WO2024203249A1 - 正極合材、リチウムイオン電池及び正極合材の製造方法 - Google Patents

正極合材、リチウムイオン電池及び正極合材の製造方法 Download PDF

Info

Publication number
WO2024203249A1
WO2024203249A1 PCT/JP2024/009414 JP2024009414W WO2024203249A1 WO 2024203249 A1 WO2024203249 A1 WO 2024203249A1 JP 2024009414 W JP2024009414 W JP 2024009414W WO 2024203249 A1 WO2024203249 A1 WO 2024203249A1
Authority
WO
WIPO (PCT)
Prior art keywords
solid electrolyte
mixing step
positive electrode
mixture
added
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2024/009414
Other languages
English (en)
French (fr)
Inventor
大和 羽二生
悠 石原
雄太 藤井
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Idemitsu Kosan Co Ltd
Original Assignee
Idemitsu Kosan Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Idemitsu Kosan Co Ltd filed Critical Idemitsu Kosan Co Ltd
Priority to JP2025510245A priority Critical patent/JPWO2024203249A1/ja
Publication of WO2024203249A1 publication Critical patent/WO2024203249A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Abstract

硫黄系活物質及び固体電解質を含み、CuKα線を利用した粉末X線回折において、2θ=15.1±0.8°に回折ピークAを、29.8±0.8°に回折ピークBを有し、元素としてP及びBを有する、正極合材。

Description

正極合材、リチウムイオン電池及び正極合材の製造方法
 本発明は、正極合材、リチウムイオン電池及び正極合材の製造方法に関する。
 具体的には、本発明は、優れた可逆放電容量を発揮できる正極合材、リチウムイオン電池及び正極合材の製造方法に関する。
 リチウムイオン電池等に用いられる硫黄系正極合材においては、硫黄を導電助剤及び固体電解質と複合化することで、絶縁性である硫黄の反応を十分に生起することができる。ここで、硫黄系正極合材の固体電解質としては、Li6PS5Clが用いられている(特許文献1)。
 一方で、硫黄系正極合材の用途ではないが、Li2S-P2S5-LiBH4固体電解質が報告されている(非特許文献1)。
特開2020-161288号公報
A.Sakuda et al., ACS OMEGA 3 (2018) 5453-5458
 本発明者らは、硫黄系正極合材の固体電解質としてLi2S-P2S5-LiBH4の使用を試みた。ところが、通常の方法で製造した正極合材は、可逆放電容量が十分に得られなかった。
 本発明の目的の1つは、優れた可逆放電容量を発揮できる正極合材、リチウムイオン電池及び正極合材の製造方法を提供することである。
 Li2S-P2S5-LiBH4は硫黄系正極合材の固体電解質としては不適と思われたが、本発明者らは検討を続けた。その結果、可逆放電容量が十分に得られない正極合材について粉末X線回折(XRD)で分析したところ、Li2S-P2S5-LiBH4固有のピークが消失していることがわかった。また、このピークの消失が、正極合材を製造する際の混合操作に起因することもわかった。
 このような知見に基づいて、本発明者らはさらに鋭意検討し、Li2S-P2S5-LiBH4を使用する場合であっても、特定の方法で製造した特定の正極合材が、優れた可逆放電容量を有することを見出した。また、そのような正極合材はLi2S-P2S5-LiBH4固有のピークを保持していることもわかった。
 本発明によれば、以下の正極合材等を提供できる。
1.硫黄系活物質及び固体電解質を含み、
 CuKα線を利用した粉末X線回折において、2θ=15.1±0.8°に回折ピークAを、29.8±0.8°に回折ピークBを有し、
 元素としてP及びBを有する、
 正極合材。
2.前記回折ピークAの半値幅が0.5°以上である、1に記載の正極合材。
3.炭素材料である導電助剤を含み、電子顕微鏡画像のエネルギー分散型X線分光法による元素分析において、炭素とリンのマッピングの重複率が45%以上である、1又は2に記載の正極合材。
4.硫黄系活物質に固体電解質を添加して混合処理することで第1混合物を得る第1混合工程と、前記第1混合物にさらなる固体電解質を添加して混合処理することで第2混合物を得る第2混合工程とを含み、前記第2混合工程で添加する前記固体電解質が固体電解質αを含む製造方法によって得られ、
 前記固体電解質αが、CuKα線を利用した粉末X線回折において、2θ=15.1±0.8°に回折ピークAを、29.8±0.8°に回折ピークBを有し、元素としてP及びBを有する、
 1~3のいずれかに記載の正極合材。
5.前記第2混合工程において前記第1混合工程よりも小さいエネルギーで混合処理する、4に記載の正極合材。
6.前記第1混合工程は、該第1混合工程において添加される前記固体電解質の非晶質化が進行する条件で混合処理し、
 前記第2混合工程は、該第2混合工程において添加される前記固体電解質αの結晶性が消失しない条件で混合処理する、
 4又は5に記載の正極合材。
7.1~6のいずれかに記載の正極合材を含む、リチウムイオン電池。
8.硫黄系活物質に固体電解質を添加して混合処理することで第1混合物を得る第1混合工程と、
 前記第1混合物にさらなる固体電解質を添加して混合処理することで第2混合物を得る第2混合工程とを含み、
 前記第2混合工程で添加する前記固体電解質が固体電解質αを含み、
 前記固体電解質αが、CuKα線を利用した粉末X線回折において、2θ=15.1±0.8°に回折ピークAを、29.8±0.8°に回折ピークBを有し、元素としてP及びBを有する、
 正極合材の製造方法。
9.前記第2混合工程において前記第1混合工程よりも小さいエネルギーで混合処理する、8に記載の正極合材の製造方法。
10.前記第1混合工程は、該第1混合工程において添加される前記固体電解質の非晶質化が進行する条件で混合処理し、
 前記第2混合工程は、該第2混合工程において添加される前記固体電解質αの結晶性が消失しない条件で混合処理する、
 8又は9に記載の正極合材の製造方法。
11.製造された正極合材に含まれる固体電解質αを100質量部としたときに、前記第2混合工程で添加された固体電解質αの割合が50~100質量部である、8~10のいずれかに記載の正極合材の製造方法。
12.前記第1混合工程で添加される固体電解質の総量を100質量部としたときに、前記第1混合工程で添加される前記固体電解質αの量が0~50質量部である、8~11のいずれかに記載の正極合材の製造方法。
13.前記第2混合工程で添加される固体電解質の総量を100質量部としたときに、前記第2混合工程で添加される前記固体電解質αの量が50~100質量部である、8~12のいずれかに記載の正極合材の製造方法。
 本発明によれば、優れた可逆放電容量を発揮できる正極合材、リチウムイオン電池及び正極合材の製造方法を提供することができる。
正極合材粉末の粉末X線回折(XRD)の結果を示す図である。 実施例1のSEM-EDS分析の結果を示す図であり、(a)は画像処理前(平滑化、圧縮及び二値化処理前)、(b)は画像処理後を示す。また、Cは炭素のマッピング、Pはリンのマッピングを示す。 比較例1のSEM-EDS分析の結果を示す図であり、(a)は画像処理前(平滑化、圧縮及び二値化処理前)、(b)は画像処理後を示す。また、Cは炭素のマッピング、Pはリンのマッピングを示す。
 以下、本発明の正極合材、リチウムイオン電池及び正極合材の製造方法について詳述する。
 尚、本明細書において、「x~y」は「x以上、y以下」の数値範囲を表すものとする。数値範囲に関して記載された上限値及び下限値は任意に組み合わせることができる。
1.正極合材
 本発明の一態様に係る正極合材は、硫黄系活物質及び固体電解質を含み、CuKα線を利用した粉末X線回折において、2θ=15.1±0.8°に回折ピークAを、29.8±0.8°に回折ピークBを有し、元素としてP及びBを有する。
 本態様の正極合材によれば、優れた可逆放電容量を発揮できる効果が得られる。
(硫黄系活物質)
 硫黄系活物質としては、特に限定はないが、硫黄、硫化リチウム(Li2S)、多硫化リチウム(Li2Sn:nは1<n≦8を満たす。)、硫化チタン(TiS2)、硫化モリブデン(MoS2)、硫化鉄(FeS、FeS2)、硫化銅(CuS)、硫化ニッケル(Ni3S2)、硫黄含有ポリマー化合物等が挙げられる。
 硫黄としては、特に限定はないが、純度が高いものが好ましい。具体的に、純度は95質量%以上が好ましく、さらに96質量%以上が好ましく、特に、97質量%以上が好ましい。
 硫黄の結晶系は、α硫黄(斜方晶系)、β(単斜晶系)、γ(単斜晶系)、無定形硫黄等が挙げられる。これらは単独でも2種以上でも併用可能である。
(固体電解質α)
 一実施形態において、正極合材は、固体電解質として、CuKα線を利用した粉末X線回折において、2θ=15.1±0.8°に回折ピークAを、29.8±0.8°に回折ピークBを有し、元素としてP及びBを有する固体電解質(「固体電解質α」ともいう)を含む。
 一実施形態において、固体電解質αは、アルジロダイト型固体電解質である。
 一実施形態において、固体電解質αは、元素として、P、B、Li及びSを有する。ここで、固体電解質αは、Bを、BH4として含み得る。
 固体電解質αの製造方法は格別限定されない。
 出発原料としては、リチウム、リン、硫黄、ホウ素等を構成元素として含む2種以上の化合物又は単体を組み合わせて使用することができ、含まれる金属原子に起因するイオン伝導度を発現するものであれば特に制限なく採用することができる。
 リチウム(Li)を含む原料としては、例えば、硫化リチウム(Li2S)、酸化リチウム(Li2O)、炭酸リチウム(Li2CO3)等のリチウム化合物、及びリチウム金属単体等が挙げられる。中でも、リチウム化合物が好ましく、硫化リチウムがより好ましい。
 リン(P)及び硫黄(S)を含む原料としては、例えば、三硫化二リン(P2S3)、五硫化二リン(P2S5)等の硫化リン、リン酸ナトリウム(Na3PO4)等のリン化合物、リン単体及び硫黄単体等が挙げられる。これらの中でも、硫化リンが好ましく、五硫化二リンがより好ましい。五硫化二リン等のリン化合物、リン単体及び硫黄単体は、工業的に製造され、販売されているものであれば、特に限定なく使用することができる。
 ホウ素(B)を含む原料としては、水素化ホウ素リチウム(LiBH4)、水素化ホウ素ナトリウム、四ホウ酸リチウム、メタホウ酸リチウム等が挙げられる。なかでも、水素化ホウ素リチウムが好ましい。
 使用原料の組み合わせとしては、硫化リチウム、五硫化二リン及び水素化ホウ素リチウムが好ましい。
 原料における硫化リチウムと五硫化二リンとのモル比は、65~85:15~35が好ましく、70~80:20~30がより好ましく、72~78:22~28が更に好ましく、75:25が特に好ましい。
 また、水素化ホウ素リチウムの配合量は、硫化リチウム、五硫化二リン及び水素化ホウ素リチウムの合計に対して、25モル%以上、95モル%以下が好ましく、30モル%以上、85モル%以下がより好ましい。
 上記の原料に機械的応力を加えて固体電解質αとする。ここで、「機械的応力を加える」とは、機械的にせん断力や衝撃力等を加えることである。機械的応力を加える手段としては、例えば、遊星型ボールミル、振動ミル、転動ミル等の粉砕機や、混練機等を挙げることができる。
 混合の順序は特に限定されない。例えば、原料として硫化リチウム、五硫化二リン及び水素化ホウ素リチウムを使用した場合、3種の化合物を混合し、上記装置で処理をしてもよく、また、予め、硫化リチウムと五硫化二リンの混合物を処理した後、得られた処理物に水素化ホウ素リチウムを加えて混合処理してもよい。
 固体電解質αは、例えば非特許文献1に記載の方法によっても製造できる。
 一実施形態において、正極合材は、固体電解質として、固体電解質αと、固体電解質α以外の固体電解質とを含む。
(固体電解質α以外の固体電解質)
 固体電解質α以外の固体電解質は格別限定されず、例えば、硫化物固体電解質が挙げられる。
 硫化物固体電解質は、少なくとも硫黄原子を含み、かつ含まれる金属原子に起因するイオン伝導度を発現する固体電解質であり、硫黄原子の他、好ましくはリチウム原子、リン原子を含み、より好ましくはリチウム原子、リン原子及びハロゲン原子を含み、リチウム原子に起因するイオン伝導度を有する固体電解質である。
 一実施形態において、固体電解質は、リチウム原子、リン原子、硫黄原子、臭素原子及びヨウ素原子を含む。この場合、リチウム原子、硫黄原子、リン原子、臭素原子及びヨウ素原子の配合比(モル比)は、格別限定されないが、1.0~1.8:1.0~2.0:0.1~0.8:0.01~0.3:0.01~0.3が好ましく、1.1~1.7:1.2~1.8:0.2~0.6:0.02~0.25:0.02~0.25がより好ましく、1.2~1.6:1.3~1.7:0.25~0.5:0.03~0.2:0.03~0.2がより好ましく、1.35~1.45:1.4~1.7:0.3~0.45:0.04~0.18:0.04~0.18が更に好ましい。
 硫化物固体電解質としては、非晶性硫化物固体電解質であってもよいし、結晶性硫化物固体電解質であってもよい。
(非晶性硫化物固体電解質)
 非晶性硫化物固体電解質としては、少なくとも硫黄原子を含み、含まれる金属原子に起因するイオン伝導度を発現するものであれば特に制限なく採用することができ、代表的なものとしては、例えば、Li2S-P2S5等の硫化リチウムと硫化リンとから構成される、硫黄原子、リチウム原子及びリン原子を含む固体電解質;Li2S-P2S5-LiI、Li2S-P2S5-LiCl、Li2S-P2S5-LiBr、Li2S-P2S5-LiI-LiBr等の、硫化リチウムと硫化リンとハロゲン化リチウムとから構成される固体電解質;更に酸素元素、珪素元素等の他の元素を含む、例えば、Li2S-P2S5-Li2O-LiI、Li2S-SiS2-P2S5-LiI等の固体電解質が好ましく挙げられる。より高いイオン伝導度を得る観点から、Li2S-P2S5-LiI、Li2S-P2S5-LiCl、Li2S-P2S5-LiBr、Li2S-P2S5-LiI-LiBr等の、硫化リチウムと硫化リンとハロゲン化リチウムとから構成される固体電解質が好ましい。
 非晶性硫化物固体電解質を構成する元素の種類は、例えば、ICP発光分光分析装置により確認することができる。
 非晶性硫化物固体電解質が、少なくともLi2S-P2S5を有するものである場合、Li2SとP2S5とのモル比は、化学的安定性が高く、より高いイオン伝導度を得る観点から、30~85:15~70が好ましく、40~80:20~60がより好ましく、45~78:22~55が更に好ましい。
 非晶性硫化物固体電解質が、例えば、Li2S-P2S5-LiI-LiBrである場合、硫化リチウム及び五硫化二リンの含有量の合計は、30~95モル%が好ましく、35~90モル%がより好ましく、40~85モル%が更に好ましい。また、臭化リチウムとヨウ化リチウムとの合計に対する臭化リチウムの割合は、1~99モル%が好ましく、20~90モル%がより好ましく、40~80モル%が更に好ましく、50~70モル%が特に好ましい。
(結晶性硫化物固体電解質)
 結晶性硫化物固体電解質としては、例えば上記の非晶性硫化物固体電解質を結晶化温度以上に加熱して得られる、いわゆるガラスセラミックスであってもよく、以下の結晶構造を有する硫化物固体電解質を採用し得る。
 リチウム原子、硫黄原子及びリン原子を含む結晶性硫化物固体電解質が有し得る結晶構造としては、Li3PS4結晶構造、Li4P2S6結晶構造、Li7PS6結晶構造、Li7P3S11結晶構造、2θ=20.2°近傍及び23.6°近傍にピークを有する結晶構造(例えば、特開2013-16423号公報)等が挙げられる。
 また、リチウム原子、硫黄原子、リン原子及びハロゲン原子を含む結晶性硫化物固体電解質が有し得る結晶構造としては、チオリシコンリージョンII型結晶構造が挙げられる。ここで、「チオリシコンリージョンII型結晶構造」としては、Li4-xGe1-xPxS4系チオリシコンリージョンII(thio-LISICON Region II)型結晶構造(Kannoら、Journal of The Electrochemical Sociey, 148(7)A742-746(2001)参照))、Li4-xGe1-xPxS4系チオリシコンリージョンII(thio-LISICON Region II)型と類似の結晶構造(Solid State Ionics,177(2006),2721-2725参照)等が挙げられる。
 CuKα線を用いたX線回折測定において、Li3PS4結晶構造の回折ピークは、例えば2θ=17.5°、18.3°、26.1°、27.3°、30.0°付近に現れ、Li4P2S6結晶構造の回折ピークは、例えば2θ=16.9°、27.1°、32.5°付近に現れ、Li7PS6結晶構造の回折ピークは、例えば2θ=15.3°、25.2°、29.6°、31.0°付近に現れ、Li7P3S11結晶構造の回折ピークは、例えば2θ=17.8°、18.5°、19.7°、21.8°、23.7°、25.9°、29.6°、30.0°付近に現れ、Li4-xGe1-xPxS4系チオリシコンリージョンII(thio-LISICON Region II)型結晶構造の回折ピークは、例えば2θ=20.1°、23.9°、29.5°付近に現れ、Li4-xGe1-xPxS4系チオリシコンリージョンII(thio-LISICON Region II)型と類似の結晶構造の回折ピークは、例えば2θ=20.2°、23.6°付近に現れる。なお、これらのピーク位置については、±0.5°の範囲内で前後していてもよい。
 固体電解質は、上記チオリシコンリージョンII型結晶構造を有するものであってもよいし、主結晶として有するものであってもよい。本明細書において、「主結晶として有する」とは、結晶構造のうち対象となる結晶構造の割合が80%以上であることを意味し、90%以上であることが好ましく、95%以上であることがより好ましい。
 また、結晶性の硫化物固体電解質の結晶構造としては、アルジロダイト型結晶構造も挙げられる。アルジロダイト型結晶構造としては、例えば、Li7PS6結晶構造;Li7PS6の構造骨格を有する組成式Li7-xP1-ySiyS6及びLi7+xP1-ySiyS6(xは-0.6~0.6、yは0.1~0.6)で示される結晶構造;Li7-x-2yPS6-x-yClx(0.8≦x≦1.7、0<y≦-0.25x+0.5)で示される結晶構造;Li7-xPS6-xHax(HaはClもしくはBr、xが好ましくは0.2~1.8)で示される結晶構造、が挙げられる。
 上記の結晶構造の中でも、結晶性硫化物固体電解質が有する結晶構造としては、Li3PS4結晶構造、チオリシコンリージョンII型結晶構造、アルジロダイト型結晶構造が好ましい。
 一実施形態において、本態様に係る正極合材の製造方法により製造された正極合材に含まれる固体電解質の20~100質量%、25~95質量%又は30~90質量%が固体電解質αである。
(粉末X線回折)
 上述したように、正極合材は、CuKα線を利用した粉末X線回折において、2θ=15.1±0.8°に回折ピークAを、29.8±0.8°に回折ピークBを有する。これら回折ピークA及びBは、固体電解質αに由来するものである。
 一実施形態において、正極合材は、前記回折ピークAの半値幅が0.5°以上である。回折ピークAの半値幅は、好ましくは0.6°以上、より好ましくは0.7°以上である。これにより、良好な圧密性が得られ、また活物質との強固な界面形成が可能になる。
 一実施形態において、正極合材は、前記回折ピークAの半値幅が0.5~3.0°、0.6~2.5°又は0.7~2.0°である。
 尚、回折ピークAの半値幅は、実施例に記載の方法により測定される値である。
(導電助剤)
 一実施形態において、正極合材は導電助剤を含む。導電助剤としては例えば炭素材料等が挙げられる。
 一実施形態において、正極合材は、炭素材料である導電助剤を含み、電子顕微鏡画像のエネルギー分散型X線分光法による元素分析において、炭素とリンのマッピングの重複率が45%以上である。前記重複率は、好ましくは55%以上、より好ましくは60%以上である。重複率が45%以上であると、正極合材中の成分(例えば、固体電解質や導電助剤、硫黄系活物質等)が十分に混合されており、合材構造の観点では、より多くの部分の硫黄系活物質への導電性を担保可能となり、活物質利用率が増加する効果が期待できる。
 導電助剤は、電子伝導性のある材料であればよく、炭素材料であることが好ましい。導電助剤は複数の細孔を有することが好ましい。特に好ましくは、細孔を有する炭素材料である。炭素材料は導電性が高く、かつ他の導電性のある材料よりも軽いため、電池の重量当りの出力密度と容量を高くすることができる。
 炭素材料としては、特に限定しないが、ケッチェンブラック、アセチレンブラック、デンカブラック、サーマルブラック、チャンネルブラック等のカーボンブラック、メソポーラス炭素、活性炭、無定形炭素、カーボンナノチューブ、気相成長カーボンファイバ(VGCF)、カーボンナノホーン等が挙げられ、導電性の炭素材料としては、フラーレン、炭素繊維、天然黒鉛、人造黒鉛、グラフェン、酸化グラフェン、還元型酸化グラフェン等が挙げられる。また、これらは単独で用いてもよく、2種以上を併用してもよい。また、これらの複合材を用いることもできる。
 一実施形態において、正極合材は、硫黄系活物質、固体電解質及び導電助剤以外の他の成分を含んでもよいし、含まなくてもよい。
 他の成分は特に限定されないが、例えば、バインダー、溶剤、分散剤等が挙げられる。
 正極合材において、硫黄系活物質、固体電解質及び導電助剤の含有量は特に限定されない。
 一実施形態において、硫黄系活物質の含有量は、固体電解質100質量部に対して40~350質量部である。
 一実施形態において、導電助剤の含有量は、固体電解質100質量部に対して10~300質量部である。
 一実施形態において、硫黄系活物質と導電助剤の質量比(硫黄系活物質:導電助剤)は、10:90~95:5又は20~90:80~10である。
 一実施形態において、固体電解質の含有量と、硫黄系活物質及び導電助剤の含有量との比(固体電解質:硫黄系活物質+導電助剤)は、10:90~90:10、15~70:85~30又は20~60:80~40である。
 一実施形態において、正極合材の50質量%以上、60質量%以上、70質量%以上、80質量%以上、90質量%以上、95質量%以上、99質量%以上、99.5質量%以上又は実質的に100質量%が、導電助剤、硫黄系活物質及び固体電解質である。尚、「実質的に100質量%」の場合、不可避不純物を含んでもよい。
 一実施形態において、正極合材は、硫黄系活物質に固体電解質を添加して混合処理することで第1混合物を得る第1混合工程と、前記第1混合物にさらなる固体電解質を添加して混合処理することで第2混合物を得る第2混合工程とを含み、前記第2混合工程で添加する前記固体電解質が固体電解質αを含む製造方法によって得られ、前記固体電解質αが、CuKα線を利用した粉末X線回折において、2θ=15.1±0.8°に回折ピークAを、29.8±0.8°に回折ピークBを有し、元素としてP及びBを有する。
 本実施形態において、前記第2混合工程において前記第1混合工程よりも小さいエネルギーで混合処理することが好ましい。
 本実施形態において、前記第1混合工程は、該第1混合工程において添加される前記固体電解質の非晶質化が進行する条件で混合処理し、前記第2混合工程は、該第2混合工程において添加される前記固体電解質の結晶性が消失しない条件で混合処理することが好ましい。
 尚、本実施形態における製造方法については、「2.正極合材の製造方法」についてする説明が援用される。
2.正極合材の製造方法
 本発明の一態様に係る正極合材の製造方法は、硫黄系活物質に固体電解質を添加して混合処理することで第1混合物を得る第1混合工程と、前記第1混合物にさらなる固体電解質を添加して混合処理することで第2混合物を得る第2混合工程とを含み、前記第2混合工程で添加する前記固体電解質が固体電解質αを含み、前記固体電解質αが、CuKα線を利用した粉末X線回折において、2θ=15.1±0.8°に回折ピークAを、29.8±0.8°に回折ピークBを有し、元素としてP及びBを有する。
 本態様に係る正極合材の製造方法によれば、本発明の一態様に係る正極合材を好適に製造できる。
(第1混合工程)
 第1混合工程では、硫黄系活物質に固体電解質を添加して混合処理することで第1混合物を得る。
 第1混合工程で添加する固体電解質は格別限定されず、固体電解質α及び固体電解質α以外の固体電解質が挙げられる。固体電解質α及び固体電解質α以外の固体電解質については、「1.正極合材」についてした説明が援用される。
 一実施形態において、第1混合工程で添加される固体電解質は、固体電解質α以外の固体電解質を含む。
 一実施形態において、第1混合工程で添加される固体電解質の総量を100質量部としたときに、第1混合工程で添加される固体電解質αの量は0~50質量部、0~50質量部、0~40質量部、0~30質量部、0~20質量部、0~10質量部、0~5質量部又は0質量部である。
(第2混合工程)
 第2混合工程では、第1混合物にさらなる固体電解質を添加して混合処理することで第2混合物(正極合材)を得る。
 第2混合工程で添加する固体電解質は、固体電解質αを含む。
 第2混合工程において、固体電解質αと共に、固体電解質α以外の固体電解質を添加してもよい。
 一実施形態において、第2混合工程で添加される固体電解質の総量を100質量部としたときに、第2混合工程で添加される固体電解質αの量が50~100質量部、60~100質量部、70~100質量部、80~100質量部、90~100質量部、95~100質量部又は100質量部である。
 一実施形態において、本態様に係る正極合材の製造方法により製造された正極合材に含まれる固体電解質αを100質量部としたときに、第2混合工程で添加された固体電解質αの割合が50~100質量部、60~100質量部、70~100質量部、80~100質量部、90~100質量部、95~100質量部又は100質量部である。
 一実施形態において、第2混合工程において第1混合工程よりも小さいエネルギーで混合処理する。言い換えれば、一実施形態において、第1混合工程及び第2混合工程のそれぞれにおける混合処理のエネルギーは、第1混合工程>第2混合工程の条件を満たす。
 一実施形態において、第1混合工程は、該第1混合工程において添加される固体電解質の非晶質化が進行する条件で混合処理し、第2混合工程は、該第2混合工程において添加される固体電解質αの結晶性が消失しない条件で混合処理する。
 例えば、第1混合工程では、該第1混合工程において添加される固体電解質の結晶ピークの強度減少、ピーク半値幅の増加あるいはピークの消失が起こり得る条件で混合処理することができる。一方、第2混合工程では、該第2混合工程において添加される固体電解質αの結晶ピークが消失しない条件、好ましくは結晶ピークの強度変化又はピーク半値幅の変化が小さい条件で混合処理することができる。ここで、「変化が小さい」というのは、例えば、その変化率が、第1混合工程における変化率よりも小さいことであり得る。
 第1混合工程において用いられる混合装置としては、例えば、遊星型ボールミル、転動ミル、ビーズミル、フィルミクス、ナウタミキサー、トルネードミキサー、二軸押出機、多軸ローラー、固相せん断混練機等が挙げられる。
 第2混合工程において用いられる混合装置としては、第1混合工程について例示したものを用いることができる。この場合、混合装置の選択や運転条件の設定に際しては、混合処理のエネルギーが第1混合工程>第2混合工程の条件を満たすことが好ましい。第1混合工程と第2混合工程で用いる装置は、同じものであっても、異なってもよい。同じ装置を用いる場合は、例えば処理時間や積算動力を第1混合工程>第2混合工程に設定する方法や、遊星型ボールミルや転動ミルのように回転動力を利用するものであれば回転数を第1混合工程>第2混合工程に設定する方法などを用いることができる。
 一実施形態において、第1混合工程において遊星型ボールミルを用いる。
 一実施形態において、第2混合工程において転動ミルを用いる。
 一実施形態において、第1混合工程に供される硫黄系活物質は、予め導電助剤(好ましくは炭素材料である導電助剤)と複合化されている。
 例えば、第1混合工程の前に、硫黄系活物質を導電助剤と共に加熱することによって、硫黄系活物質を導電助剤と複合化することができる。この加熱温度は特に限定されず、例えば、120℃を超える温度、例えば、150℃以上、170℃以上、200℃以上、150℃以上、200℃以上、250℃以上又は300℃以上であり得る。上限は、例えば350℃以下である。
 一実施形態において、硫黄系活物質と導電助剤の質量比(硫黄系活物質:導電助剤)は、10:90~95:5又は20~90:80~10である。
 一実施形態において、本態様に係る正極合材の製造方法により製造される正極合材において、固体電解質の合計質量と、硫黄系活物質及び導電助剤の合計質量との比(固体電解質:硫黄系活物質+導電助剤)は10:90~90:10、15~70:85~30又は20~60:80~40である。
 一実施形態において、本態様に係る正極合材の製造方法により製造される正極合材は、上述した本発明の一態様に係る正極合材であり、本発明の一態様に係る正極合材についてした説明が援用される。
3.リチウムイオン電池
 本発明の一態様に係るリチウムイオン電池は、本発明の一態様に係る正極合材を含む。
 本態様のリチウムイオン電池によれば、優れた可逆放電容量を発揮できる効果が得られる。
 正極合材は、リチウムイオン電池の正極層として用いることができる。この場合、リチウムイオン電池の他の構成は本技術分野にて公知のものが使用でき、負極活物質にリチウムイオンを含まない負極層を選択できる。
 尚、リチウムイオン電池の負極層に含まれる負極活物質を「リチウムイオンを含む負極活物質」とすることが可能である。また、リチウムイオン電池の負極層に含まれる負極活物質は「リチウムイオンを正極に供給する負極活物質」であってもよい。
 リチウムイオン電池の負極は、通常の電池に使用できるものであれば、特に制限されない。負極は、負極活物質と固体電解質を混合した負極合剤からなるものでもよい。
 負極活物質としては、市販されているものを使用できる。例えば、炭素材料、Sn金属、In金属、Si金属、これらの金属に合金等を使用できる。具体的には、天然黒鉛や各種グラファイト、Si,Sn,Al,Sb,Zn,Bi等の金属粉、SiAl,Sn5Cu6,Sn2Co,Sn2Fe等の金属合金、その他アモルファス合金やメッキ合金が挙げられる。粒径に関しても特に制限はないが、平均粒径が数μm~80μmのものを好適に使用できる。
 電解質層は、特に制限はなく、公知のものが使用できる。例えば、酸化物系固体電解質、硫化物系固体電解質、ポリマー系電解質が好ましく、イオン伝導度の観点から硫化物系固体電解質がより好ましい。この硫化物系固体電解質は上述した正極合材に使用するものが好ましい。
 リチウムイオン電池の製造方法は、特に制限されない。例えば、正極集電体上に本発明の一態様に係る正極合材からなる正極層を形成したシートに固体電解質層を形成し、予め形成した負極集電体上に負極層を形成したシートを積層し、プレスする方法等が挙げられる。
 以下に本発明の実施例を説明するが、本発明はこれらの実施例により限定されない。
1.正極合材の作製
(実施例1)
(1)複合粉末Aの作製
 ガラス瓶に、活性炭(関西熱化学製MSC-30)と硫黄を3:7の質量比で入れ、SUS管容器内に封入した。電気炉にて150℃で6時間、300℃で2.75時間加熱し、活性炭と硫黄の複合粉末Aを得た。
(2)固体電解質Aの作製
 硫化リチウム0.4127g、五硫化二リン0.6655g、ヨウ化リチウム0.2137g、臭化リチウム0.2080gと、直径10mmのジルコニア製ボール10個を、45mLのジルコニア製ポットに投入し密閉した。遊星型ボールミル装置(フリッチュ社製、型番P-7)を用いて、回転速度370rpmで40時間混合(メカニカルミリング)して得られた粉末に対して195℃、3時間の条件で加熱処理することで固体電解質Aを得た。
(3)固体電解質αの作製
 硫化リチウム0.3830g、五硫化二リン0.6170gと、直径10mmのジルコニア製ボール10個を、45mLのジルコニア製ポットに投入し密閉した。遊星型ボールミル装置(フリッチュ社製、型番P-7)を用いて、回転速度370rpmで40時間混合(メカニカルミリング)して、粉末を得た。
 次いで、得られた粉末0.8053g、水素化ホウ素リチウム0.1947gと、直径4mmのジルコニア製ボール100gを、45mLのジルコニア製ポットに投入し密閉した。遊星型ボールミル装置(フリッチュ社製、型番P-7)を用いて、回転速度510rpmで15時間混合(メカニカルミリング)することで、固体電解質α(粉末)を得た。
(4)正極合材粉末の作製
第1混合工程
 複合粉末A 0.9gと固体電解質A 0.18gを直径10mmのジルコニア製ボール10個と共に、45mLのジルコニア製ポットに投入し、密閉した。遊星型ボールミル(フリッチュ社製、型番P-7)を用いて、回転速度370rpm、20時間、室温(25℃。以下同様。)の条件で混合を行い、複合粉末Bを得た。
第2混合工程
 複合粉末B 0.54gと固体電解質α 0.36gを直径2mmのジルコニア製ボール34gと共に、45mLのジルコニア製ポットに投入し、密閉した。転動ミル(「小型ボールミル架台」、アサヒ理化製作所製、型番AV-1)を用いて、回転速度600rpm、1時間、室温の条件で混合を行い、正極合材粉末を得た。
(比較例1)
 実施例1と同様にして得られた複合粉末A 0.45gと、実施例1と同様にして得られた固体電解質α 0.45gを直径10mmのジルコニア製ボール10個と共に、45mLのジルコニア製ポットに投入し、密閉した。遊星型ボールミル装置(フリッチュ社製、型番P-7)を用いて、回転速度370rpm、20時間、室温の条件で混合を行い、正極合材粉末を得た。
 得られた正極合材粉末について、実施例1と同様に充放電試験を行った。得られた可逆放電容量(2ndサイクルにおける放電容量)を表1に示す。
2.測定方法及び試験方法
(1)正極合材粉末の粉末X線回折(XRD)
 実施例及び比較例で得られた正極合材粉末のそれぞれについて、XRD測定を行った。
 具体的には、正極合材粉末を、直径20mm、深さ0.2mmの溝に充填し、ガラスで均して試料とした。この試料を、XRD用カプトンフィルムでシールして空気に触れさせずに測定した。
 XRD測定は、株式会社BRUKERの粉末X線回折測定装置D2 PHASERを用いて下記測定条件にて実施した。
[測定条件]
   管電圧:30kV
   管電流:10mA
   X線波長:Cu-Kα線(1.5418Å)
   光学系:集中法
   スリット構成:ソーラースリット4°(入射側・受光側共に)、発散スリット1mm、Kβフィルター(Ni板0.5%)、エアスキャッタースクリーン(3mmを使用)
   検出器:半導体検出器
   測定範囲:2θ=10-60deg
   ステップ幅、スキャンスピード:0.05deg、0.05deg/秒
 尚、XRD測定は、固体電解質αのみからなる参照用試料(参考例1)についても行った。
 結果を図1に示す。
 また、X線回折パターンについて、以下の方法により、2θ=15.1±0.8°における回折ピークA、及び2θ=29.8±0.8°における回折ピークBのそれぞれが存在するか否かを判定した。また、以下の方法により、回折ピークAの半値幅を求めた。
回折ピークA及び回折ピークBのそれぞれが存在するか否かの判定方法
回折ピークA
 2θ=15.1°±0.8°の範囲に回折ピークAが存在するか否かは、X線回折パターンにおいて、2θ=(15.1°-0.8°)±0.2すなわち2θ=14.3°±0.2°と、2θ=(15.1°+0.8°)±0.2°すなわち2θ=15.9°±0.2°とのX線強度(counts)の平均値をバックグラウンド(BG)の強度Ibgとし、2θ=15.1°±0.8°のX線強度(counts)の最大値をピーク強度Ipeakとしたときに、その比(Ipeak/Ibg)が、1.100以上であれば、回折ピークAが存在するものと判定する。
 回折ピークAに係る比(Ipeak/Ibg)は、1.150以上であることが好ましく、1.200以上であることがより好ましい。
回折ピークB
 2θ=29.8±0.8°の範囲に回折ピークBが存在するか否かは、X線回折パターンにおいて、2θ=(29.8°-0.8°)±0.2すなわち2θ=29.0°±0.2°と、2θ=(29.8°+0.8°)±0.2°すなわち2θ=30.6°±0.2°とのX線強度(counts)の平均値をバックグラウンド(BG)の強度Ibgとし、2θ=29.8°±0.8°のX線強度(counts)の最大値をピーク強度Ipeakとしたときに、その比(Ipeak/Ibg)が、1.055以上であれば、回折ピークBが存在するものと判定する。
 回折ピークBに係る比(Ipeak/Ibg)は、1.070以上であることが好ましく、1.100以上であることがより好ましい。
 以上の結果、実施例1の正極合材において、回折ピークAは、比(Ipeak/Ibg)が1.247であることから「存在する」と判定され、回折ピークBは、比(Ipeak/Ibg)が1.129であることから「存在する」と判定された。
 一方、比較例1の正極合材において、回折ピークAは、比(Ipeak/Ibg)が1.085であることから「存在しない」と判定され、回折ピークBは、比(Ipeak/Ibg)が1.049であることから「存在しない」と判定された。
回折ピークAの半値幅の算出
 回折ピークAの半値幅(β)は、測定により得られる半値幅(w)から測定装置固有の装置定数(B)を差し引き、β=w-Bとして算出した。
w:測定により得られた15.1±0.8°のピーク(回折ピークA)の半値幅
B:装置定数(標準物質(シリコン)を同様に測定し、2θ=28.4°のピークから、B=0.1269°を求めた。)
 w(測定により得られた半値幅)は次のようにして求めた。XRDの測定により得られたピーク形状に直線によるベースラインを設定し、各点の強度とベースラインの差分をとり、XRD曲線とした。XRD曲線をローレンツ関数L(x)とガウス関数G(x)からなる式(f(x)=(1-α)×L(x)+α×G(x))として、カーブフィッティングによりパラメータA(補正ピーク強度)、w、x0(ピークトップの2θ)及びα(ローレンツ関数の割合)を決定した。
Figure JPOXMLDOC01-appb-M000001
 カーブフィッティングでは、ピークトップから±1.0°程度の範囲をフィッティング範囲として適宜設定する。各θでのf(x)で計算されるフィッティング曲線の強度とXRD曲線の強度の誤差を取り、フィッティング範囲全体の誤差を足し合わせた値を最小化することによりフィッティングを行った。ここでは表計算ソフト(エクセル、マイクロソフト)のソルバー機能(GRG非線形)を用いた。
 以上の結果、実施例1の回折ピークAの半値幅は、1.18°であった。
(2)電子顕微鏡画像のエネルギー分散型X線分光法(SEM-EDS分析)及び炭素とリンの重複率算出
正極合材ペレットの作製
 実施例及び比較例で得られた正極合材粉末のそれぞれについて、SEM-EDS分析を行った。
 具体的には、直径10mmのマコール製の円筒に、固体電解質A 100mgを投入し、加圧成型した。加圧面に、得られた正極合材粉末を20mgになるよう投入し、再度加圧成型した。続いて逆側の加圧面に正極合材粉末を20mgになるよう投入し、再々度加圧成型し、円筒から成型体を抜き出すことで正極合材ペレットを得た。
SEM-EDS分析
 正極合材ペレットを垂直方向に割り、露出した面に対してイオンミリング処理(日立ハイテク社製、IM4000)を行うことで正極合材ペレットの断面出しを行った。得られた断面に対してSEM(日立ハイテク社製、SU8220)、EDS(Bruker社製、QUANTAX FlatQUAD)を用いてSEM-EDS元素マッピング測定を行い、二次電子像及び炭素、リンのEDS像を10視野得た。観察倍率は5000倍で、加速電圧は10kV、スキャン領域は1024×768で実施した。EDSマッピングに関しては特別な画像処理は行わず、実際の測定強度がマッピングされた像を用いた。
 尚、SEM-EDS元素マッピング測定に際しては、イオンミリングにより断面加工した領域を上下に2等分割し、2等分割した領域をそれぞれ左右に5等分割した。このようにして10分割された領域それぞれの中心部を観察倍率5000倍でSEM-EDS元素マッピングを取得した。
炭素とリンのマッピングの重複率の算出
 上記の手順で得られた画像処理については、Python(3.9.9)のOpenCV(4.5.1)を用いた。炭素、リンのEDS像10視野全てに対して、d=15、sigmaColor=64、sigmaSpace=64のバイラテラルフィルタを用いた平滑化処理を二回行った。得られた画像に対し、ニューラルネットワークオープンライブラリKeras(2.4.3)のMaxPooling2D(pool_size=3、strides=3)を用いて画素を1/3に圧縮し、メディアンフィルタで平滑化した。平滑化した画像をグレースケール化し、炭素は最低輝度30、最高輝度255、リンは最低輝度40、最高輝度255にて二値化処理を行った。
 以上の画像処理を含めたSEM-EDS分析の結果を図2(実施例1)及び図3(比較例1)に示す。これらの図において、(a)は画像処理前(平滑化、圧縮及び二値化処理前)、(b)は画像処理後を示す。また、Cは炭素のマッピング、Pはリンのマッピングを示す。
 これらの処理により、画像データを、元素が存在しない場合は0、存在する場合は255の数値行列に変換した。炭素、リンの数値行列の中で、255が同一座標にて重なるピクセルの総数を全ピクセル数で除することで1視野の重複率を算出した。全10視野の重複率の平均を本態様の重複率(炭素とリンのマッピングの重複率)とした。
 以上の結果、実施例1では、炭素とリンのマッピングの重複率は70.9%であった。比較例1では、炭素とリンのマッピングの重複率は99.7%であった。
(3)可逆放電容量(充放電試験)
リチウムイオン電池(全固体電池)の作製
 実施例及び比較例で得られた正極合材粉末のそれぞれ5mgを用いてリチウムイオン電池(全固体電池)を作製した。
 具体的には、まず、直径10mmのマコール製の円筒内で固体電解質A 100mgを加圧成型した。
 次いで、成型された固体電解質Aにおける一方の面に、正極合材粉末を5mgになるよう投入し、再度加圧成型した。
 次いで、成形された固体電解質Aにおける他方の面(正極合材と反対側の面)に、インジウム箔3枚とリチウム箔2枚を交互に積層するように投入し、加圧することで、全固体電池を得た。
充放電試験
 得られた全固体電池について、定電流充放電試験を行った。定電流充放電試験は、放電スタートで、電圧範囲は0.8~2.2V、電流値は0.147mAに設定した。
 以上の結果、可逆放電容量(2ndサイクルにおける放電容量)は、実施例1では1474mAh/g、比較例1では397mAh/gであった。
 よって、実施例1は、比較例1に比べて、可逆放電容量が顕著に向上していることがわかる。
 上記に本発明の実施形態及び/又は実施例を幾つか詳細に説明したが、当業者は、本発明の新規な教示及び効果から実質的に離れることなく、これら例示である実施形態及び/又は実施例に多くの変更を加えることが容易である。従って、これらの多くの変更は本発明の範囲に含まれる。
 この明細書に記載の文献、及び本願のパリ条約による優先権の基礎となる出願の内容を全て援用する。

Claims (13)

  1.  硫黄系活物質及び固体電解質を含み、
     CuKα線を利用した粉末X線回折において、2θ=15.1±0.8°に回折ピークAを、29.8±0.8°に回折ピークBを有し、
     元素としてP及びBを有する、
     正極合材。
  2.  前記回折ピークAの半値幅が0.5°以上である、請求項1に記載の正極合材。
  3.  炭素材料である導電助剤を含み、電子顕微鏡画像のエネルギー分散型X線分光法による元素分析において、炭素とリンのマッピングの重複率が45%以上である、請求項1又は2に記載の正極合材。
  4.  硫黄系活物質に固体電解質を添加して混合処理することで第1混合物を得る第1混合工程と、前記第1混合物にさらなる固体電解質を添加して混合処理することで第2混合物を得る第2混合工程とを含み、前記第2混合工程で添加する前記固体電解質が固体電解質αを含む製造方法によって得られ、
     前記固体電解質αが、CuKα線を利用した粉末X線回折において、2θ=15.1±0.8°に回折ピークAを、29.8±0.8°に回折ピークBを有し、元素としてP及びBを有する、
     請求項1~3のいずれかに記載の正極合材。
  5.  前記第2混合工程において前記第1混合工程よりも小さいエネルギーで混合処理する、請求項4に記載の正極合材。
  6.  前記第1混合工程は、該第1混合工程において添加される前記固体電解質の非晶質化が進行する条件で混合処理し、
     前記第2混合工程は、該第2混合工程において添加される前記固体電解質αの結晶性が消失しない条件で混合処理する、
     請求項4又は5に記載の正極合材。
  7.  請求項1~6のいずれかに記載の正極合材を含む、リチウムイオン電池。
  8.  硫黄系活物質に固体電解質を添加して混合処理することで第1混合物を得る第1混合工程と、
     前記第1混合物にさらなる固体電解質を添加して混合処理することで第2混合物を得る第2混合工程とを含み、
     前記第2混合工程で添加する前記固体電解質が固体電解質αを含み、
     前記固体電解質αが、CuKα線を利用した粉末X線回折において、2θ=15.1±0.8°に回折ピークAを、29.8±0.8°に回折ピークBを有し、元素としてP及びBを有する、
     正極合材の製造方法。
  9.  前記第2混合工程において前記第1混合工程よりも小さいエネルギーで混合処理する、請求項8に記載の正極合材の製造方法。
  10.  前記第1混合工程は、該第1混合工程において添加される前記固体電解質の非晶質化が進行する条件で混合処理し、
     前記第2混合工程は、該第2混合工程において添加される前記固体電解質αの結晶性が消失しない条件で混合処理する、
     請求項8又は9に記載の正極合材の製造方法。
  11.  製造された正極合材に含まれる固体電解質αを100質量部としたときに、前記第2混合工程で添加された固体電解質αの割合が50~100質量部である、請求項8~10のいずれかに記載の正極合材の製造方法。
  12.  前記第1混合工程で添加される固体電解質の総量を100質量部としたときに、前記第1混合工程で添加される前記固体電解質αの量が0~50質量部である、請求項8~11のいずれかに記載の正極合材の製造方法。
  13.  前記第2混合工程で添加される固体電解質の総量を100質量部としたときに、前記第2混合工程で添加される前記固体電解質αの量が50~100質量部である、請求項8~12のいずれかに記載の正極合材の製造方法。
PCT/JP2024/009414 2023-03-24 2024-03-11 正極合材、リチウムイオン電池及び正極合材の製造方法 Ceased WO2024203249A1 (ja)