unit derived from phenol of the following formula (1) multiple reaction points of the polyphenylene ether are present on side chains protruding from the molecular main chain, so there is less steric hindrance and the frequency of collisions between molecules increases, resulting in high reactivity.
  • the vulcanization speed can be increased, the vulcanization adhesion during retreading is improved, and further, the rubber composition tends to have excellent fuel efficiency, wet grip properties, ice grip properties, tensile strength, and tensile elongation.
  • R 13 is a saturated or unsaturated hydrocarbon group having 15 carbon atoms which may be substituted, and R 11 and R 12 are each independently at least one selected from the group consisting of a hydrogen atom, a linear saturated hydrocarbon group having 1 to 12 carbon atoms, and a substituent represented by formula (3).
  • R 11 and R 12 are each independently at least one selected from a hydrogen atom, a methyl group, an ethyl group, and a substituent represented by formula (3). More preferably, R 11 is a substituent represented by formula (3). Particularly preferably, R 11 is a substituent represented by formula (3) and R 12 is a hydrogen atom.
  • each R 31 is independently a linear alkyl group having 1 to 8 carbon atoms which may be substituted, or atoms contained in two R 31 are bonded to each other to form a cyclic alkyl group having 1 to 8 carbon atoms; each R 32 is independently an alkylene group having 1 to 8 carbon atoms which may be substituted; each b is independently 0 or 1; and R 33 is a hydrogen atom, an alkyl group having 1 to 8 carbon atoms which may be substituted, or a phenyl group which may be substituted.
  • the substituent represented by the above formula (3) is preferably a group containing a secondary and/or tertiary carbon, such as an isopropyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a tert-amyl group, a 2,2-dimethylpropyl group, a cyclohexyl group, and groups in which the hydrogen of the terminal hydrocarbon group in these groups is replaced with a phenyl group. More preferably, the substituent represented by the above formula (3) is a tert-butyl group or a cyclohexyl group, and even more preferably a tert-butyl group. Furthermore, the atoms contained therein may be bonded to each other to form a ring structure.
  • a secondary and/or tertiary carbon such as an isopropyl group, an isobutyl group, a sec-butyl group, a tert-butyl
  • R 11 is a t-butyl group and R 12 is a hydrogen atom.
  • R 13 is a saturated or unsaturated hydrocarbon group having 15 carbon atoms which may be substituted, and preferably R 13 is represented by C 15 H 31-2n (wherein each n is independently an integer of 0 to 3).
  • the polyphenylene ether may contain a repeating unit derived from a phenol of formula (2) in addition to the repeating unit derived from a phenol of formula (1).
  • each R 21 is independently an optionally substituted saturated hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom
  • each R 22 is independently a hydrogen atom, an optionally substituted saturated hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom.
  • each R 21 is preferably independently a saturated hydrocarbon group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms, more preferably a methyl group or a phenyl group, and even more preferably a methyl group.
  • each R 22 is preferably independently a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms, more preferably a hydrogen atom or a methyl group.
  • the two R 22 may be the same or different.
  • Preferred embodiments include an embodiment in which both of R 22 are hydrogen atoms, or an embodiment in which one is a hydrogen atom and the other is a hydrocarbon group having 1 to 6 carbon atoms (more preferably a methyl group).
  • the structure of the polyphenylene ether can be identified by analyzing the polyphenylene ether by a technique such as NMR or mass spectrometry.
  • a technique such as NMR or mass spectrometry.
  • FD-MS field desorption mass spectrometry
  • the structure of the polyphenylene ether can be determined by an analytical method such as 1 H NMR.
  • the content of the repeating unit derived from phenol of the above formula (1) is preferably 31 mol % or more and 100 mol % or less
  • the content of the repeating unit derived from phenol of the above formula (2) is preferably more than 0 mol % and 69 mol % or less, relative to 100 mol % in total of the repeating unit derived from phenol of the above formula (1) and the repeating unit derived from phenol of the above formula (2).
  • the content ratio of the repeating unit derived from phenol of the above formula (1) to the total 100 mol % of the repeating unit derived from phenol of the above formula (1) and the repeating unit derived from phenol of the above formula (2) is preferably 40 mol % or more, more preferably 50 mol % or more, and even more preferably 60 mol % or more. Meanwhile, there is no upper limit for the content ratio of the above formula (1).
  • the content of the repeating unit derived from the phenol of the formula (2) can be appropriately selected depending on the application. For example, when it is desired to improve heat resistance, it is preferable that the repeating unit derived from the phenol of the formula (2) is more.
  • the total molar ratio of the repeating units derived from phenol of the above formula (1) and the repeating units derived from phenol of the above formula (2) relative to 100 mol % of the polyphenylene ether of the present embodiment is preferably 80 mol % or more, more preferably 90 mol % or more, and even more preferably 95 mol % or more, and may be 100 mol %.
  • the molar ratio of the repeating unit derived from phenol of the above formula (1) and the molar ratio of the repeating unit derived from phenol of the above formula (2) relative to the total of 100 mol % of the repeating unit derived from phenol of the above formula (1) and the repeating unit derived from phenol of the above formula (2) can be determined using an analytical method such as 1 H-NMR or 13 C-NMR, and more specifically, can be measured by the method described in the Examples below.
  • the polyphenylene ether (A) may also contain a repeating unit derived from phenol of the following formula (4).
  • the Tg of the rubber composition can be lowered, thereby further improving the wet grip property and ice grip property.
  • R 41 , R 42 , and R 43 are each independently an organic group having 7 to 25 carbon atoms and having one or more atoms selected from the group consisting of a linear saturated hydrocarbon group having 1 to 12 carbon atoms, and an optionally substituted nitrogen atom, oxygen atom, and sulfur atom, and at least one of R 41 , R 42 , and R 43 is an organic group having 7 to 25 carbon atoms and having one or more atoms selected from the group consisting of a nitrogen atom, an oxygen atom, and a sulfur atom.
  • At least one of R 41 , R 42 and R 43 is preferably an organic group having a sulfur atom and 8 to 20 carbon atoms, and more preferably an organic group having a sulfur atom and 9 to 15 carbon atoms.
  • the phenol of the above formula (4) is preferably 4,6-bis(octylthiomethyl)-o-cresol or 4,6-bis(dodecylthiomethyl)-o-cresol.
  • the polyphenylene ether of the present embodiment may contain a repeating unit derived from a phenol of the above formula (2), in addition to the repeating unit derived from a phenol of the formula (4).
  • the content of the repeating unit derived from phenol of the above formula (4) is preferably 7 to 50 mol % and the content of the repeating unit derived from phenol of the above formula (2) is preferably 50 to 93 mol % relative to the total 100 mol % of the repeating unit derived from phenol of the above formula (4) and the repeating unit derived from phenol of the above formula (2).
  • the content ratio of the repeating unit derived from phenol of the above formula (4) relative to the total 100 mol% of the repeating unit derived from phenol of the above formula (4) and the repeating unit derived from phenol of the above formula (2) is preferably 7 mol% or more, more preferably 10 mol% or more, and even more preferably 15 mol% or more.
  • the content ratio of the repeating units derived from phenol of the above formula (4) relative to the total of 100 mol% of the repeating units derived from phenol of the above formula (4) and the repeating units derived from phenol of the above formula (2) is preferably 50 mol% or less, more preferably 30 mol% or less, and even more preferably 20 mol% or less.
  • the total molar ratio of the repeating units derived from phenol of the above formula (4) and the repeating units derived from phenol of the above formula (2) relative to 100 mol% of the polyphenylene ether of this embodiment is preferably 80 mol% or more, more preferably 90 mol% or more, even more preferably 95 mol% or more, and may be 100 mol%.
  • the polyphenylene ether in the present embodiment may have at least one partial structure selected from the group consisting of a partial structure of the following formula (10), a partial structure of the following formula (11), a partial structure of the following formula (12), and a partial structure of the following formula (13).
  • R 4 is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated hydrocarbon may have a substituent within the range in which the total carbon number of R 4 is 1 to 10.
  • R 5 is a saturated or unsaturated divalent hydrocarbon group having 1 to 10 carbon atoms, which may have a substituent such that the total number of carbon atoms in R 5 is 1 to 10
  • R 6 is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, which may have a substituent such that the total number of carbon atoms in R 6 is 1 to 10.
  • At least one partial structure selected from the group consisting of the partial structure of the above formula (10), the partial structure of the above formula (11), the partial structure of the above formula (12), and the partial structure of the above formula (13) may be introduced by a modification process described below, and may be directly bonded to the oxygen atom of the hydroxyl group contained in the polyphenylene ether.
  • the viscosity of the polyphenylene ether (A) at 80°C is preferably less than 1,000,000 cP, more preferably less than 500,000 cP, and even more preferably less than 300,000 cP, from the viewpoint of processability of the resulting rubber composition.
  • the means for adjusting the viscosity is not particularly limited, and can be adjusted, for example, by the molecular weight of the polyphenylene ether (A) or the content ratio of the repeating unit in the polyphenylene ether (A).
  • the number average molecular weight (Mn) of the polyphenylene ether (A) is preferably less than 5,500, more preferably less than 5,000, and even more preferably less than 4,500, from the viewpoint of processability of the resulting rubber composition.
  • the reduced viscosity ( ⁇ sp/c) of the polyphenylene ether (A), measured using an Ubbelohde type viscometer in a chloroform solution having a concentration of 0.5 g/dL at 30° C., is preferably 0.03 to 0.90 dL/g, and more preferably 0.05 to 0.60 dL/g, from the viewpoint of processability of the resulting rubber composition.
  • the rubber composition By melting the polyphenylene ether during kneading to prepare the rubber composition, it is possible to improve the compatibility with the filler contained in the rubber composition described below, and the rubber composition tends to have excellent fuel economy, wet grip properties, ice grip properties, tensile strength, and tensile elongation.
  • Examples of the phenol of the above formula (1) include 3-pentadecylphenol, commercially available cardanol, modified 3-pentadecylphenol obtained by introducing a linear saturated hydrocarbon group having 1 to 12 carbon atoms or a substituent represented by the above formula (3) into 3-pentadecylphenol, and modified cardanol obtained by introducing a linear saturated hydrocarbon group having 1 to 12 carbon atoms or a substituent represented by the above formula (3) into commercially available cardanol.
  • Examples of the phenol of the above formula (2) include 2,6-dimethylphenol, 2-methyl-6-ethylphenol, 2,6-diethylphenol, 2-ethyl-6-n-propylphenol, 2-methyl-6-chlorophenol, 2-methyl-6-bromophenol, 2-methyl-6-n-propylphenol, 2-ethyl-6-bromophenol, 2-methyl-6-n-butylphenol, 2,6-di-n-propylphenol, 2-ethyl-6-chlorophenol, 2-methyl-6-phenylphenol, 2,6-diphenylphenol, 2-methyl-6-tolylphenol, 2,6-ditolylphenol, 2,3,6-trimethylphenol, 2,3-diethyl-6-n-propylphenol, 2,3,6-tributylphenol, 2,6-di-n-butyl-3-methylphenol, 2,6-dimethyl-3-n-butylphenol, and 2,6-dimethyl-3-t-butylphenol.
  • the polyphenylene ether (A) can be obtained by a method including at least a step of oxidatively polymerizing a monovalent raw material phenol containing the phenol of the formula (4) above.
  • the step of oxidatively polymerizing is preferably a step of oxidatively polymerizing raw material phenols containing the phenol of the formula (4) above and the phenol of the formula (2) above.
  • the phenol of the above formula (4) commercially available products such as 4,6-bis(octylthiomethyl)-o-cresol and 4,6-bis(dodecylthiomethyl)-o-cresol are preferred.
  • the polyphenylene ether preferably contains a biomass-derived monomer. If even a part of the rubber composition contains a biomass-derived raw material, the amount of fossil fuel used can be reduced compared to the conventional method.
  • the degree of biomass in the polyphenylene ether can be obtained by measuring the content of carbon derived from biomass by radiocarbon (C14) measurement. Carbon dioxide in the atmosphere contains a certain proportion of C14 (105.5 pMC), and it is known that the C14 content in plants that grow by absorbing carbon dioxide from the atmosphere, such as corn, is also about 105.5 pMC. It is also known that fossil fuels contain almost no C14. Therefore, the proportion of carbon derived from biomass can be calculated by measuring the proportion of C14 contained in the total carbon atoms in the polyphenylene ether.
  • biomass refers to living organisms, particularly plants such as wood, bamboo, coconuts, and cashew nut shells; polysaccharides such as cellulose, starch, and pullulan; oligosaccharides such as dextrin, sucrose, and maltose; monosaccharides such as fructose and glucose; and plant components such as lignin and hemicellulose. It also includes, for example, wood waste from the wood and pulp industries, thinning materials, demolition materials from buildings, agricultural waste such as rice straw, rice husks, and bagasse, various lignocelluloses, and even resource rice, old rice, and food industry waste. In this specification, unless otherwise specified, these substances are collectively referred to as biomass.
  • a biomass-derived phenolic compound is cardanol obtained from cashew nut shell liquid (CNSL).
  • Cashews are naturally occurring tropical plants, and their fruit, cashew nuts, contains protein and carbohydrates and is used as food in snacks such as mixed nuts and in cooking.
  • Cashew nuts are a natural fruit, and when harvested as a resource, they are a renewable biomass resource.
  • CNSL is an oily liquid whose main component is cardanol and is contained in the shells of cashew nuts, which are the inedible part of the nuts that is obtained as a by-product when harvesting natural cashew nuts, which are used for food.
  • Natural CNSL is a mixture of anacardic acid, cardanol, cardol, and 2-methylcardol, and each component is an organic compound consisting of a phenol moiety and a linear hydrocarbon moiety R, as shown in the following formulas (2) to (5).
  • the linear hydrocarbon portion R of each component has one of the structures shown below. That is, there are four types, each having 0, 1, 2, or 3 unsaturated bonds, and an average of two double bonds.
  • Each of the compounds represented by formulas (2) to (5) may be one type alone or two or more types with different R.
  • the main component of natural CNSL is anacardic acid, as shown in formula (2) above.
  • This natural CNSL is decarboxylated for industrial use, and cardanol, as shown in formula (3) above, becomes the main component.
  • the proportions of each component in industrial CNSL vary depending on the place of origin, but are generally cardanol (3): 70-80% by mass, cardol (4): 15-25% by mass, and 2-methylcardol (5): 5% by mass or less.
  • the proportion of cardanol can be increased by distilling industrial CNSL.
  • the CNSL used as the raw material for phenol production in this embodiment may be a product in which the unsaturated bonds in the linear hydrocarbon moiety R in the side chain of each component shown in the above formulas (2) to (5) have been hydrogenated (hydrogenated) in advance, or may be chemically modified (denatured).
  • an aromatic solvent that is a good solvent for polyphenylene ether can be used as the polymerization solvent in the oxidative polymerization step.
  • a good solvent for polyphenylene ether is a solvent that can dissolve polyphenylene ether.
  • solvents include aromatic hydrocarbons such as benzene, toluene, xylene (including o-, m-, and p-isomers) and ethylbenzene, halogenated hydrocarbons such as chlorobenzene and dichlorobenzene, nitro compounds such as nitrobenzene, etc.
  • the polymerization catalyst used in this embodiment may be a known catalyst system that can generally be used for the production of polyphenylene ether.
  • Commonly known catalyst systems include those that consist of a transition metal ion having oxidation-reduction ability and an amine compound that can form a complex with the transition metal ion, such as a catalyst system consisting of a copper compound and an amine compound, a catalyst system consisting of a manganese compound and an amine compound, and a catalyst system consisting of a cobalt compound and an amine compound. Since the polymerization reaction proceeds efficiently under slightly alkaline conditions, a small amount of alkali or an additional amine compound may be added to this.
  • the polymerization catalyst preferably used in the present embodiment is a catalyst containing a copper compound, a halogen compound, and an amine compound as catalyst components, and more preferably a catalyst containing a diamine compound represented by the following formula (14) as the amine compound:
  • R 14 , R 15 , R 16 , and R 17 are each independently a hydrogen atom or a linear or branched alkyl group having 1 to 6 carbon atoms, but are not all simultaneously a hydrogen atom.
  • R 18 is a linear or methyl-branched alkylene group having 2 to 5 carbon atoms.
  • Suitable copper compounds include cuprous compounds, cupric compounds, and mixtures thereof.
  • cupric compounds include cupric chloride, cupric bromide, cupric sulfate, and cupric nitrate.
  • cuprous compounds include cuprous chloride, cuprous bromide, and cuprous sulfate.
  • particularly preferred metal compounds are cuprous chloride, cupric chloride, cuprous bromide, and cupric bromide.
  • These copper salts may be synthesized at the time of use from oxides (e.g., cuprous oxide), carbonates, hydroxides, and the like and the corresponding halogens or acids. A method that is often used is to mix the cuprous oxide exemplified above with hydrogen halide (or a solution of hydrogen halide) to prepare the copper salt.
  • the halogen compounds include, for example, hydrogen chloride, hydrogen bromide, hydrogen iodide, sodium chloride, sodium bromide, sodium iodide, potassium chloride, potassium bromide, potassium iodide, tetramethylammonium chloride, tetramethylammonium bromide, tetramethylammonium iodide, tetraethylammonium chloride, tetraethylammonium bromide, tetraethylammonium iodide, etc. These can be used as aqueous solutions or solutions using appropriate solvents. These halogen compounds can be used alone as components, or in combination of two or more types. Preferred halogen compounds are aqueous solutions of hydrogen chloride and hydrogen bromide.
  • the amount of these compounds used is not particularly limited, but is preferably in the range of 2 to 20 times, more preferably 2 to 15 times, and even more preferably 2 to 10 times, the number of moles of halogen atoms relative to the number of moles of copper atoms.
  • the amount of copper atoms used is preferably in the range of 0.02 to 0.6 mol, more preferably 0.02 to 0.5 mol, and even more preferably 0.02 to 0.4 mol, per 100 mol of the phenol compound added to the polymerization reaction.
  • examples of the diamine compound of the catalyst component are listed below.
  • N,N,N',N'-tetramethylethylenediamine N,N,N'-trimethylethylenediamine, N,N'-dimethylethylenediamine, N,N-dimethylethylenediamine, N-methylethylenediamine, N,N,N',N'-tetraethylethylenediamine, N,N,N'-triethylethylenediamine, N,N'-diethylethylenediamine, N,N-diethylethylenediamine, N-ethylethylenediamine, N,N-dimethyl-N'-ethylethylenediamine, N,N'-dimethyl-N-ethylethylenediamine, N-n-propylethylenediamine, N,N'-n-propylethylenediamine, N-i-propylethylenediamine, N,N'-i-propylethylenediamine, N-i-propylethylenediamine, N,N'-i
  • a preferred diamine compound for this embodiment is one in which the number of carbon atoms in the alkylene group connecting two nitrogen atoms is 2 or 3.
  • the amount of these diamine compounds used is not particularly limited, but is preferably in the range of 0.01 mol to 10 mol, more preferably in the range of 0.01 mol to 8.0 mol, and even more preferably in the range of 0.01 mol to 6 mol, relative to 100 mol of the phenol compound added to the polymerization reaction.
  • the polymerization catalyst may contain a primary amine and a secondary monoamine as components.
  • secondary monoamines include, but are not limited to, dimethylamine, diethylamine, di-n-propylamine, di-i-propylamine, di-n-butylamine, di-i-butylamine, di-t-butylamine, dipentylamines, dihexylamines, dioctylamines, didecylamines, dibenzylamines, methylethylamine, methylpropylamine, methylbutylamine, cyclohexylamine, N-phenylmethanolamine, N-phenylethanolamine, N-phenylpropanolamine, N-(m-methylphenyl)ethanolamine, N-(p-methylphenyl)ethanolamine, N-(2',6'-dimethylphenyl)ethanolamine, N-(p-chlorophenyl)ethanolamine, N-e
  • the polymerization catalyst may also contain a tertiary monoamine compound as a component thereof.
  • Tertiary monoamine compounds are aliphatic tertiary amines including alicyclic tertiary amines. Examples include trimethylamine, triethylamine, tripropylamine, tributylamine, triisobutylamine, dimethylethylamine, dimethylpropylamine, allyldiethylamine, dimethyl-n-butylamine, diethylisopropylamine, and N-methylcyclohexylamine. These tertiary monoamines may be used alone or in combination of two or more. The amount of these used is not particularly limited, but is preferably 15 moles or less, more preferably 14 moles or less, and even more preferably 13 moles or less, per 100 moles of the phenol compound added to the polymerization reaction.
  • a surfactant that has been known to have an effect of improving polymerization activity.
  • examples of such surfactants include trioctylmethylammonium chloride, known under the trade names Aliquat 336 and Capriquat.
  • the amount of the surfactant used is preferably within a range not exceeding 0.1% by mass with respect to the total amount (100% by mass) of the polymerization reaction mixture.
  • the oxygen-containing gas in the polymerization of this embodiment in addition to pure oxygen, a mixture of oxygen and an inert gas such as nitrogen in any ratio, air, or a mixture of air and an inert gas such as nitrogen in any ratio can be used.
  • Normal pressure is sufficient for the pressure in the system during the polymerization reaction, but reduced or increased pressure can be used as necessary.
  • the polymerization temperature is not particularly limited, but if it is too low, the reaction does not proceed easily, and if it is too high, the reaction selectivity may decrease and gel may be formed, so it is in the range of 0 to 60°C, preferably 10 to 40°C.
  • the polymerization can also be carried out in a poor solvent such as alcohol.
  • the post-treatment method after the polymerization reaction is completed.
  • an acid such as hydrochloric acid or acetic acid, or ethylenediaminetetraacetic acid (EDTA) and its salts, nitrilotriacetic acid and its salts, etc.
  • EDTA ethylenediaminetetraacetic acid
  • the method of removing the dihydric phenol by-product generated by the polymerization of polyphenylene ether can be performed using a conventionally known method. If the metal ions, which are the catalyst, are substantially deactivated as described above, the mixture can be decolorized simply by heating it.
  • a method of adding a required amount of a known reducing agent is also possible. Examples of known reducing agents include hydroquinone and sodium dithionite.
  • water may be added to extract the compound that has deactivated the copper catalyst, and liquid-liquid separation may be performed into an organic phase and an aqueous phase, after which the aqueous phase may be removed to remove the copper catalyst from the organic phase.
  • This liquid-liquid separation step is not particularly limited, but examples include methods such as static separation and separation using a centrifuge. To promote the liquid-liquid separation, a known surfactant or the like may be used.
  • the organic phase containing the polyphenylene ether after liquid-liquid separation may be concentrated and dried by volatilizing the solvent.
  • the temperature is preferably 200° C. or lower, more preferably 180° C. or lower, and even more preferably 160° C. or lower.
  • the method of increasing the drying temperature is preferable from the viewpoint of production efficiency. It is preferable to use a dryer with a mixing function for the drying process. Examples of mixing functions include stirring and rolling dryers. This allows the processing volume to be increased, and productivity to be maintained at a high level.
  • the total amount of solvent remaining in the polyphenylene ether (A) is preferably less than 1 mass % of the total amount, more preferably less than 0.6 mass %, even more preferably less than 0.5 mass %, particularly preferably less than 0.3 mass %, and particularly preferably less than 0.1 mass %.
  • the polyphenylene ether (A) preferably has a residual metal catalyst content of less than 1.0 ppm, more preferably less than 0.5 ppm.
  • the total amount of amines remaining in the polyphenylene ether (A) is preferably less than 1.0% by mass of the total amount, more preferably less than 0.5% by mass, and even more preferably less than 0.1% by mass.
  • the residual amine amount referred to here is the amount of amines excluding amines chemically bonded to the polyphenylene ether out of the total amount of amines contained in the polyphenylene ether after the drying step is completed.
  • the polyphenylene ether (A) preferably has a residual monomer content of less than 5 mass %, more preferably less than 4 mass %, and even more preferably less than 3 mass %.
  • the polyphenylene ether (A) can also be produced by a redistribution reaction in which a polyphenylene ether derived from a phenol of the above formula (2) is equilibrated with a phenol compound of the above formula (1) in the presence of an oxidizing agent. Redistribution reactions are known in the art and are described, for example, in U.S. Pat. No. 3,496,236 to Cooper et al. and U.S. Pat. No. 5,880,221 to Liska et al.
  • the method for introducing functional groups into the hydroxyl groups of unmodified polyphenylene ether is not limited, and for example, it can be obtained by a reaction between the hydroxyl groups of unmodified polyphenylene ether and a carboxylic acid having a carbon-carbon double bond (hereinafter referred to as carboxylic acid) to form an ester bond.
  • carboxylic acid a carboxylic acid having a carbon-carbon double bond
  • the ester bond can be formed by a variety of known methods. For example, a. reaction between a carboxylic acid halide and a hydroxyl group at the end of the polymer, b. formation of an ester bond by reaction with a carboxylic acid anhydride, c. direct reaction with a carboxylic acid, d. a method using an ester exchange reaction, etc.
  • the reaction of a with an carboxylic acid halide is one of the most common methods. Chlorides and bromides are commonly used as carboxylic acid halides, but other halogens can also be used.
  • the reaction can be either a direct reaction with a hydroxyl group or a reaction with an alkali metal salt of a hydroxyl group. Since a direct reaction between a carboxylic acid halide and a hydroxyl group generates an acid such as hydrogen halide, a weak base such as an amine can be used in the presence of the reaction to trap the acid.
  • the reaction mixture may be washed with water, an acidic or alkaline aqueous solution to remove by-products such as amine salts, or the polymer solution may be dropped into a poor solvent such as an alcohol and the target product may be recovered by reprecipitation. After washing the polymer solution, the solvent may be distilled off under reduced pressure to recover the polymer.
  • the method for producing the modified polyphenylene ether is not limited to the method for producing the polyfunctional modified polyphenylene ether of the present embodiment described above, and the order and number of the above-mentioned oxidative polymerization step, copper extraction and by-product removal step, liquid-liquid separation step, and concentration/drying step may be appropriately adjusted.
  • the polyphenylene ether of the present embodiment may be obtained by oxidatively polymerizing 3-pentadecylphenol or commercially available cardanol, and optionally 2,6-dimethylphenol as the phenol of the above formula (2), and then introducing at least one partial structure selected from the group consisting of the above formulas (10), (11), (12), and (13) into the obtained polyphenylene ether.
  • the polyphenylene ether of the present embodiment may be obtained by oxidatively polymerizing 3-pentadecylphenol or commercially available cardanol as the phenol of the above formula (1), and optionally 2,6-dimethylphenol as the phenol of the above formula (2). Further, for example, the polyphenylene ether of the present embodiment may be obtained by oxidative polymerization of modified 3-pentadecylphenol or modified cardanol as the phenol of the above formula (1), and optionally 2,6-dimethylphenol as the phenol of the above formula (2), and then introducing at least one partial structure selected from the group consisting of the above formulas (10), (11), (12), and (13) into the obtained polyphenylene ether.
  • the polyphenylene ether of the present embodiment may be prepared by using 4,6-bis(octylthiomethyl)-o-cresol, 4,6-bis( dodecylthiomethyl)-o-cresol and, optionally, 2,6-dimethylphenol as the phenol of the above formula (2), and then introducing at least one partial structure selected from the group consisting of the above formulas (10), (11), (12), and (13) into the obtained polyphenylene ether.
  • the diene elastomer (B) is at least one selected from synthetic rubber and natural rubber.
  • the synthetic rubber and natural rubber may be used alone or in combination of two or more.
  • the diene elastomer (B) of the present embodiment preferably has a weight average molecular weight of 100,000 or more, more preferably 120,000 or more, and even more preferably 150,000 or more.
  • the synthetic rubber examples include styrene butadiene rubber (hereinafter also referred to as "SBR"), butadiene rubber, isoprene rubber, butyl rubber, halogenated butyl rubber, ethylene propylene diene rubber, butadiene acrylonitrile polymer rubber, chloroprene rubber, etc., and among these, SBR, isoprene rubber, and butadiene rubber are preferred, and SBR and butadiene rubber are more preferred. These may be used alone or in combination of two or more.
  • the diene elastomer of the present embodiment does not include a polymer block consisting of only vinyl aromatic monomer units.
  • SBR -Styrene butadiene rubber
  • the SBR may be any of those commonly used in tires, but specifically, the styrene content is preferably 0.1 to 70 mass%, more preferably 5 to 60 mass%, and even more preferably 5 to 50 mass%, and the vinyl content is preferably 0.1 to 80 mass%, and more preferably 5 to 70 mass%.
  • the vinyl content of SBR refers to the content of monomer units having a vinyl group among all butadiene-derived units contained in SBR.
  • the vinyl content of the diene elastomer (B) refers to the content of monomer units actually having a vinyl group relative to the total amount of monomer units that may have a vinyl group due to the bonding form.
  • potassium salts or sodium salts of fatty acids such as capric acid, lauric acid, myristic acid, palmitic acid, oleic acid, and stearic acid.
  • water is usually used, and may contain a water-soluble organic solvent such as methanol or ethanol to the extent that stability during polymerization is not impaired.
  • persulfates such as ammonium persulfate and potassium persulfate, organic peroxides, hydrogen peroxide, etc. can be used.
  • a chain transfer agent can also be used.
  • chain transfer agent examples include mercaptans such as t-dodecyl mercaptan and n-dodecyl mercaptan; carbon tetrachloride, thioglycolic acid, diterpene, terpinolene, ⁇ -terpinene, and ⁇ -methylstyrene dimer.
  • the temperature of the emulsion polymerization can be appropriately selected depending on the type of radical polymerization initiator used, but is usually preferably 0 to 100°C, more preferably 0 to 60°C.
  • the polymerization method may be either continuous polymerization or batch polymerization.
  • the polymerization reaction can be terminated by adding a polymerization terminator.
  • polymerization terminator examples include amine compounds such as isopropylhydroxylamine, diethylhydroxylamine, and hydroxylamine; quinone compounds such as hydroquinone and benzoquinone, and sodium nitrite. After the polymerization reaction is terminated, an anti-aging agent may be added as necessary.
  • the polymerization reaction is stopped, unreacted monomers are removed from the obtained latex as necessary, and then the polymer is coagulated using a salt such as sodium chloride, calcium chloride, or potassium chloride as a coagulant, and an acid such as nitric acid or sulfuric acid is added as necessary to adjust the pH of the coagulation system to a predetermined value, and then the dispersion solvent is separated to recover the polymer as crumbs.
  • the crumbs are washed with water, dehydrated, and dried with a band dryer or the like to obtain E-SBR.
  • the latex and an extender oil that has been previously made into an emulsified dispersion may be mixed as necessary to recover the polymer as an oil-extended rubber.
  • alkali metals and alkaline earth metals are preferred, and alkali metals are more preferred.
  • organic alkali metal compounds are more preferably used.
  • the solvent include aliphatic hydrocarbons such as n-butane, n-pentane, isopentane, n-hexane, n-heptane, and isooctane; alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane; and aromatic hydrocarbons such as benzene and toluene. It is preferable to use these solvents in a range in which the monomer concentration is 1 to 50% by mass.
  • organic alkali metal compound examples include organic monolithium compounds such as n-butyllithium, sec-butyllithium, t-butyllithium, hexyllithium, phenyllithium, and stilbenelithium; polyfunctional organic lithium compounds such as dilithiomethane, 1,4-dilithiobutane, 1,4-dilithio-2-ethylcyclohexane, and 1,3,5-trilithiobenzene; sodium naphthalene, and potassium naphthalene.
  • organic lithium compounds are preferred, and organic monolithium compounds are more preferred.
  • the amount of the organic alkali metal compound used is appropriately determined depending on the molecular weight of the required S-SBR.
  • the organic alkali metal compound can also be used as an organic alkali metal amide by reacting it with a secondary amine such as dibutylamine, dihexylamine, or dibenzylamine.
  • the polar compound is not particularly limited as long as it is a compound that is usually used in anionic polymerization to adjust the microstructure of the butadiene moiety and the distribution of styrene in the polymer chain without inactivating the reaction.
  • the polar compound examples include ether compounds such as dibutyl ether, tetrahydrofuran, and ethylene glycol diethyl ether; tertiary amines such as tetramethylethylenediamine and trimethylamine; alkali metal alkoxides, and phosphine compounds.
  • the temperature of the polymerization reaction is usually in the range of -80 to 150°C, preferably 0 to 100°C, and more preferably 30 to 90°C.
  • the polymerization mode may be either batch polymerization or continuous polymerization.
  • the composition ratio of styrene and butadiene in the polymerization system is within a specific range.
  • the polymerization reaction can be terminated by adding an alcohol such as methanol or isopropanol as a polymerization terminator.
  • a coupling agent such as tin tetrachloride, tetrachlorosilane, tetramethoxysilane, tetraglycidyl-1,3-bisaminomethylcyclohexane, or 2,4-tolylene diisocyanate that can react with the polymerization active terminal, or a polymerization terminal modifier such as 4,4'-bis(diethylamino)benzophenone or N-vinylpyrrolidone may be added.
  • the solvent can be separated from the polymerization solution by direct drying, steam stripping, etc., to recover the desired S-SBR. Note that, before removing the solvent, the polymerization solution may be mixed with an extender oil and recovered as an oil-extended rubber.
  • Modified styrene butadiene rubber (modified SBR)
  • modified SBR in which a functional group is introduced into SBR may be used.
  • the functional group include an amino group, an alkoxysilyl group, a hydroxy group, an epoxy group, and a carboxyl group.
  • a method for producing modified SBR includes, for example, a method of adding a coupling agent capable of reacting with a polymerization active terminal, such as tin tetrachloride, tetrachlorosilane, dimethyldichlorosilane, dimethyldiethoxysilane, tetramethoxysilane, tetraethoxysilane, 3-aminopropyltriethoxysilane, tetraglycidyl-1,3-bisaminomethylcyclohexane, or 2,4-tolylenediisocyanate, a polymerization terminal modifier, such as 4,4'-bis(diethylamino)benzophenone or N-vinylpyrrolidone, or other modifiers described in JP-A-2011-132298, before adding a polymerization terminator.
  • a coupling agent capable of reacting with a polymerization active terminal such as tin tetrachloride, tet
  • isoprene Rubber for example, commercially available isoprene rubber polymerized using Ziegler catalysts such as titanium tetrahalide-trialkylaluminum, diethylaluminum chloride-cobalt, trialkylaluminum-boron trifluoride-nickel, and diethylaluminum chloride-nickel; lanthanoid rare earth metal catalysts such as triethylaluminum-organic acid neodymium-Lewis acid; or organic alkali metal compounds similar to S-SBR can be used.
  • Ziegler catalysts such as titanium tetrahalide-trialkylaluminum, diethylaluminum chloride-cobalt, trialkylaluminum-boron trifluoride-nickel, and diethylaluminum chloride-nickel
  • lanthanoid rare earth metal catalysts such as triethylaluminum-organic acid neodymium-Lewis acid
  • the vinyl content of the isoprene rubber is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less. If the vinyl content exceeds 50% by mass, fuel economy tends to deteriorate. There is no particular limit to the lower limit of the vinyl content.
  • the glass transition temperature varies depending on the vinyl content, but is preferably -20°C or less, and more preferably -30°C or less.
  • the weight average molecular weight (Mw) of the isoprene rubber is preferably 90,000 to 2,000,000, more preferably 150,000 to 1,500,000.
  • the isoprene rubber may have a branched structure or a polar functional group formed by using a polyfunctional modifier, such as tin tetrachloride, silicon tetrachloride, an alkoxysilane having an epoxy group in the molecule, or an amino group-containing alkoxysilane.
  • a polyfunctional modifier such as tin tetrachloride, silicon tetrachloride, an alkoxysilane having an epoxy group in the molecule, or an amino group-containing alkoxysilane.
  • butadiene Rubber for example, commercially available butadiene rubber polymerized using Ziegler catalysts such as titanium tetrahalide-trialkylaluminum, diethylaluminum chloride-cobalt, trialkylaluminum-boron trifluoride-nickel, diethylaluminum chloride-nickel; lanthanoid rare earth metal catalysts such as triethylaluminum-organic acid neodymium-Lewis acid, or organic alkali metal compounds as with S-SBR can be used.
  • Ziegler catalysts such as titanium tetrahalide-trialkylaluminum, diethylaluminum chloride-cobalt, trialkylaluminum-boron trifluoride-nickel, diethylaluminum chloride-nickel
  • lanthanoid rare earth metal catalysts such as triethylaluminum-organic acid neodymium-Lewis acid, or organic alkali metal compounds as
  • the weight average molecular weight (Mw) of the butadiene rubber is preferably 90,000 to 2,000,000, more preferably 150,000 to 1,500,000.
  • the butadiene rubber may have a branched structure or a polar functional group formed by using a polyfunctional modifier, such as tin tetrachloride, silicon tetrachloride, an alkoxysilane having an epoxy group in the molecule, or an amino group-containing alkoxysilane.
  • butyl rubber halogenated butyl rubber, ethylene propylene diene rubber, butadiene acrylonitrile polymer rubber, chloroprene rubber, etc.
  • SBR isoprene rubber
  • butadiene rubber there is no particular limitation on the manufacturing method of these, and commercially available products can be used.
  • Natural Rubber examples of natural rubbers used in the diene elastomer (B) include TSRs such as SMR, SIR, and STR, natural rubbers commonly used in the tire industry such as RSS, and modified natural rubbers such as high-purity natural rubber, epoxidized natural rubber, hydroxylated natural rubber, hydrogenated natural rubber, and grafted natural rubber.
  • TSRs such as SMR, SIR, and STR
  • RSS natural rubbers commonly used in the tire industry
  • modified natural rubbers such as high-purity natural rubber, epoxidized natural rubber, hydroxylated natural rubber, hydrogenated natural rubber, and grafted natural rubber.
  • SMR20, STR20, and RSS#3 are preferred from the viewpoints of less variation in quality and ease of availability. These may be used alone or in combination of two or more.
  • the polyphenylene ether (A) is preferably contained in an amount of 0.01 to 65 parts by mass, more preferably 0.01 to 60 parts by mass, and even more preferably 0.01 to 55 parts by mass, per 100 parts by mass of the diene-based elastomer (B).
  • a rubber composition containing more than 65 parts by mass of the polyphenylene ether (A) per 100 parts by mass of the diene-based elastomer (B) tends to have inferior fuel economy, wet grip performance, and ice grip performance.
  • the rubber composition of the present embodiment may contain other components such as a filler, a silane coupling agent, a vulcanizing agent, a vulcanization accelerator, and a vulcanization aid in addition to the above-mentioned polyphenylene ether and diene-based elastomer, as long as the effects of the present invention are not impaired.
  • the filler is not particularly limited as long as it is one that is commonly used in rubber compositions, but from the viewpoint of improving the dispersibility of the filler in the rubber composition, and from the viewpoint of improving fuel efficiency and grip, it is preferable that the filler contains at least one type selected from silica and carbon black.
  • silica examples include wet silica (hydrated silicic acid), dry silica (anhydrous silicic acid), calcium silicate, and aluminum silicate. Among them, wet silica is preferred from the viewpoint of further improving the fuel economy and grip of the rubber composition. These may be used alone or in combination of two or more.
  • the average particle size of the silica is preferably 0.5 nm or more, more preferably 2 nm or more, even more preferably 5 nm or more, even more preferably 8 nm or more, even more preferably 10 nm or more, and preferably 200 nm or less, more preferably 150 nm or less, even more preferably 100 nm or less, even more preferably 50 nm or less, even more preferably 30 nm or less, and even more preferably 20 nm or less.
  • the average particle size of the silica can be determined by measuring the diameter of the particles using a transmission electron microscope and calculating the average value.
  • Carbon Black examples of the carbon black that can be used include furnace black, channel black, thermal black, acetylene black, and ketjen black. Among these, furnace black is preferred from the viewpoint of improving the fuel economy and grip of the rubber composition.
  • furnace black products that can be used in this embodiment include, for example, "Diablack” manufactured by Mitsubishi Chemical Corporation and “Seat” manufactured by Tokai Carbon Co., Ltd.
  • commercially available acetylene black products include, for example, “Denka Black” manufactured by Denki Kagaku Kogyo Co., Ltd.
  • Commercially available ketjen black products include, for example, "ECP600JD” manufactured by Lion Corporation.
  • the average particle size of the carbon black is preferably 5 nm or more, more preferably 10 nm or more, even more preferably 15 nm or more, and is preferably 100 nm or less, more preferably 80 nm or less, even more preferably 70 nm or less, and even more preferably 60 nm or less, from the viewpoint of improving the fuel efficiency performance, moldability, wear resistance, and grip of the rubber composition.
  • the average particle size of the carbon black can be determined by measuring the diameter of the particles using a transmission electron microscope and calculating the average value.
  • the particle size of the carbon black can be adjusted by pulverization or the like.
  • a high-speed rotary pulverizer (hammer mill, pin mill, cage mill), various ball mills (rolling mill, vibration mill, planetary mill), stirring mill (bead mill, attritor, flow tube type mill, annular mill), etc.
  • the carbon black may be subjected to an acid treatment using nitric acid, sulfuric acid, hydrochloric acid, or a mixture of these acids, or a surface oxidation treatment using a heat treatment in the presence of air.
  • the carbon black may be subjected to a heat treatment at 2,000 to 3,000° C. in the presence of a graphitization catalyst.
  • a graphitization catalyst boron, boron oxides (e.g., B2O2, B2O3, B4O3, B4O5, etc.), boron oxoacids (e.g., orthoboric acid, metaboric acid, tetraboric acid, etc.) and salts thereof, boron carbides (e.g., B4C, B6C, etc.), boron nitride (BN), and other boron compounds are preferably used.
  • fillers other than silica and carbon black may be contained for the purpose of improving the mechanical strength of the rubber composition and improving the production cost by compounding the filler as an extender.
  • examples of fillers other than silica and carbon black that can be used include organic fillers and inorganic fillers such as clay, talc, mica, calcium carbonate, magnesium hydroxide, aluminum hydroxide, barium sulfate, titanium oxide, glass fiber, fibrous fillers, and glass balloons. These fillers may be used alone or in combination of two or more.
  • the content of the silica is, from the viewpoint of improving the fuel efficiency and ice grip of a tire using the rubber composition for tire treads as a part thereof, preferably 10 parts by mass or more, more preferably 20 parts by mass or more, even more preferably 25 parts by mass or more, even more preferably 30 parts by mass or more, even more preferably 35 parts by mass or more, even more preferably 40 parts by mass or more, even more preferably 45 parts by mass or more, and is preferably 115 parts by mass or less, more preferably 90 parts by mass or less, even more preferably 80 parts by mass or less, even more preferably 75 parts by mass or less, even more preferably 70 parts by mass or less, and even more preferably 65 parts by mass or less, per 100 parts by mass of the diene-based elastomer (B).
  • the content of the carbon black is, from the viewpoint of improving the fuel economy performance, abrasion resistance, and gripping properties of the rubber composition, preferably 5 parts by mass or more, more preferably 10 parts by mass or more, even more preferably 15 parts by mass or more, even more preferably 20 parts by mass or more, even more preferably 25 parts by mass or more, even more preferably 30 parts by mass or more, and is preferably 75 parts by mass or less, more preferably 65 parts by mass or less, even more preferably 55 parts by mass or less, even more preferably 45 parts by mass or less, even more preferably 40 parts by mass or less, and even more preferably 35 parts by mass or less, per 100 parts by mass of the diene-based elastomer (B).
  • the rubber composition of the present embodiment may further contain a silane coupling agent.
  • silane coupling agent include sulfide compounds, mercapto compounds, vinyl compounds, amino compounds, glycidoxy compounds, nitro compounds, and chloro compounds.
  • the sulfide compounds include, for example, bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(3-trimethoxysilylpropyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, 3-trimethoxysilylpropyl Examples include silylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-triethoxysilylpropyl-N,N-dimethylthiocarbam
  • Examples of the mercapto-based compounds include 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 2-mercaptoethyltrimethoxysilane, and 2-mercaptoethyltriethoxysilane.
  • vinyl compounds examples include vinyltriethoxysilane and vinyltrimethoxysilane.
  • amino compounds examples include 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-(2-aminoethyl)aminopropyltriethoxysilane, and 3-(2-aminoethyl)aminopropyltrimethoxysilane.
  • Examples of the glycidoxy compounds include ⁇ -glycidoxypropyltriethoxysilane, ⁇ -glycidoxypropyltrimethoxysilane, ⁇ -glycidoxypropylmethyldiethoxysilane, and ⁇ -glycidoxypropylmethyldimethoxysilane.
  • nitro-based compounds examples include 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane.
  • silane coupling agents may be used alone or in combination of two or more.
  • silane coupling agents containing sulfur such as sulfide-based compounds and mercapto-based compounds, are preferred from the viewpoint of their large reinforcing effect.
  • the rubber composition of the present embodiment may contain a vulcanization aid.
  • the vulcanization aid include fatty acids such as stearic acid, metal oxides such as zinc oxide, and fatty acid metal salts such as zinc stearate. These may be used alone or in combination of two or more.
  • the content thereof is preferably 0.1 to 15 parts by mass, and more preferably 1 to 10 parts by mass, based on 100 parts by mass of the diene elastomer (B).
  • antioxidant examples include hindered phenol compounds, phosphorus compounds, lactone compounds, and hydroxyl compounds.
  • the rubber composition of this embodiment may contain a crosslinking agent in addition to the vulcanizing agent.
  • crosslinking agents include oxygen, organic peroxides, phenolic resins, amino resins, quinone and quinone dioxime derivatives, halogen compounds, aldehyde compounds, alcohol compounds, epoxy compounds, metal halides, organometallic halides, and silane compounds. These may be used alone or in combination of two or more.
  • the amount of crosslinking agent is preferably 0.1 to 10 parts by mass per 100 parts by mass of the diene elastomer (B).
  • the method for producing the rubber composition for tire treads is not limited as long as it can uniformly mix the above-mentioned components.
  • Examples of the method for uniformly mixing include a tangential or intermeshing internal mixer such as a kneader-ruder, a Brabender, a Banbury mixer, or an internal mixer, a single screw extruder, a twin screw extruder, a mixing roll, and a roller, and the mixture can usually be mixed at a temperature in the range of 30 to 270°C.
  • the glass transition temperature of polyphenylene ether was measured using a differential scanning calorimeter DSC250 (TA Instruments). In a nitrogen atmosphere, the sample was heated from -120 to 250°C at a temperature increase rate of 10°C per minute, then cooled to -120°C at a rate of 20°C per minute, and the glass transition temperature was then measured at a temperature increase rate of 10°C per minute.
  • the temperature of the reaction solution was lowered to 40°C, and toluene (300g) was added to the reaction solution. Furthermore, 5% aqueous sodium hydroxide solution (27g) was dropped. Ion-exchanged water (320g) was added, the temperature of the reaction solution was raised to 70°C, and after stirring for 30 minutes, the organic layer was recovered using a separatory funnel. Ion-exchanged water (760g) was added to the recovered organic layer, the temperature of the reaction solution was raised to 70°C, and after stirring for 30 minutes, it was left to stand. The organic layer was recovered using a separatory funnel. The washed organic layer was concentrated using a rotary evaporator to obtain a pale yellow oily modified cardanol (370g).
  • Cardanol raw material 1 H-NMR (CDCl 3 ) ⁇ 7.15-7.10 (m, 1H), 6.78-6.73 (m, 1H), 6.68-6.62 (m, 2H), 5.88-5.77 (m, 0.37H), 5.50-5.29 (m, 3.44H), 5.10-4.95 (m, 0.80H), 4.81-4.64 ( m, 1H), 2.88-2.75 (m, 2.14H), 2.55 (t, 2.13H), 2.08-1.98 (m, 3.31H), 1.69-1.53 (m, 3.15H), 1.51-1.12 (m, 14.10H), 0.94-0.85 (m, 1.95H) Modified cardanol (product): 1 H-NMR (CDCl 3 ) ⁇ 7.16 (m, 1H), 6.78-6.73 (m, 1H), 6.68-6.62 (m, 2H), 5.88-5.77 (m, 0.37H), 5.50-5.29 (m, 3.44H), 5.10-4.95 (m,
  • each component was mixed with the materials and methods described below to prepare a rubber composition sample.
  • the components other than the polyphenylene ether (A) were uniformly mixed as shown below.
  • a closed mixer (capacity: 0.5 L) equipped with a temperature control device was used, and in the first stage of kneading, materials other than sulfur and the vulcanization accelerator were kneaded under the conditions of a filling rate of 65% and a rotor rotation speed of 50 to 90 rpm.
  • the temperature of the closed mixer was controlled, and the discharge temperature was 150 to 160°C to obtain a compound.
  • the mixture obtained above was cooled to room temperature and then mixed again to improve the dispersion of the reinforcing filler.
  • the discharge temperature of the mixture was adjusted to 150 to 160°C by controlling the temperature of the mixer.
  • a vulcanization accelerator and sulfur were added and kneaded using an open roll set at 70° C. to obtain an unvulcanized rubber composition.
  • the rubber composition was molded and vulcanized in a vulcanizing press at 160° C. for a predetermined vulcanization time to obtain a vulcanized rubber composition.
  • the vulcanization time was set to a value obtained by adding 5 minutes to the 90% vulcanization time of the unvulcanized rubber composition.
  • iene-based elastomer (B) Styrene-butadiene rubber (SBR (HS265 manufactured by Asahi Kasei Corporation): 70 parts by mass)
  • Silica product name "Ultrasil 7000GR” manufactured by Evonik Degussa, nitrogen adsorption specific surface area 170 m 2 /g
  • Silane coupling agent Evonik Degussa Corporation, "Si75", bis(triethoxysilylpropyl)disulfide: 6.0 parts by mass Carbon black (Tokai Carbon Corporation, Seest KH (N339)): 5.0 parts by mass Softener (TDAE oil (H&R Corporation, product name "V500”)): 32 parts by mass Zinc oxide: 2.5 parts by mass Stearic acid: 2.0 parts by mass Wax, Sunnock: 1.5 parts by mass Antiaging agent (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine): 2.0 parts by mass Sulfur: 2.2 parts by mass
  • Ice grip property (tan ⁇ at -20°C)
  • the vulcanized rubber composition samples obtained in the Examples and Comparative Examples were measured in a torsion mode at -20°C, a frequency of 10 Hz, and a strain of 1% using a viscoelasticity tester "ARES" manufactured by Rheometrics Scientific, Inc. Tan ⁇ was used as an index of ice gripping properties.
  • the value of tan ⁇ was determined according to the following index, with a larger value indicating better ice gripping properties.
  • ⁇ : tan ⁇ at -20°C is 0.302 or more
  • tan ⁇ at -20°C is 0.275 or more and less than 0.302
  • tan ⁇ at -20°C is less than 0.275
  • Vulcanization speed The rubber composition obtained above was measured for a vulcanization curve at a temperature of 160°C using a rotorless vulcanization tester in accordance with JIS K6300-2 "Method of determining vulcanization characteristics using a vibration vulcanization tester".
  • the vertical axis represents the torque obtained, and the horizontal axis represents the vulcanization time.
  • the vulcanization time required from the start of vulcanization until the torque reached the maximum value MH was taken as tc (max).
  • Performance Balance Considering the fuel economy (tan ⁇ at 50°C), wet grip performance (tan ⁇ at 0°C), and ice grip performance (tan ⁇ at -20°C) of the vulcanized rubber composition samples obtained in the Examples and Comparative Examples, the performance balance was judged using the following indexes. Good: Good for fuel economy, wet grip, and ice grip ⁇ : ⁇ in any one of fuel economy, wet grip, and ice grip ⁇ : ⁇ in any one of fuel economy, wet grip, and ice grip
  • Examples 1 to 16 are excellent in hardness, tensile strength, breaking elongation, processability, fuel economy, wet grip performance, ice grip performance and vulcanization speed, and have a good balance of the above properties. It was found that Comparative Examples 1 to 7 were inferior to the Examples in any one of hardness, tensile strength, breaking elongation, processability, fuel economy, wet grip performance, ice grip performance, and vulcanization speed, or in the balance thereof.
  • the rubber composition of the present embodiment has industrial applicability as a material for tires such as truck tires, bus tires, automobile tires, motorcycle tires, off-road tires, and aircraft tires; materials for tire components such as treads, sidewalls, chafer strips, tire rubber layers, reinforcing cord coating materials, and cushion layers; industrial parts such as fibers, thin films, laminates, automobile parts, and medical parts; molded articles such as equipment housings, consumer products, and packaging; tire curing bladders, inner tubes, air sleeves, hoses, belts such as conveyor belts or automobile belts, solid tires, tires for retreading, footwear components, rollers for graphic arts applications, vibration isolation devices, pharmaceutical equipment, adhesives, caulking materials, sealants, glazing compounds, protective coatings, air cushions, air springs, air bellows, accumulator bags, and materials for various bladders for liquid storage and curing methods, automobile suspension bumpers, automobile exhaust hangers, and molded rubber parts such as body mounts.
  • tires such as truck tires, bus tires, automobile tires, motorcycle tires, off-

Landscapes

  • Chemical & Material Sciences (AREA)
  • Health & Medical Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Medicinal Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Organic Chemistry (AREA)
  • Engineering & Computer Science (AREA)
  • Mechanical Engineering (AREA)
  • Polyethers (AREA)
  • Compositions Of Macromolecular Compounds (AREA)
PCT/JP2024/043903 2023-12-15 2024-12-11 ゴム組成物及びポリフェニレンエーテルの使用方法 Pending WO2025127084A1 (ja)

Priority Applications (3)

Application Number Priority Date Filing Date Title
KR1020267015277A KR20260088604A (ko) 2023-12-15 2024-12-11 고무 조성물 및 폴리페닐렌에테르의 사용 방법
CN202480073655.3A CN122270518A (zh) 2023-12-15 2024-12-11 橡胶组合物和聚苯醚的使用方法
JP2025563547A JPWO2025127084A1 (cg-RX-API-DMAC7.html) 2023-12-15 2024-12-11

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2023-212526 2023-12-15
JP2023212526 2023-12-15

Publications (1)

Publication Number Publication Date
WO2025127084A1 true WO2025127084A1 (ja) 2025-06-19

Family

ID=96057465

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2024/043903 Pending WO2025127084A1 (ja) 2023-12-15 2024-12-11 ゴム組成物及びポリフェニレンエーテルの使用方法

Country Status (4)

Country Link
JP (1) JPWO2025127084A1 (cg-RX-API-DMAC7.html)
KR (1) KR20260088604A (cg-RX-API-DMAC7.html)
CN (1) CN122270518A (cg-RX-API-DMAC7.html)
WO (1) WO2025127084A1 (cg-RX-API-DMAC7.html)

Citations (13)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US3496236A (en) 1966-05-03 1970-02-17 Gen Electric Equilibration of poly-(1,4-phenylene ethers)
JPH0940809A (ja) * 1995-07-14 1997-02-10 Pirelli Coordinamento Pneumatici Spa タイヤ用の加硫可能なゴム組成物
US5880221A (en) 1997-02-14 1999-03-09 General Electric Company Redistribution of polyphenylene ethers and polyphenylene ethers with novel structure
WO2001000702A1 (fr) * 1999-06-29 2001-01-04 Japan As Represented By Secretary Of Agency Of Industrial Science And Technology Composition a base de resine et procede de production de cette composition
JP2001200051A (ja) * 2000-01-17 2001-07-24 Toyo Ink Mfg Co Ltd 硬化性組成物
JP2002194076A (ja) * 2000-12-27 2002-07-10 National Institute Of Advanced Industrial & Technology 硬化性樹脂組成物およびその製造方法
JP2011132298A (ja) 2009-12-22 2011-07-07 Sumitomo Rubber Ind Ltd 変性共重合体、それを用いたゴム組成物および空気入りタイヤ
JP2014218631A (ja) 2013-05-10 2014-11-20 住友ゴム工業株式会社 ゴム組成物及び空気入りタイヤ
JP2021500432A (ja) * 2017-10-20 2021-01-07 コンパニー ゼネラール デ エタブリッスマン ミシュラン 可塑剤としてポリフェニレンエーテル樹脂を含むゴム組成物
CN113087894A (zh) * 2021-04-01 2021-07-09 上海邦高化学有限公司 一种腰果酚聚氧乙烯醚、其制备方法及应用
WO2022244817A1 (ja) * 2021-05-21 2022-11-24 旭化成株式会社 ポリフェニレンエーテル、その製造方法、熱硬化組成物、プリプレグ、及び積層体
JP2024134377A (ja) * 2023-03-20 2024-10-03 旭化成株式会社 樹脂組成物、硬化体及びその製造方法、封止剤、接着剤、並びに、解体性接着剤
JP2025001935A (ja) * 2023-06-21 2025-01-09 旭化成株式会社 樹脂組成物及びその製造方法

Patent Citations (13)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US3496236A (en) 1966-05-03 1970-02-17 Gen Electric Equilibration of poly-(1,4-phenylene ethers)
JPH0940809A (ja) * 1995-07-14 1997-02-10 Pirelli Coordinamento Pneumatici Spa タイヤ用の加硫可能なゴム組成物
US5880221A (en) 1997-02-14 1999-03-09 General Electric Company Redistribution of polyphenylene ethers and polyphenylene ethers with novel structure
WO2001000702A1 (fr) * 1999-06-29 2001-01-04 Japan As Represented By Secretary Of Agency Of Industrial Science And Technology Composition a base de resine et procede de production de cette composition
JP2001200051A (ja) * 2000-01-17 2001-07-24 Toyo Ink Mfg Co Ltd 硬化性組成物
JP2002194076A (ja) * 2000-12-27 2002-07-10 National Institute Of Advanced Industrial & Technology 硬化性樹脂組成物およびその製造方法
JP2011132298A (ja) 2009-12-22 2011-07-07 Sumitomo Rubber Ind Ltd 変性共重合体、それを用いたゴム組成物および空気入りタイヤ
JP2014218631A (ja) 2013-05-10 2014-11-20 住友ゴム工業株式会社 ゴム組成物及び空気入りタイヤ
JP2021500432A (ja) * 2017-10-20 2021-01-07 コンパニー ゼネラール デ エタブリッスマン ミシュラン 可塑剤としてポリフェニレンエーテル樹脂を含むゴム組成物
CN113087894A (zh) * 2021-04-01 2021-07-09 上海邦高化学有限公司 一种腰果酚聚氧乙烯醚、其制备方法及应用
WO2022244817A1 (ja) * 2021-05-21 2022-11-24 旭化成株式会社 ポリフェニレンエーテル、その製造方法、熱硬化組成物、プリプレグ、及び積層体
JP2024134377A (ja) * 2023-03-20 2024-10-03 旭化成株式会社 樹脂組成物、硬化体及びその製造方法、封止剤、接着剤、並びに、解体性接着剤
JP2025001935A (ja) * 2023-06-21 2025-01-09 旭化成株式会社 樹脂組成物及びその製造方法

Also Published As

Publication number Publication date
JPWO2025127084A1 (cg-RX-API-DMAC7.html) 2025-06-19
CN122270518A (zh) 2026-06-23
KR20260088604A (ko) 2026-06-12

Similar Documents

Publication Publication Date Title
KR102550882B1 (ko) 타이어용 고무 조성물
US11034821B2 (en) Rubber compositions
KR102550282B1 (ko) 타이어용 고무 조성물
US11590799B2 (en) Heavy-duty tire rubber compositions and tires
US11970561B2 (en) Modified liquid diene polymer and rubber composition
KR102550883B1 (ko) 중하중 타이어용 고무 조성물 및 타이어
KR102550283B1 (ko) 고그립 타이어용 고무 조성물
US20190194429A1 (en) Rubber compositions
KR102542093B1 (ko) 고그립 타이어용 고무 조성물
KR20210088674A (ko) 고무 조성물
CA3074203C (en) Tire rubber compositions
WO2025018211A1 (ja) タイヤトレッド用ゴム組成物およびタイヤトレッド

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 24903737

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2025563547

Country of ref document: JP

Kind code of ref document: A

WWE Wipo information: entry into national phase

Ref document number: 2025563547

Country of ref document: JP

ENP Entry into the national phase

Ref document number: 1020267015277

Country of ref document: KR

Free format text: ST27 STATUS EVENT CODE: A-0-1-A10-A15-NAP-PA0105 (AS PROVIDED BY THE NATIONAL OFFICE)

WWE Wipo information: entry into national phase

Ref document number: 1020267015277

Country of ref document: KR

WWP Wipo information: published in national office

Ref document number: 1020267015277

Country of ref document: KR