WO2024085970A1 - Method to selectively etch silicon nitride to silicon oxide using water crystallization - Google Patents

Method to selectively etch silicon nitride to silicon oxide using water crystallization Download PDF

Info

Publication number
WO2024085970A1
WO2024085970A1 PCT/US2023/032042 US2023032042W WO2024085970A1 WO 2024085970 A1 WO2024085970 A1 WO 2024085970A1 US 2023032042 W US2023032042 W US 2023032042W WO 2024085970 A1 WO2024085970 A1 WO 2024085970A1
Authority
WO
WIPO (PCT)
Prior art keywords
layer
substrate
plasma
silicon nitride
silicon
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/US2023/032042
Other languages
English (en)
French (fr)
Other versions
WO2024085970A8 (en
Inventor
Yu-Hao TSAI
Mingmei Wang
Du Zhang
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Tokyo Electron Ltd
Tokyo Electron US Holdings Inc
Original Assignee
Tokyo Electron Ltd
Tokyo Electron US Holdings Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Tokyo Electron Ltd, Tokyo Electron US Holdings Inc filed Critical Tokyo Electron Ltd
Priority to KR1020257015143A priority Critical patent/KR20250091229A/ko
Priority to JP2025522154A priority patent/JP2025534555A/ja
Priority to CN202380070418.7A priority patent/CN119968697A/zh
Publication of WO2024085970A1 publication Critical patent/WO2024085970A1/en
Anticipated expiration legal-status Critical
Publication of WO2024085970A8 publication Critical patent/WO2024085970A8/en
Ceased legal-status Critical Current

Links

Classifications

    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P50/00—Etching of wafers, substrates or parts of devices
    • H10P50/69—Etching of wafers, substrates or parts of devices using masks for semiconductor materials
    • H10P50/691—Etching of wafers, substrates or parts of devices using masks for semiconductor materials for Group IV materials or Group III-V materials
    • H10P50/692—Etching of wafers, substrates or parts of devices using masks for semiconductor materials for Group IV materials or Group III-V materials characterised by their composition, e.g. multilayer masks or materials
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P50/00—Etching of wafers, substrates or parts of devices
    • H10P50/20—Dry etching; Plasma etching; Reactive-ion etching
    • H10P50/28—Dry etching; Plasma etching; Reactive-ion etching of insulating materials
    • H10P50/282—Dry etching; Plasma etching; Reactive-ion etching of insulating materials of inorganic materials
    • H10P50/283—Dry etching; Plasma etching; Reactive-ion etching of insulating materials of inorganic materials by chemical means
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P50/00—Etching of wafers, substrates or parts of devices
    • H10P50/69—Etching of wafers, substrates or parts of devices using masks for semiconductor materials
    • H10P50/691—Etching of wafers, substrates or parts of devices using masks for semiconductor materials for Group IV materials or Group III-V materials
    • H10P50/693—Etching of wafers, substrates or parts of devices using masks for semiconductor materials for Group IV materials or Group III-V materials characterised by their size, orientation, disposition, behaviour or shape, in horizontal or vertical plane
    • H10P50/695—Etching of wafers, substrates or parts of devices using masks for semiconductor materials for Group IV materials or Group III-V materials characterised by their size, orientation, disposition, behaviour or shape, in horizontal or vertical plane characterised by the process involved to create the mask, e.g. lift-off masks or sidewalls or to modify the mask
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P95/00—Generic processes or apparatus for manufacture or treatments not covered by the other groups of this subclass

Definitions

  • various materials formed on a substrate may be removed by patterned etching, chemical-mechanical polishing, as well as other techniques.
  • a variety of techniques are known for etching layers on a substrate, including plasma-based or vapor-phase etching (otherwise referred to as dry etching) and liquid based etching (otherwise referred to as wet etching).
  • plasma-based or vapor-phase etching otherwise referred to as dry etching
  • liquid based etching otherwise referred to as wet etching
  • Silicon nitride is used in a wide variety of semiconductor devices as a barrier layer for dopant diffusion, a gate sidewall spacer layer, a buffer layer, a liner layer, an etch stop layer, etc. due to its high insulating characteristics, high thermal and mechanical stability, etc. Because SiN layers are commonly formed on substrates having silicon (Si) and/or silicon oxide (SiO2) layers disposed thereon, selective etching of silicon nitride over silicon and/or silicon oxide is important for various microelectronic applications.
  • fabrication of nanosheet FETs typically require the removal of silicon nitride spacers with etch processes that are selective to silicon channel regions that are encapsulated by the silicon nitride spacers.
  • a contact etch stop layer (CESL) on epitaxial semiconductor material (epi) fins and/or along a gate sidewall is typically required to be removed with a highly selective etch. For example, a loss of less than 3 nanometers (nm) of material from epi fins is often required.
  • removal of CESL residues from valleys situated between epi diamond structures can be a significant challenge for certain process flows.
  • fluorocarbon e.g., CxFz-based
  • hydrofluorocarbon e.g., CxHyFz-based
  • fluorine e.g., NF x -based
  • Cx H y F z /O 2 /H 2 plasmas have been used to create thicker depositions on SiN and CF4/O2/N2 plasmas have been used to enhance nitrogen elimination in SiN layers.
  • This two-step process uses a dry etch technique for surface modification and a wet etch technique for removal of the modified surface layer, and as such, cannot be implemented as a cyclical process.
  • Another two-step process used to selectively etch silicon nitride in a cyclic dry etch process uses a hydrogen plasma to modify exposed SiN surfaces and a fluorinated plasma to remove the modified surface layer.
  • This two-step dry etch process is typically performed in a plasma processing chamber (e.g., an inductively coupled plasma, ICP, or capacitively coupled, CCP, process chamber) at relatively low pressure (e.g., 10-100 mTorr) and moderate to high temperature (e.g., 10°C - 100°C) to selectively etch SiN in a cyclic process.
  • a plasma processing chamber e.g., an inductively coupled plasma, ICP, or capacitively coupled, CCP, process chamber
  • relatively low pressure e.g., 10-100 mTorr
  • moderate to high temperature e.g. 10°C - 100°C
  • SiN silicon nitride
  • oxide e.g., SiO 2
  • a highly selective etch of silicon nitride to oxide is critical in many semiconductor fabrication processes.
  • Embodiments of improved processes and methods that provide selective etching of silicon nitride are disclosed herein.
  • a cyclic, two-step dry etch process is used to selectively etch silicon nitride layers formed on a substrate, while protecting oxide layers formed on the same substrate.
  • the cyclic, two-step dry etch process disclosed herein sequentially exposes the substrate to: (1) a hydrogen plasma to modify exposed surfaces of the silicon nitride layer and the oxide layer to form a modified silicon nitride surface layer and a modified oxide surface layer, and (2) a halogen plasma to selectively etch silicon nitride by removing the modified silicon nitride surface layer without removing the modified oxide surface layer.
  • the oxide layer is protected from etching during the removal step (i.e., step 2) by creating a crystallized water layer on the oxide layer during the surface modification step (i.e., step 1).
  • the crystallized water layer improves selectivity of silicon nitride to oxide by providing a protective layer on the oxide layer, which prevents reactive species of the halogen plasma from reaching the modified oxide surface layer.
  • the process gas(es) used to generate the halogen plasma may further reduce (or eliminate) etching of the oxide layer by providing a highly selective etch of the modified silicon nitride surface layer to the modified oxide surface layer.
  • the embodiments disclosed herein create a protective water layer on the oxide layer by leveraging the different volatilities of reaction byproducts produced during the surface modification step (i.e., step 1).
  • hydrogen ions within the hydrogen plasma (a) react with exposed surface of the silicon nitride layer to form a first reaction byproduct (e.g., ammonia, NH3), and (b) react with exposed surfaces of the oxide layer to form a second reaction byproduct (e.g., water, H 2 O).
  • a first reaction byproduct e.g., ammonia, NH3
  • a second reaction byproduct e.g., water, H 2 O
  • the embodiments disclosed herein may vaporize the first reaction byproduct, leaving a silicon (Si) surface layer on the SiN layer, and freeze the second reaction byproduct, leaving a crystallized water layer on the oxide layer.
  • a method is provided herein of selectively etching silicon nitride over oxide in accordance with the present disclosure.
  • the method may include providing a substrate having a silicon nitride layer and an oxide layer exposed on a surface of the substrate, and exposing the surface of the substrate to a hydrogen plasma to: (a) modify an exposed surface of the silicon nitride layer to form a first modified layer, and (b) modify an exposed surface of the oxide layer to form a second modified layer.
  • a gas pressure used to generate the hydrogen plasma and a temperature of the substrate create a crystallized water layer, which bonds with the oxide layer to form the second modified layer.
  • the method may include exposing the surface of the substrate to a halogen plasma to selectively etch the silicon nitride layer by removing the first modified layer without removing the second modified layer, and repeating said exposing the surface of the substrate to the hydrogen plasma and said exposing the surface of the substrate to the halogen plasma one or more times until a predetermined amount of the silicon nitride layer is selectively etched.
  • a wide variety of gas pressures and substrate temperatures may be used in the method described above.
  • the gas pressure may range between 10 mTorr and 1500 Torr and the substrate temperature may range between 20°C and -150°C, in some embodiments. In other embodiments, the gas pressure may range between 10 mTorr and 100 Torr and the substrate temperature may range between 0°C and -80°C.
  • the hydrogen plasma may react with the exposed surface of the silicon nitride layer to form a first reaction byproduct, which is vaporized at the gas pressure and the temperature of the substrate to form the first modified layer.
  • the first reaction byproduct may be ammonia (NH 3 ) and the first modified layer may be a silicon layer.
  • the hydrogen plasma may also react with the exposed surface of the oxide layer to produce a second reaction byproduct, which freezes at the gas pressure and the temperature of the substrate to create the crystallized water layer on the oxide layer and form the second modified layer.
  • the second reaction byproduct may be water (H2O) and the second modified layer may be a silicon dioxide layer.
  • the crystallized water layer may reduce etching of the oxide layer by preventing reactive species of the halogen plasma from reaching the second modified layer.
  • the first modified layer may be a silicon layer and the second modified layer may be a silicon dioxide layer.
  • the reactive species of the halogen plasma may selectively etch silicon over silicon dioxide to further reduce or eliminate etching of the oxide layer.
  • the method may further include generating the halogen plasma from one or more process gases, which have an etch selectivity of silicon to silicon dioxide of 5:1 or greater.
  • the one or more processing gases used to generate the halogen plasma may include one or more of chlorine (Cl2), hydrogen bromide (HBr), difluoride (F2), xenon difluoride (XeF2), tetrafluoromethane (CF 4 ), nitrogen trifluoride (NF 3 ) and sulfur hexafluoride (SF 6 ).
  • the method may include providing a substrate having a silicon nitride layer and an oxide layer exposed on a surface of the substrate, generating a hydrogen plasma at a gas pressure less than 1500 Torr and a temperature of the substrate less than or equal to 0°C and exposing the surface of the substrate to the hydrogen plasma.
  • the hydrogen plasma When exposed to the hydrogen plasma, the hydrogen plasma may: (a) react with an exposed surface of the silicon nitride layer to form a first reaction byproduct, which is vaporized at the gas pressure and the temperature of the substrate to form a first modified layer on the silicon nitride layer, and (b) react with an exposed surface of the oxide layer to produce a second reaction byproduct, which freezes at the gas pressure and the temperature of the substrate to create a crystallized water layer and form a second modified layer on the oxide layer.
  • the method may further include exposing the surface of the substrate to a halogen plasma to selectively etch the silicon nitride layer by removing the first modified layer without removing the second modified layer.
  • the method may further include repeating said exposing the surface of the substrate to the hydrogen plasma and said exposing the surface of the substrate to the halogen plasma a number of cycles to selectively etch a predetermined amount of the silicon nitride layer.
  • gas pressure may range between 10 mTorr and 1500 Torr and the substrate temperature may range between 0°C and - 80°C.
  • the crystallized water layer may reduce etching of the oxide layer by preventing reactive species of the halogen plasma from reaching the second modified layer.
  • the first modified layer may be a silicon layer and the second modified layer may be a silicon dioxide layer.
  • the reactive species of the halogen plasma may selectively etch silicon over silicon dioxide to further reduce or eliminate etching of the oxide layer.
  • the halogen plasma may be generated from one or more process gases, which have an etch selectivity of silicon to silicon dioxide of 5:1 or greater.
  • process gases may be used to generate the hydrogen plasma and the halogen plasma described herein.
  • the hydrogen plasma may be generated from one or more process gases including, but not limited to, hydrogen (H2), hydrogen bromide (HBr), methane (CH4) and hydrogen sulfide (H2S).
  • the halogen plasma may be generated from one or more process gases including, but not limited to, chlorine (Cl 2 ), hydrogen bromide (HBr), difluoride (F2), xenon difluoride (XeF2), tetrafluoromethane (CF4), nitrogen trifluoride (NF3) and sulfur hexafluoride (SF6).
  • the first reaction byproduct may be ammonia (NH 3 )
  • the first modified layer may be a silicon layer
  • the second reaction byproduct may be water (H 2 O)
  • the second modified layer may be a silicon dioxide layer.
  • the gas pressure used to generate the hydrogen plasma and the temperature of the substrate may: (a) vaporize the ammonia (NH 3 ) from the exposed surface of the silicon nitride layer to form the silicon layer, and (b) freeze the water (H2O) on the exposed surface of the oxide layer to create the crystallized water layer, which bonds with the exposed surface of the oxide layer to form the silicon dioxide layer.
  • the gas pressure used to generate the hydrogen plasma and the temperature of the substrate may be selected from a pressure-temperature window comprising a pressure range between 10 mTorr and 1500 Torr and a temperature range between 0°C and -80°C.
  • FIG.1 is a process flow diagram of an example embodiment of a cyclic, two-step dry etch process that utilizes sequential application of plasma etch steps, including a hydrogen plasma (in Step 1) followed by a halogen plasma (in Step 2), to selectively etch silicon nitride over oxide.
  • FIG.2 is a process flow diagram of an example embodiment of a cyclic, two-step dry etch process, which uses: (1) a hydrogen plasma to modify exposed surfaces of silicon nitride and oxide layers to form a modified silicon nitride surface layer and a modified oxide surface layer, and (2) a halogen plasma to selectively etch the silicon nitride layer by removing the modified silicon nitride surface layer without removing the modified oxide surface layer.
  • FIG. 3 is a phase diagram for ammonia (NH 3 ) and water (H 2 O) illustrating a pressure-temperature window, which may be used in the cyclic, two-step dry etch process described herein to select appropriate pressure and temperature conditions.
  • FIG.4 is a flow chart diagram illustrating one embodiment of a method that utilizes the techniques described herein to selectively etch silicon nitride over oxide.
  • FIG. 5 is a flow chart diagram illustrating another embodiment of a method that utilizes the techniques described herein to selectively etch silicon nitride over oxide.
  • FIG. 6 is a block diagram illustrating one embodiment of a plasma processing apparatus that can be used as an etch chamber for the embodiments described herein.
  • DETAILED DESCRIPTION [0028] The present disclosure provides various embodiments of improved processes and methods to provide selective etching of silicon nitride over oxide.
  • a cyclic, two-step dry etch process is used to selectively etch a silicon nitride layer formed on a substrate, while protecting an oxide layer formed on the same substrate.
  • the cyclic, two-step dry etch process disclosed herein sequentially exposes the substrate to: (1) a hydrogen plasma to modify exposed surfaces of the silicon nitride and oxide layers to form a modified silicon nitride surface layer and a modified oxide surface layer, and (2) a halogen plasma to selectively etch the silicon nitride layer by removing the modified silicon nitride surface layer without removing the modified oxide surface layer.
  • the oxide layer is protected from etching during the removal step (i.e., step 2) by creating a crystallized water layer on the oxide layer during the surface modification step (i.e., step 1).
  • the crystallized water layer improves selectivity of silicon nitride to oxide by providing a protective layer on the oxide layer, which prevents reactive species of the halogen plasma from reaching the modified oxide surface layer.
  • the process gas(es) used to generate the halogen plasma may further reduce (or eliminate) etching of the oxide layer by providing a highly selective etch of the modified silicon nitride surface layer to the modified oxide surface layer.
  • the embodiments disclosed herein create a protective water layer on the oxide layer by leveraging the different volatilities of reaction byproducts produced during the surface modification step (i.e., step 1).
  • a first reaction byproduct e.g., ammonia, NH 3
  • a second reaction byproduct e.g., water, H2O
  • the surface modification step pressure and temperature conditions are carefully selected, so as to vaporize NH3 leaving a silicon (Si) surface layer on the SiN layer, and freeze H 2 O leaving a crystallized water layer on the oxide layer.
  • the crystallized water layer protects the oxide layer during the subsequently performed removal step (i.e., step 2), thereby providing a two-step dry etch process that etches SiN over oxide with high etch selectivity. Since dry etch processes are utilized for both surface modification and removal, the two-step process described herein may be repeated in a cyclical manner to selectively etch a predetermined amount of SiN without significantly etching oxide.
  • FIG.1 is a process flow diagram of an example embodiment of a cyclic, two-step dry etch process 100 that may be used to selectively etch silicon nitride over oxide in accordance with the techniques described herein.
  • the cyclic, two-step dry etch process 100 shown in FIG.1 may be used to selectively etch silicon nitride layers formed on the substrate, while protecting oxide layers formed on the same substrate.
  • the dry etch process shown in FIG.1 may be performed on a wide variety of substrates, which may be disposed within a wide variety of plasma processing systems. Examples of plasma processing systems used to perform the dry etch process shown in FIG.
  • the dry etch process 100 shown in FIG.1 is cyclic, two-step process that generally includes a surface modification step (Step 1) followed by a removal step (Step 2).
  • the dry etch process 100 generates a hydrogen plasma within the plasma processing chamber at a gas pressure less than 1500 Torr and a substrate temperature less than 0°C (in block 110), and exposes a substrate having a silicon nitride (SiN) layer and an oxide (Ox) layer (e.g., SiO2) formed thereon to the hydrogen plasma to form a first modified layer on the SiN layer and a second modified layer on the oxide layer (in block 120).
  • SiN silicon nitride
  • Ox oxide
  • hydrogen ions within the hydrogen plasma (a) react with exposed SiN surfaces to remove nitrogen (N) atoms from the exposed SiN surfaces, and (b) react with exposed oxide surfaces to remove oxygen (O) atoms from the exposed oxide surfaces.
  • This reaction modifies the exposed SiN surfaces and the exposed oxide surfaces, leaving a first modified layer (e.g., a silicon layer) on the unmodified SiN layer and a second modified layer (e.g., an O-defected silicon dioxide layer) on the unmodified oxide layer.
  • the dry etch process 100 generates a halogen plasma within the plasma processing chamber (in block 130), and exposes the substrate to the halogen plasma (in block 140) to selectively etch the silicon nitride layer by removing the first modified layer without removing the second modified layer.
  • the first modified layer is etched at a significantly higher etch rate than the second modified layer to selectively etch the modified portions of the silicon nitride layer.
  • FIG.2 illustrates the surface modification step (Step 1) and the removal step (Step 2) in more detail.
  • a substrate comprising a SiN layer 200 and an oxide (Ox) layer 220 (e.g., SiO 2 ) is exposed to a hydrogen plasma 250 during the surface modification step (Step 1)
  • hydrogen ions within the hydrogen plasma 250 react with nitrogen (N) atoms on the exposed surfaces of the SiN layer 200 to produce a first reaction byproduct (e.g., ammonia, NH3), which is vaporized at the gas pressure within the plasma processing chamber and the substrate temperature to form a silicon (Si) layer 210 (i.e., a first modified layer) on the underlying, unmodified portions of the SiN layer 200.
  • a first reaction byproduct e.g., ammonia, NH3
  • the hydrogen ions within the hydrogen plasma 250 also react with oxygen (O) atoms on exposed surfaces of the oxide (Ox) layer 220 to produce a second reaction byproduct (e.g., water, H 2 O), which condenses and freezes at the gas pressure within the plasma processing chamber and the substrate temperature to create a crystallized water layer 230 on the oxide layer 220.
  • the crystallized water layer 230 forms an O-defected silicon dioxide (SiO 2-x ) layer 240 (i.e., a second modified layer) on the underlying, unmodified oxide layer 220, instead of a Si layer, through the formation of Si-O bonds.
  • the crystallized water layer 230 protects the oxide layer 220 from etching by preventing reactive species of the halogen plasma 260 from reaching the O-defected silicon dioxide (SiO2-x) layer 240 (i.e., a second modified layer) and the underlying, unmodified oxide layer 220.
  • SiO2-x O-defected silicon dioxide
  • the process gas(es) used to generate the halogen plasma 260 may further reduce (or eliminate) etching of the oxide layer 220 by providing high etch selectivity of the Si layer 210 (i.e., the first modified layer) to the O-defected silicon dioxide (SiO2-x) layer 240 (i.e., the second modified layer).
  • the process gas(es) used to generate the halogen plasma 260 may provide an etch selectivity of Si to SiO 2 of 5:1, or more preferably, 10:1 or greater.
  • halogen-containing gases may include, but are not limited to, hydrogen bromide (HBr), chlorine (Cl 2 ), difluoride (F 2 ), xenon difluoride (XeF 2 ) and other halogen-containing process gases.
  • HBr hydrogen bromide
  • Cl 2 chlorine
  • F 2 difluoride
  • XeF 2 xenon difluoride
  • This enables the Si layer 210 to be etched at a significantly higher etch rate than the O-defected silicon dioxide (SiO2-x) layer 240 during the removal step (Step 2).
  • the surface modification step (Step 1) and the removal step (Step 2) can be repeated one or more cycles (as needed) to remove a desired amount of SiN from the substrate, as indicated by arrow 270.
  • the surface modification step (Step 1) and the removal step (Step 2) can be repeated N cycles (where N ranges between 1 and 100) to remove a predetermined amount of the SiN layer 200, as shown for example, in FIG.2.
  • the dry etch process 100 provides one example of an improved process that may be used to selectively etch silicon nitride over oxide. As described above with respect to FIGS.
  • dry etch process 100 utilizes sequential surface modification and removal steps to selectively etch a silicon nitride layer on a substrate, without etching an oxide layer on the same substrate.
  • the silicon nitride layer can be implemented as silicon nitride (SiN), or as a silicon nitride material that includes SiN along with one or more other elements.
  • the silicon nitride layer may be a Silicon Carbonitride/Boron Nitride (SiBCN) spacer.
  • SiBCN Silicon Carbonitride/Boron Nitride
  • Other silicon nitride materials may also be selectively etched using the dry etch process 100 shown in FIGS.1 and 2.
  • the dry etch process 100 can be repeated a number of times to etch any desired amount of silicon nitride.
  • the surface modification step (Step 1) tends to have a practical limit to the depth of modified nitride that can be generated with a single exposure of the silicon nitride layer to the hydrogen plasma. As such, sequential use of the surface modification and removal steps would typically be used to remove a predetermined or desired amount of the silicon nitride layer from the surface of the substrate.
  • Step 1 and 2 may be include additional process step(s) before and/or after the surface modification step (Step 1) and/or the removal step (Step 2).
  • purge steps may be performed between the surface modification step (Step 1) and/or the removal step (Step 2) to remove process gases from the processing space of the plasma processing chamber.
  • Other variations can also be implemented while still taking advantage of the techniques described herein.
  • a wide variety of plasma process systems, parameters and process conditions may be utilized to provide selective etching of silicon nitride layers over oxide layers formed on a substrate in accordance with the techniques described herein.
  • plasma processing equipment such as, e.g., a CCP or ICP processing system
  • the plasma processing equipment may also allow a selected gas pressure (P) to be applied within the processing chamber, a selected temperature (T) to be applied to the substrate, a selected radio frequency (RF) energy to be applied to the processing chamber, and a duration of the plasma processing steps to be controlled.
  • P gas pressure
  • T selected temperature
  • RF radio frequency
  • a wide variety of processing gases can be utilized to generate the hydrogen plasma used in Step 1 and the halogen plasma used in Step 2 under a wide variety of process conditions.
  • the hydrogen plasma may be generated by injecting one or more hydrogen containing gases, such as hydrogen (H 2 ), hydrogen bromide (HBr), methane (CH 4 ) or hydrogen sulfide (H2S), into the process chamber.
  • hydrogen containing gases such as hydrogen (H 2 ), hydrogen bromide (HBr), methane (CH 4 ) or hydrogen sulfide (H2S)
  • H2S hydrogen sulfide
  • the process chamber is maintained at a sufficient gas pressure (e.g., less than 1500 Torr) and substrate temperature (e.g., less than 0°C) to vaporize the first reaction byproduct (e.g., NH 3 ) and freeze or crystallize the second reaction byproduct (e.g., H2O) during the surface modification step (Step 1).
  • the halogen plasma may be generated by injecting one or more halogen-containing gases, such as hydrogen bromide (HBr), chlorine (Cl 2 ), difluoride (F 2 ), xenon difluoride (XeF2), tetrafluoromethane (CF4), nitrogen trifluoride (NF3) or sulfur hexafluoride (SF6), into the process chamber.
  • halogen-containing gases such as hydrogen bromide (HBr), chlorine (Cl 2 ), difluoride (F 2 ), xenon difluoride (XeF2), tetrafluoromethane (CF4), nitrogen trifluoride (NF3) or sulfur hexafluoride (SF6).
  • halogen-containing gases such as hydrogen bromide (HBr), chlorine (Cl 2 ), difluoride (F 2 ), xenon difluoride (XeF2), tetrafluoromethane (CF4), nitrogen trifluoride (NF3) or sulfur
  • the following parameters set forth in the TABLE below may be used in the dry etch process 100 shown in FIGS.1-2 to provide selective etching of silicon nitride layers over oxide layers in accordance with the techniques described herein.
  • the gas pressure is expressed in Torr; the substrate temperature is expressed in degrees Celsius (°C); the radio frequency (RF) energy is expressed in Watts (W); and the duration is expressed in seconds (sec).
  • the hydrogen plasma used in Step 1 may be generated, in one embodiment, by supplying hydrogen (H2) and argon (Ar) gases to a process chamber maintained at a gas pressure range between 0.01 - 1500 Torr and a substrate temperature range -150°C - 20°C. In some embodiments, the gas pressure may range between 0.01 - 100 Torr and a substrate temperature range -80°C - 0°C, as noted further herein. While supplying the process gases to the process chamber, RF energy between 10W - 1000W may be supplied to one or more electrodes to ignite the process gases and generate the hydrogen plasma within the process chamber.
  • a substrate disposed within the process chamber may be exposed to the hydrogen plasma for approximately 5 - 300 seconds to perform the surface modification step (Step 1) shown in FIGS.1 and 2.
  • a hydrogen-containing gas e.g., H 2
  • Table 1 one example hydrogen-containing gas (e.g., H 2 ) is illustrated in Table 1, other hydrogen-containing gases and/or inert gases may also be supplied to the process chamber to generate the hydrogen plasma used in Step 1.
  • the halogen plasma used in Step 2 may be generated, in one embodiment, by supplying hydrogen bromide (HBr) gas to a process chamber maintained at a gas pressure range between 0.01 - 1500 Torr and a substrate temperature range -150°C - 20°C.
  • HBr hydrogen bromide
  • a higher gas pressure and a lower substrate temperature may be selected from the range provided above to generate the halogen.
  • RF energy between 10W - 1000W may be supplied to one or more electrodes to ignite the process gases and generate the halogen plasma within the process chamber.
  • a substrate disposed within the process chamber may be exposed to the halogen plasma for approximately 5 - 180 seconds to perform the removal step (Step 2) shown in FIGS.1 and 2.
  • halogen-containing gas e.g., HBr
  • other halogen-containing gases and/or inert gases may also be supplied to the process chamber to generate the halogen plasma used in Step 2.
  • the dry etch process 100 shown in FIGS.1 and 2 improves dry etch selectivity of silicon nitride to oxide, and prevents oxide layers from etching, by leveraging the different volatilities of reaction byproducts (e.g., NH 3 and H 2 O) produced during the surface modification step (Step 1).
  • FIG.3 provides a phase diagram 300 for ammonia (NH3) and water (H2O) at various gas pressures (Torr) and substrate temperatures (°C).
  • ammonia (NH3) is vaporized into a gas at gas pressures and substrate temperatures below phase curve 310, and is condensed into a liquid at gas pressures and substrate temperatures above phase curve 310.
  • water (H2O) is vaporized into a gas at gas pressures and substrate temperatures below phase curve 320, condensed into a liquid at gas pressures above phase curve 320 and substrate temperatures above 0°C, and frozen (or crystallized) into a solid at gas pressures above phase curve 320 and substrate temperatures below 0°C.
  • the dry etch process 100 shown in FIGS.1 and 2 takes advantage of the different volatilities of ammonia (NH 3 ) and water (H 2 O) to ensure that NH 3 is vaporized from the exposed SiN surfaces and H 2 O is crystallized on the exposed oxide surfaces during the surface modification step (Step 1).
  • NH 3 ammonia
  • H 2 O water
  • FIGS. 4 and 5 illustrate embodiments of exemplary methods that utilize the techniques described herein to provide selective etching of silicon nitride layers over oxide layers formed on a substrate. It will be recognized that the embodiments shown in FIGS.4 and 5 are merely exemplary and additional methods may utilize the techniques described herein.
  • FIG. 4 illustrates one embodiment of a method 400 that utilizes the techniques described herein to provide selective etching of silicon nitride layers over oxide layers formed on a substrate.
  • the method 400 may include providing a substrate having a silicon nitride layer and an oxide layer exposed on a surface of the substrate (in step 410) and exposing the surface of the substrate to a hydrogen plasma (in step 420) to: (a) modify an exposed surface of the silicon nitride layer to form a first modified layer, and (b) modify an exposed surface of the oxide layer to form a second modified layer, wherein a gas pressure used to generate the hydrogen plasma and a temperature of the substrate create a crystallized water layer, which bonds with the oxide layer to form the second modified layer.
  • the method 400 may further include exposing the surface of the substrate to a halogen plasma to selectively etch the silicon nitride layer by removing the first modified layer without removing the second modified layer (in step 430), and repeating said exposing the surface of the substrate to the hydrogen plasma and said exposing the surface of the substrate to the halogen plasma one or more times until a predetermined amount of the silicon nitride layer is selectively etched (in step 440).
  • FIG.5 illustrates another embodiment of a method 500 that utilizes the techniques described herein to provide selective etching of silicon nitride layers over oxide layers formed on a substrate.
  • the method 500 may begin by providing a substrate having a silicon nitride layer and an oxide layer exposed on a surface of the substrate (in step 510).
  • the method 500 may include generating a hydrogen plasma at a gas pressure less than 1500 Torr and a temperature of the substrate less than or equal to 0°C (in step 520) and exposing the surface of the substrate to the hydrogen plasma (in step 530).
  • the hydrogen plasma step 530, the hydrogen plasma: (a) reacts with an exposed surface of the silicon nitride layer to form a first reaction byproduct, which is vaporized at the gas pressure and the temperature of the substrate to form a first modified layer on the silicon nitride layer, and (b) reacts with an exposed surface of the oxide layer to produce a second reaction byproduct, which freezes at the gas pressure and the temperature of the substrate to create a crystallized water layer and form a second modified layer on the oxide layer.
  • a first reaction byproduct which is vaporized at the gas pressure and the temperature of the substrate to form a first modified layer on the silicon nitride layer
  • a second reaction byproduct which freezes at the gas pressure and the temperature of the substrate to create a crystallized water layer and form a second modified layer on the oxide layer.
  • the method 500 may further include exposing the surface of the substrate to a halogen plasma (in step 540) to selectively etch the silicon nitride layer by removing the first modified layer without removing the second modified layer.
  • the method 500 may further include repeating said exposing the surface of the substrate to the hydrogen plasma (in step 530) and said exposing the surface of the substrate to the halogen plasma (in step 540) a number of cycles to selectively etch a predetermined amount of the silicon nitride layer.
  • the methods 400 and 500 shown in FIGS. 4 and 5 provide various examples of improved methods that may be used to selectively etch silicon nitride over oxide.
  • the methods 400, 500 improve selectivity of silicon nitride over oxide by creating a crystallized water layer on the oxide layer during the surface modification step (i.e., in steps 420 and 530) used to form the first modified layer and the second modified layer.
  • the crystallized water layer prevents reactive species of the halogen plasma from reaching the second modified layer to reduce etching of the oxide layer.
  • the methods 400, 500 shown in FIGS.4 and 5 improve dry etch selectivity of silicon nitride to oxide, and prevent the oxide layer from etching, by leveraging the different volatilities of reaction byproducts produced during the surface modification step (i.e., in steps 420 and 530).
  • the hydrogen plasma reacts with the exposed surface of the silicon nitride layer to form a first reaction byproduct (e.g., ammonia, NH3), which is vaporized at the gas pressure and the temperature of the substrate to form the first modified layer (e.g., a silicon layer) on the silicon nitride layer.
  • a first reaction byproduct e.g., ammonia, NH3
  • the hydrogen plasma also reacts with the exposed surface of the oxide layer to produce a second reaction byproduct (e.g., water, H2O), which freezes at the gas pressure and the temperature of the substrate to create the crystallized water layer on the oxide layer and form the second modified layer (e.g., a silicon dioxide layer) on the oxide layer.
  • a second reaction byproduct e.g., water, H2O
  • the gas pressure used to generate the hydrogen plasma and the temperature of the substrate are selected from a pressure-temperature window, which: (a) vaporizes the ammonia (NH 3 ) from the exposed surface of the silicon nitride layer to form the silicon layer, and (b) freezes the water (H2O) condensed on the exposed surface of the oxide layer to create the crystallized water layer, which bonds with the exposed surface of the oxide layer to form the silicon dioxide layer.
  • the gas pressure used to generate the hydrogen plasma and the temperature of the substrate may be selected from a pressure-temperature window that includes a pressure range between 10 mTorr and 1500 Torr and a temperature range between 20°C and -150°C.
  • the gas pressure used to generate the hydrogen plasma and the temperature of the substrate may be selected from a pressure- temperature window that includes a pressure range between 10 mTorr and 100 Torr and a temperature range between 0°C and -80°C.
  • the methods 400, 500 may further reduce (or eliminate) etching of the oxide layer by selecting the appropriate process gas(es) used to selectively etch the silicon nitride layer in steps 430 and 540.
  • the first modified layer may be a silicon layer and the second modified layer may be a silicon dioxide layer.
  • the reactive species of the halogen plasma may be chosen to selectively etch silicon over silicon dioxide to further reduce or eliminate etching of the oxide layer.
  • processing gases that may be used to selectively etch silicon over silicon dioxide include halogen-containing gases, such as but are not limited to, chlorine (Cl2), hydrogen bromide (HBr), difluoride (F 2 ) and xenon difluoride (XeF2).
  • halogen-containing gases such as but are not limited to, chlorine (Cl2), hydrogen bromide (HBr), difluoride (F 2 ) and xenon difluoride (XeF2).
  • Other halogen-containing gases which have an etch selectivity of silicon to silicon dioxide of 5:1 or greater, may also be used to generate the halogen plasma.
  • CF4 tetrafluoromethane
  • NF3 nitrogen trifluoride
  • sulfur hexafluoride SF6
  • one or more deposition processes can be used to form the silicon nitride and oxide layers described herein as is well known to those skilled in the art.
  • one or more depositions can be implemented using chemical vapor deposition (CVD), plasma enhanced CVD (PECVD), physical vapor deposition (PVD), atomic layer deposition (ALD), and/or other deposition processes utilizing any of a wide-ranging deposition.
  • CVD chemical vapor deposition
  • PECVD plasma enhanced CVD
  • PVD physical vapor deposition
  • ALD atomic layer deposition
  • Lithography processes with respect to PR layers can be implemented using optical lithography, extreme ultra-violet (EUV) lithography, and/or other lithography processes.
  • EUV extreme ultra-violet
  • the etch processes utilized to selectively etch silicon nitride over oxide can be implemented using plasma etch processes, discharge etch processes, and/or other desired etch processes.
  • plasma etch processes can be implemented using hydrogen-containing gases and halogen-containing gases in combination with one or more dilution gases (e.g., argon, nitrogen, etc.), though other techniques may be utilized.
  • operating variables for process steps can be controlled to ensure that desired etch parameters are achieved.
  • the operating variables may include, for example, the chamber temperature, chamber pressure, flowrates of gases, frequency and/or power applied to electrode assembly in the generation of plasma, and/or other operating variables for the processing steps. Variations can also be implemented while still taking advantage of the techniques described herein.
  • the improved processes and methods described above may be performed using a wide variety of plasma processing systems.
  • One embodiment of an example plasma processing system 600 is described with respect to FIG.6.
  • FIG.6 provides a block diagram of an example plasma processing system 600 that can be used as an etch chamber for the embodiments described herein. More specifically, FIG. 6 provides a schematic cross-sectional view of a capacitively coupled plasma (CCP) processing system 600 that includes a process space (PS), or process chamber, for receiving and processing semiconductor substrates.
  • CCP capacitively coupled plasma
  • PS process space
  • plasma processing systems may also be utilized, including for example, but not limited to, inductively coupled plasma (ICP) processing systems, microwave plasma processing systems, and the like.
  • ICP inductively coupled plasma
  • a CCP processing system may be particularly well suited for practicing the techniques described herein as the electrode spacing of such a system allows for beneficial control of gases to a localized region of the plasma space, thus providing localized plasma processing on the substrate.
  • the plasma processing system 600 can be used for multiple operations including ashing, etching, deposition, cleaning, plasma polymerization, plasma-enhanced chemical vapor deposition (PECVD), atomic layer deposition (ALD), and so forth.
  • PECVD plasma-enhanced chemical vapor deposition
  • ALD atomic layer deposition
  • the structure of the CCP processing system 600 is well known, and the particular structure provided herein is merely exemplary.
  • plasma processing can be executed within processing chamber 601, which can be a vacuum chamber made of a metal such as aluminum or stainless steel.
  • the processing chamber 601 defines a processing vessel providing a process space (PS) for plasma generation.
  • An inner wall of the processing vessel can be coated with alumina, yttria, or another protectant.
  • the processing vessel can be cylindrical in shape or have other geometric configurations.
  • a susceptor 612 (which can be disc-shaped) can serve as a mounting table on which, for example, a substrate 602 to be processed (such as a semiconductor wafer) can be mounted.
  • Substrate 602 can be moved into the processing chamber 601 through a loading/unloading port and gate valve.
  • Susceptor 612 forms part of a lower electrode assembly 620 as an example of a second electrode acting as a mounting table for mounting substrate 602 thereon.
  • the susceptor 612 can be formed of, e.g., an aluminum alloy.
  • Susceptor 612 is provided thereon with an electrostatic chuck (as part of the lower electrode assembly) for holding the substrate 602.
  • the electrostatic chuck is provided with an electrode 635.
  • Electrode 635 is electrically connected to a direct current (DC) power source (not shown).
  • the electrostatic chuck attracts the substrate 602 thereto via an electrostatic force generated when DC voltage from the DC power source is applied to the electrode 635.
  • the susceptor 612 can be electrically connected to a high-frequency power source via a matching unit.
  • two or more power sources can be used and connected to electrode 635 and/or other electrodes within the processing chamber.
  • This high-frequency power source (a second power source) can output a high- frequency voltage in a range from, for example, 2 MHz (megahertz) to 20 MHz.
  • Applying high frequency bias power causes ions, in plasma generated within the processing chamber 601, to be attracted to substrate 602.
  • a focus ring assembly 638 is provided on an upper surface of the susceptor 612 to surround the electrostatic chuck.
  • An exhaust path 633 can be formed through one or more exhaust ports (not shown) which connect to a gas exhaust unit.
  • the gas exhaust unit can include a vacuum pump such as a turbo molecular pump configured to pump out the plasma processing space within the processing chamber 601 to a desired vacuum condition.
  • the gas exhaust unit evacuates the inside of the processing chamber 601 thereby depressurizing the inner pressure thereof down to the desired degree of vacuum.
  • An upper electrode assembly 670 is an example of a first electrode and is positioned vertically above the lower electrode assembly 620 to face the lower electrode assembly 620 in parallel.
  • the plasma generation space, or process space (PS) is defined between the lower electrode assembly 620 and the upper electrode assembly 670.
  • the upper electrode assembly 670 includes an inner upper electrode 671, having a disk shape, and an outer upper electrode which may be annular and surrounding a periphery of the inner upper electrode 671.
  • the inner upper electrode 671 also functions as a processing gas inlet for injecting a specific amount of processing gas into the process space (PS) above substrate 602 mounted on the lower electrode assembly 620.
  • the upper electrode assembly 670 thereby forms a showerhead. More specifically, the inner upper electrode 671 includes gas injection openings 682.
  • the upper electrode assembly 670 may include one or more buffer chamber(s) 689A, 689B, and 689C.
  • the buffer chambers are used for diffusing process gas and can define a disk-shaped space.
  • Processing gas from a process gas supply system 680 supplies gas to the upper electrode assembly 670.
  • the process gas supply system 680 can be configured to supply a processing gas for performing specific processes, such as film-forming, etching, and the like, on the substrate 602.
  • the process gas supply system 680 is connected to gas supply lines 681A, 681B, and 681C forming a processing gas supply path.
  • the gas supply lines are connected to the buffer chambers of the inner upper electrode 671.
  • the processing gas can then move from the buffer chambers to the gas injection openings 682 at a lower surface thereof.
  • a flow rate of processing gas introduced into the buffer chambers 689A-C can be adjusted, e.g., by using a mass flow controller. Further, the processing gas introduced is discharged from the gas injection openings 682 of the electrode plate (showerhead electrode) to the process space (PS).
  • the inner upper electrode 671 functions in part to provide a showerhead electrode assembly. [0061] As shown in FIG.
  • three buffer chambers 689A, 689B, and 689C are provided corresponding to edge buffer chamber 689A, middle buffer chamber 689B, and center buffer chamber 689C.
  • gas supply lines 681A, 681B, and 681C may be configured as edge gas supply line 681A, middle gas supply line 681B and center gas supply line 681C.
  • the buffer chambers are provided in a manner corresponding to different localized regions of the substrate in this case edge, middle and center. As will be discussed more below, these regions may correspond to specific process plasma process conditions for localized regions of the substrate 602. It will be recognized that the use of three localized regions is merely exemplary. Thus, the plasma processing apparatus may be configured to provided localize plasma process conditions on any number of regions of the substrate.
  • the upper electrode assembly 670 is electrically connected with a high-frequency power source (not shown) (first high-frequency power source) via a power feeder 665 and a matching unit 668.
  • the high-frequency power source can output a high-frequency voltage having a frequency of 40 MHz (megahertz) or higher (e.g., 60 MHz), or can output a very high frequency (VHF) voltage having a frequency of 30-300 MHz.
  • This power source can be referred to as the main power supply as compared to a bias power supply.
  • the plasma processing apparatus can be connected to, and controlled by, a control unit, which in turn can be connected to a corresponding memory storage unit and user interface (all not shown).
  • a control unit which in turn can be connected to a corresponding memory storage unit and user interface (all not shown).
  • Various plasma processing operations can be executed via the user interface, and various plasma processing recipes and operations can be stored in a storage unit. Accordingly, a given substrate can be processed within the plasma processing chamber with various microfabrication techniques.
  • the plasma processing apparatus uses the upper and lower electrodes to generate a plasma in the process space (PS).
  • This generated plasma can then be used for processing a target substrate (such as substrate 602 or any material to be processed) in various types of treatments such as plasma etching, chemical vapor deposition, treatment of semiconductor material, glass material and large panels such as thin- film solar cells, other photovoltaic cells, and organic/inorganic plates for flat panel displays, etc.
  • a target substrate such as substrate 602 or any material to be processed
  • treatments such as plasma etching, chemical vapor deposition, treatment of semiconductor material, glass material and large panels such as thin- film solar cells, other photovoltaic cells, and organic/inorganic plates for flat panel displays, etc.
  • substrate means and includes a base material or construction upon which materials are formed. It will be appreciated that the substrate may include a single material, a plurality of layers of different materials, a layer or layers having regions of different materials or different structures in them, etc. These materials may include semiconductors, insulators, conductors, or combinations thereof.
  • the substrate may be a semiconductor substrate, a base semiconductor layer on a supporting structure, a metal electrode or a semiconductor substrate having one or more layers, structures or regions formed thereon.
  • the substrate may be a conventional silicon substrate or other bulk substrate comprising a layer of semi-conductive material.
  • the term “bulk substrate” means and includes not only silicon wafers, but also silicon-on-insulator (“SOI”) substrates, such as silicon-on-sapphire (“SOS”) substrates and silicon-on-glass (“SOG”) substrates, epitaxial layers of silicon on a base semiconductor foundation, and other semiconductor or optoelectronic materials, such as silicon-germanium, germanium, gallium arsenide, gallium nitride, and indium phosphide.
  • SOI silicon-on-insulator
  • SOS silicon-on-sapphire
  • SOOG silicon-on-glass
  • the substrate may be doped or undoped.

Landscapes

  • Drying Of Semiconductors (AREA)
  • Weting (AREA)
PCT/US2023/032042 2022-10-18 2023-09-06 Method to selectively etch silicon nitride to silicon oxide using water crystallization Ceased WO2024085970A1 (en)

Priority Applications (3)

Application Number Priority Date Filing Date Title
KR1020257015143A KR20250091229A (ko) 2022-10-18 2023-09-06 물 결정화를 사용하여 산화규소에 대해 질화규소를 선택적으로 에칭하는 방법
JP2025522154A JP2025534555A (ja) 2022-10-18 2023-09-06 水の結晶化を使用してケイ素酸化物に対してケイ素窒化物を選択的にエッチングする方法
CN202380070418.7A CN119968697A (zh) 2022-10-18 2023-09-06 使用水结晶相对于氧化硅选择性蚀刻氮化硅的方法

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
US17/967,996 US12424447B2 (en) 2022-10-18 2022-10-18 Method to selectively etch silicon nitride to silicon oxide using water crystallization
US17/967,996 2022-10-18

Publications (2)

Publication Number Publication Date
WO2024085970A1 true WO2024085970A1 (en) 2024-04-25
WO2024085970A8 WO2024085970A8 (en) 2025-05-22

Family

ID=90626859

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/US2023/032042 Ceased WO2024085970A1 (en) 2022-10-18 2023-09-06 Method to selectively etch silicon nitride to silicon oxide using water crystallization

Country Status (6)

Country Link
US (1) US12424447B2 (enExample)
JP (1) JP2025534555A (enExample)
KR (1) KR20250091229A (enExample)
CN (1) CN119968697A (enExample)
TW (1) TW202433596A (enExample)
WO (1) WO2024085970A1 (enExample)

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2026054927A1 (en) * 2024-09-04 2026-03-12 Applied Materials, Inc. Ion beam-induced epitaxial crystallization on an integrated processing architecture

Families Citing this family (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
KR102323579B1 (ko) * 2020-12-18 2021-11-09 피에스케이 주식회사 기판 처리 방법 및 기판 처리 장치

Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2015099789A1 (en) * 2013-12-27 2015-07-02 Intel Corporation Technologies for selectively etching oxide and nitride materials and products formed using the same
US20180166303A1 (en) * 2016-12-13 2018-06-14 Tokyo Electron Limited Method of selectively etching first region made of silicon nitride against second region made of silicon oxide
US20180350617A1 (en) * 2017-05-31 2018-12-06 Applied Materials, Inc. Water-free etching methods
US20200027740A1 (en) * 2018-07-20 2020-01-23 Asm Ip Holding B.V. Selective cyclic dry etching process of dielectric materials using plasma modification
WO2020160437A1 (en) * 2019-02-01 2020-08-06 L'air Liquide, Societe Anonyme Pour L'etude Et L'exploitation Des Procedes Georges Claude Method to improve profile control during selectively etching of silicon nitride spacers

Family Cites Families (14)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US5786276A (en) 1997-03-31 1998-07-28 Applied Materials, Inc. Selective plasma etching of silicon nitride in presence of silicon or silicon oxides using mixture of CH3F or CH2F2 and CF4 and O2
US20060292883A1 (en) 2005-06-28 2006-12-28 Chang-Hu Tsai Etching of silicon nitride with improved nitride-to-oxide selectivity utilizing halogen bromide/chlorine plasma
US8187486B1 (en) 2007-12-13 2012-05-29 Novellus Systems, Inc. Modulating etch selectivity and etch rate of silicon nitride thin films
US8501630B2 (en) 2010-09-28 2013-08-06 Tokyo Electron Limited Selective etch process for silicon nitride
US20160181116A1 (en) 2014-12-18 2016-06-23 Lam Research Corporation Selective nitride etch
US10629473B2 (en) 2016-09-09 2020-04-21 Applied Materials, Inc. Footing removal for nitride spacer
US9899515B1 (en) 2016-10-31 2018-02-20 International Business Machines Corporation Fabrication of a pair of vertical fin field effect transistors having a merged top source/drain
US10026621B2 (en) 2016-11-14 2018-07-17 Applied Materials, Inc. SiN spacer profile patterning
US11469079B2 (en) 2017-03-14 2022-10-11 Lam Research Corporation Ultrahigh selective nitride etch to form FinFET devices
FR3065576B1 (fr) 2017-04-25 2020-01-24 Commissariat A L'energie Atomique Et Aux Energies Alternatives Procede de gravure d'une couche a base de sin
US10510838B2 (en) 2017-11-29 2019-12-17 Taiwan Semiconductor Manufacturing Co., Ltd. High surface dopant concentration formation processes and structures formed thereby
US10818507B2 (en) 2018-05-11 2020-10-27 Tokyo Electron Limited Method of etching silicon nitride layers for the manufacture of microelectronic workpieces
US10872778B2 (en) * 2018-07-06 2020-12-22 Applied Materials, Inc. Systems and methods utilizing solid-phase etchants
KR102345211B1 (ko) 2020-09-21 2022-01-03 주식회사 이엔에프테크놀로지 실리콘 질화막 식각 조성물 및 이를 이용한 방법

Patent Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2015099789A1 (en) * 2013-12-27 2015-07-02 Intel Corporation Technologies for selectively etching oxide and nitride materials and products formed using the same
US20180166303A1 (en) * 2016-12-13 2018-06-14 Tokyo Electron Limited Method of selectively etching first region made of silicon nitride against second region made of silicon oxide
US20180350617A1 (en) * 2017-05-31 2018-12-06 Applied Materials, Inc. Water-free etching methods
US20200027740A1 (en) * 2018-07-20 2020-01-23 Asm Ip Holding B.V. Selective cyclic dry etching process of dielectric materials using plasma modification
WO2020160437A1 (en) * 2019-02-01 2020-08-06 L'air Liquide, Societe Anonyme Pour L'etude Et L'exploitation Des Procedes Georges Claude Method to improve profile control during selectively etching of silicon nitride spacers

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2026054927A1 (en) * 2024-09-04 2026-03-12 Applied Materials, Inc. Ion beam-induced epitaxial crystallization on an integrated processing architecture

Also Published As

Publication number Publication date
CN119968697A (zh) 2025-05-09
US20240128089A1 (en) 2024-04-18
WO2024085970A8 (en) 2025-05-22
US12424447B2 (en) 2025-09-23
KR20250091229A (ko) 2025-06-20
TW202433596A (zh) 2024-08-16
JP2025534555A (ja) 2025-10-16

Similar Documents

Publication Publication Date Title
KR102564160B1 (ko) 펄스된 저주파수 rf 전력에 의한 고 선택도 및 저 응력의 탄소 하드마스크
US12482663B2 (en) Processing apparatus
US9269587B2 (en) Methods for etching materials using synchronized RF pulses
US9666414B2 (en) Process chamber for etching low k and other dielectric films
TWI774688B (zh) 蝕刻處理中保護超低介電材料不受損害以得到期望的特徵部之製造方法
US8592327B2 (en) Formation of SiOCl-containing layer on exposed low-k surfaces to reduce low-k damage
WO2004006303A2 (en) Method for fabricating an ultra shallow junction of a field effect transistor
US11342195B1 (en) Methods for anisotropic etch of silicon-based materials with selectivity to organic materials
US12463046B2 (en) Silicon-and-germanium etching
US12424447B2 (en) Method to selectively etch silicon nitride to silicon oxide using water crystallization
US10818507B2 (en) Method of etching silicon nitride layers for the manufacture of microelectronic workpieces
JP2022533388A (ja) in-situ原子層堆積プロセス
US20260005030A1 (en) Selective etching between silicon-and-germanium-containing materials with varying germanium concentrations
US9472416B2 (en) Methods of surface interface engineering
US12394631B2 (en) Selective etching of silicon-and-germanium-containing materials with increased surface purities
US10283370B1 (en) Silicon addition for silicon nitride etching selectivity
US20250331267A1 (en) Self-limited etching of low-k materials
US20250259850A1 (en) Selective etching of silicon-and-germanium-containing materials with reduced under layer loss
US11495436B2 (en) Systems and methods to control critical dimension (CD) shrink ratio through radio frequency (RF) pulsing
US20260052918A1 (en) Selective etching of silicon-and-germanium-containing material
WO2026084923A1 (en) Processing methods to improve etched silicon-and-germanium-containing material surface properties
WO2026039271A1 (en) Selective etching of silicon-containing material

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 23880399

Country of ref document: EP

Kind code of ref document: A1

WWE Wipo information: entry into national phase

Ref document number: 202380070418.7

Country of ref document: CN

ENP Entry into the national phase

Ref document number: 2025522154

Country of ref document: JP

Kind code of ref document: A

WWE Wipo information: entry into national phase

Ref document number: 2025522154

Country of ref document: JP

ENP Entry into the national phase

Ref document number: 20257015143

Country of ref document: KR

Kind code of ref document: A

WWP Wipo information: published in national office

Ref document number: 202380070418.7

Country of ref document: CN

NENP Non-entry into the national phase

Ref country code: DE

WWP Wipo information: published in national office

Ref document number: 1020257015143

Country of ref document: KR

122 Ep: pct application non-entry in european phase

Ref document number: 23880399

Country of ref document: EP

Kind code of ref document: A1