WO2023166935A1 - 鋼板および鋼板の製造方法 - Google Patents
鋼板および鋼板の製造方法 Download PDFInfo
- Publication number
- WO2023166935A1 WO2023166935A1 PCT/JP2023/004276 JP2023004276W WO2023166935A1 WO 2023166935 A1 WO2023166935 A1 WO 2023166935A1 JP 2023004276 W JP2023004276 W JP 2023004276W WO 2023166935 A1 WO2023166935 A1 WO 2023166935A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- less
- steel sheet
- content
- steel
- toughness
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C38/00—Ferrous alloys, e.g. steel alloys
- C22C38/04—Ferrous alloys, e.g. steel alloys containing manganese
-
- C—CHEMISTRY; METALLURGY
- C21—METALLURGY OF IRON
- C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
- C21D8/00—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment
- C21D8/02—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips
-
- C—CHEMISTRY; METALLURGY
- C21—METALLURGY OF IRON
- C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
- C21D8/00—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment
- C21D8/02—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips
- C21D8/0221—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips characterised by the working steps
- C21D8/0226—Hot rolling
-
- C—CHEMISTRY; METALLURGY
- C21—METALLURGY OF IRON
- C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
- C21D8/00—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment
- C21D8/02—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips
- C21D8/0247—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips characterised by the heat treatment
- C21D8/0263—Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment during manufacturing of plates or strips characterised by the heat treatment following hot rolling
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C38/00—Ferrous alloys, e.g. steel alloys
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C38/00—Ferrous alloys, e.g. steel alloys
- C22C38/001—Ferrous alloys, e.g. steel alloys containing N
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C38/00—Ferrous alloys, e.g. steel alloys
- C22C38/002—Ferrous alloys, e.g. steel alloys containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C38/00—Ferrous alloys, e.g. steel alloys
- C22C38/005—Ferrous alloys, e.g. steel alloys containing rare earths, i.e. Sc, Y, Lanthanides
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C38/00—Ferrous alloys, e.g. steel alloys
- C22C38/02—Ferrous alloys, e.g. steel alloys containing silicon
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C38/00—Ferrous alloys, e.g. steel alloys
- C22C38/06—Ferrous alloys, e.g. steel alloys containing aluminium
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C38/00—Ferrous alloys, e.g. steel alloys
- C22C38/14—Ferrous alloys, e.g. steel alloys containing titanium or zirconium
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C38/00—Ferrous alloys, e.g. steel alloys
- C22C38/18—Ferrous alloys, e.g. steel alloys containing chromium
- C22C38/40—Ferrous alloys, e.g. steel alloys containing chromium with nickel
- C22C38/42—Ferrous alloys, e.g. steel alloys containing chromium with nickel with copper
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C38/00—Ferrous alloys, e.g. steel alloys
- C22C38/18—Ferrous alloys, e.g. steel alloys containing chromium
- C22C38/40—Ferrous alloys, e.g. steel alloys containing chromium with nickel
- C22C38/44—Ferrous alloys, e.g. steel alloys containing chromium with nickel with molybdenum or tungsten
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C38/00—Ferrous alloys, e.g. steel alloys
- C22C38/18—Ferrous alloys, e.g. steel alloys containing chromium
- C22C38/40—Ferrous alloys, e.g. steel alloys containing chromium with nickel
- C22C38/46—Ferrous alloys, e.g. steel alloys containing chromium with nickel with vanadium
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C38/00—Ferrous alloys, e.g. steel alloys
- C22C38/18—Ferrous alloys, e.g. steel alloys containing chromium
- C22C38/40—Ferrous alloys, e.g. steel alloys containing chromium with nickel
- C22C38/48—Ferrous alloys, e.g. steel alloys containing chromium with nickel with niobium or tantalum
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C38/00—Ferrous alloys, e.g. steel alloys
- C22C38/18—Ferrous alloys, e.g. steel alloys containing chromium
- C22C38/40—Ferrous alloys, e.g. steel alloys containing chromium with nickel
- C22C38/50—Ferrous alloys, e.g. steel alloys containing chromium with nickel with titanium or zirconium
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C38/00—Ferrous alloys, e.g. steel alloys
- C22C38/18—Ferrous alloys, e.g. steel alloys containing chromium
- C22C38/40—Ferrous alloys, e.g. steel alloys containing chromium with nickel
- C22C38/52—Ferrous alloys, e.g. steel alloys containing chromium with nickel with cobalt
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C38/00—Ferrous alloys, e.g. steel alloys
- C22C38/18—Ferrous alloys, e.g. steel alloys containing chromium
- C22C38/40—Ferrous alloys, e.g. steel alloys containing chromium with nickel
- C22C38/54—Ferrous alloys, e.g. steel alloys containing chromium with nickel with boron
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C38/00—Ferrous alloys, e.g. steel alloys
- C22C38/18—Ferrous alloys, e.g. steel alloys containing chromium
- C22C38/40—Ferrous alloys, e.g. steel alloys containing chromium with nickel
- C22C38/58—Ferrous alloys, e.g. steel alloys containing chromium with nickel with more than 1.5% by weight of manganese
-
- C—CHEMISTRY; METALLURGY
- C21—METALLURGY OF IRON
- C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
- C21D2211/00—Microstructure comprising significant phases
- C21D2211/005—Ferrite
-
- C—CHEMISTRY; METALLURGY
- C21—METALLURGY OF IRON
- C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
- C21D2211/00—Microstructure comprising significant phases
- C21D2211/009—Pearlite
Definitions
- the present invention provides a steel plate with excellent toughness and corrosion resistance that can be applied to high heat input welding, especially a multi-purpose tank for mixed loading of liquefied petroleum gas (hereinafter referred to as LPG) and liquefied ammonia (hereinafter referred to as a liquefied gas storage tank.
- LPG liquefied petroleum gas
- a liquefied gas storage tank liquefied gas storage tank.
- the present invention relates to a steel sheet excellent in low-temperature toughness and ammonia stress corrosion cracking resistance to be used in ) and a method for producing the same.
- liquefied gas storage tanks may carry not only LPG but also liquefied ammonia.
- the steel sheets used in liquefied gas storage tanks are required to have high low-temperature toughness.
- TS tensile strength
- liquefied ammonia is known to cause stress corrosion cracking of steel sheets, and the IMO gas code and ship classification regulations require that the yield strength (YS) be 440 MPa or less in order to minimize the risk of ammonia stress corrosion cracking. regulated by Therefore, the liquefied gas storage tank is required to have a high tensile strength of 490 MPa or more and a low yield strength of 440 MPa or less.
- Patent Documents 1 and 2 describe techniques for manufacturing steel that has the low-temperature toughness required for the liquefied gas storage tanks described above and that satisfies the strength range.
- high low-temperature toughness and predetermined strength characteristics are achieved by a method of tempering after quenching a hot-rolled thick steel plate several times.
- these methods have the problem of reducing the flatness of the steel sheet.
- the flatness that is a problem here means flatness such that the maximum value of the gap between the surface of the steel sheet and the long length exceeds 14 mm in a steel sheet having a thickness of less than 13 mm.
- HAZ Heat Affected Zone
- the austenite grains tend to coarsen, and such coarsened austenite grains are reduced by subsequent cooling. Transformation into an upper bainite structure containing island-shaped martensite, which is inferior in toughness, can be mentioned. As a result, the toughness of the HAZ is lowered.
- Patent Document 3 discloses a technique for suppressing coarsening of the austenite grain size in the HAZ by dispersing a large amount of TiN.
- Patent Document 4 discloses a technique for reducing island martensite (MA) in the HAZ by reducing the content of P as well as the content of C and Si.
- Patent Document 5 discloses a technique for achieving both brittle crack arrestability and HAZ toughness during high heat input welding by dispersing particles such as TiN in a ferrite-based microstructure with a refined grain size. ing.
- quenching is performed after hot rolling, so quenching is necessary. Especially when applied to a thin steel sheet having a thickness of less than 13 mm, quenching causes strain inside the steel sheet, There is a problem that the flatness of the steel plate is lowered.
- Patent Documents 3 and 5 which utilizes TiN to improve HAZ toughness during high heat input welding, heats the weld heat affected zone to the melting temperature range of TiN when subjected to high heat input welding. Therefore, there is a problem that TiN decomposes and the effect of TiN dispersion is reduced, and the solid solution Ti and solid solution N generated by the decomposition of TiN embrittle the ground structure of the steel, and the problem that the toughness of the HAZ is significantly reduced. was there.
- the present invention has a steel plate with a suitable strength range and the low temperature toughness of the base material (absorbed energy at -55 ° C. of 100 J or more) necessary for a liquefied gas storage tank.
- An object of the present invention is to provide a steel plate having excellent toughness (absorbed energy of 100 J or more at -55°C) in the HAZ of a joint after heat welding.
- Another object of the present invention is to provide a method for suitably manufacturing such a steel plate.
- the present inventors have developed low-temperature toughness and strength properties in the base metal portion of a steel plate, and toughness in the HAZ when welding with a large heat input (hereinafter, also referred to as HAZ toughness by welding with a large heat input. (1) to (3) below.
- high heat input welding refers to welding with a heat input of 10 kJ/cm or more and 20 kJ/cm or less.
- the amount of Ti and N in the steel sheet is such that the mass% ratio (Ti/N) of Ti and N is 2.00 or more and 4.00 or less, and formula (1) described later It was found that the dispersed state of TiN during high heat input welding is maintained by making the chemical composition that satisfies the condition of .
- the carbon equivalent (Ceq) represented by the formula (2) described later is controlled to 0.390 or less, and the content of C contained in the steel sheet is 0.090% or less. , it is important that the Si content be 0.10% or less. Furthermore, it is also necessary to set the Mn content to 1.800% or less and the Al content to 0.100% or less in order not to lower the HAZ toughness.
- the phrase "almost no MA is generated” means that the volume fraction of MA in the microstructure of the HAZ is 10% or less.
- the gist of the present invention is as follows. [1] % by mass, C: 0.060% or more and 0.090% or less, Si: 0.02% or more and 0.10% or less, Mn: 1.200% or more and 1.800% or less, P: 0.010% or less, S: 0.010% or less, Al: 0.020% or more and 0.100% or less, O: 0.0100% or less, Ti: 0.010% or more and 0.031% or less, N: 0.0038% or more and 0.0100% or less, Furthermore, Ti and N are contained in a range where Ti/N, which is the ratio of Ti and N, is 2.00 or more and 4.00 or less and satisfies the following formula (1), Furthermore, the carbon equivalent Ceq defined by the following formula (2) is 0.340 or more and 0.390 or less, Having a component composition in which the balance is Fe and unavoidable impurities, The total volume fraction of ferrite and pearlite at
- each element symbol represents the content (% by mass) of each component, and is set to 0 when not contained.
- the component composition further includes, in % by mass, Cu: 0.010% or more and 1.000% or less, Ni: 0.010% or more and 1.000% or less, Cr: 0.010% or more and 0.500% or less, Mo: 0.010% or more and 0.500% or less, V: 0.010% or more and 0.500% or less, W: 0.01% or more and 0.50% or less, Co: 0.01% or more and 0.50% or less, Nb: 0.005% or more and 0.050% or less, B: The steel sheet according to [1], containing one or more selected from 0.0001% or more and 0.0100% or less.
- the component composition further includes, in % by mass, Ca: 0.0005% or more and 0.0100% or less, Mg: 0.0005% or more and 0.0100% or less and REM: 0.0005% or more and 0.0200% or less containing one or more selected from [1] or [2] steel plate.
- a method for producing a steel sheet comprising hot rolling with a ratio of 65% or more and a rolling end temperature of Ar 3 transformation point or higher, followed by air cooling.
- the present invention has a tensile strength of 490 MPa or more and a yield strength of 440 MPa or less, so that it has excellent ammonia stress corrosion cracking resistance, and the absorbed energy at -55 ° C. is 100 J or more. It is possible to provide a steel plate having excellent toughness in the HAZ of the joint after high heat input welding, and excellent flatness even if the plate thickness is less than 13 mm, and a method for producing the same, which is industrially remarkable. effect.
- the steel sheet of the present invention will be specifically described.
- the steel plate and the steel material used to manufacture the steel plate have the above strength.
- “%” regarding a component composition shall mean “mass %” unless otherwise indicated.
- the thickness of the steel sheet manufactured by the present invention is less than 13 mm.
- the strength characteristics in the present invention are yield strength (YS (yield point YP when there is a yield point, 0.2% yield strength ⁇ 0.2 when there is no yield point)): 440 MPa or less and tensile strength (TS): 490 MPa or more.
- Yield strength (YS) is closely related to ammonia stress corrosion cracking resistance. The yield point is defined as 440 MPa or less in order to minimize the Therefore, it can be said empirically that if YS is 440 MPa or less, excellent ammonia stress corrosion cracking resistance is obtained.
- the yield strength YS for ensuring ammonia stress corrosion cracking resistance yield point YP when there is a yield point, 0.2% proof stress ⁇ 0.2 when there is no yield point
- the tensile strength (TS) of the steel sheet is preferably 620 MPa or less.
- the tensile strength (TS) of the steel sheet obtained by the present invention is substantially 620 MPa or less.
- C 0.060% or more and 0.090% or less C is an element that has the effect of increasing the strength of steel, and needs to be added to achieve high strength.
- the C content is made 0.060% or more.
- the C content is preferably 0.065% or more, more preferably 0.070% or more.
- the C content is preferably 0.085% or less, more preferably 0.080% or less.
- Si 0.02% or more and 0.10% or less
- Si is a component necessary for deoxidation and the like, and is an element that has the effect of increasing the strength of steel by forming a solid solution in ferrite.
- the Si content is made 0.02% or more.
- the Si content is preferably 0.03% or more, more preferably 0.04% or more, in order to reduce the content of other alloying elements and manufacture the steel sheet at a lower cost.
- the Si content is high, the toughness of the base material is deteriorated.
- the Si content is made 0.10% or less.
- the Si content is preferably 0.09% or less, more preferably 0.08% or less.
- Mn 1.200% or more and 1.800% or less
- Mn is an element that has the effect of increasing the hardenability of steel, and must be added to achieve high strength.
- the Mn content is set to 1.200% or more.
- the Mn content is preferably 1.300% or more, more preferably 1.400% or more, in order to reduce the content of other alloying elements and to manufacture at a lower cost.
- the Mn content is set to 1.800% or less.
- the Mn content is preferably 1.700% or less, more preferably 1.600% or less.
- P 0.010% or less
- P is an element contained in steel components as an unavoidable impurity, and when it segregates at grain boundaries, it has adverse effects such as lowering toughness and weldability. Therefore, it is desirable to reduce the P content as much as possible, but a P content of 0.010% or less is acceptable.
- the lower limit of the P content is not particularly limited and may be 0%, but usually P is an element that is unavoidably contained in steel as an impurity, so industrially it is more than 0%. you can Moreover, since an excessive reduction causes a rise in refining costs, the P content is preferably 0.0005% or more.
- S 0.010% or less
- S is an element contained in steel components as an unavoidable impurity. It is an element that adversely affects the toughness of the material and HAZ. Therefore, it is desirable to reduce the S content as much as possible, but 0.010% or less is permissible.
- the lower limit of the S content is not particularly limited, and may be 0%. However, since S is an element that is unavoidably contained in steel as an impurity, industrially it is not more than 0%. may That is, since an excessive reduction causes an increase in refining cost, it is preferable to set the S content to 0.0005% or more.
- Al 0.020% or more and 0.100% or less
- Al is an element that functions as a deoxidizing agent and has the effect of refining crystal grains and improving the toughness of the base material.
- the Al content should be 0.020% or more.
- the Al content is set to 0.100% or less.
- the Al content is preferably 0.080% or less, more preferably 0.060% or less.
- O 0.0100% or less
- O is an element contained in steel components as an unavoidable impurity. is an element. Therefore, the O content is limited to 0.0100% or less.
- the O content is preferably 0.0050% or less, more preferably 0.0030% or less.
- the lower limit of the O content is not particularly limited, and may be 0%, but usually O is an element that is unavoidably contained in steel as an impurity, so industrially it is more than 0%. you can That is, since excessive reduction causes a rise in refining cost, it is preferable to set the O content to 0.0020% or more from the viewpoint of cost.
- Ti and N precipitate and disperse as TiN during solidification of steel, suppress coarsening of austenite in the HAZ, and become ferrite transformation nuclei to contribute to high toughness.
- Ti/N 2.00 or more and 4.00 or less
- Ti/N is set to 2.00 or more.
- Ti/N is preferably 2.10 or more, more preferably 2.20 or more.
- the upper limit of Ti/N is set to 4.00. From the viewpoint of improving HAZ toughness, it is preferably 3.90 or less, more preferably 3.80 or less.
- each element is the content (% by mass) in the steel.
- the calculated value of the middle side of the above formula (1) should be 360 or less.
- it is preferably less than 360, more preferably 330 or less, and even more preferably 300 or less.
- each element symbol represents the content (% by mass) of each component, and is set to 0 when not contained.
- the range of the content of Ti and N is as specified above. It is as follows.
- Ti 0.010% or more and 0.031% or less Ti precipitates as TiN when the steel solidifies, suppresses coarsening of austenite in the HAZ, and serves as ferrite transformation nuclei to contribute to high toughness. It is one of the important elements in invention.
- the Ti content In order to secure the necessary amount of TiN, the Ti content should be 0.010% or more.
- the Ti content is preferably 0.012% or more, more preferably 0.014% or more.
- the addition exceeds 0.031%, a large amount of TiN is generated or the TiN particles are coarsened, and the expected effect cannot be obtained, and instead the toughness of the base metal and the toughness of the weld zone are lowered. Therefore, the Ti content should be 0.031% or less. In order to improve toughness, it is preferably 0.028% or less, more preferably 0.025% or less, and even more preferably 0.0022% or less.
- N is an element necessary for the formation of TiN described above, and the N content is made 0.0038% or more in order to secure the necessary amount of TiN.
- the N content is preferably 0.0040% or more, more preferably 0.0042% or more.
- the N content is set to 0.0100% or less. In order to improve toughness, the content is preferably 0.0090% or less, more preferably 0.0080% or less, even more preferably 0.0070% or less.
- Ceq is set to 0.390 or less.
- Ceq is 0.380 or less.
- Ceq is more preferably 0.370 or less, and even more preferably 0.360 or less.
- each element symbol represents the content (% by mass) of each component, and is set to 0 when not contained.
- the basic chemical composition of the steel sheet of the present invention contains each element in the content described above, and the balance is Fe and unavoidable impurities.
- this basic composition can optionally include Cu: 1.00% or less, Ni: 1.00% or less, Cr : 1.00% or less, Mo: 0.50% or less, V: 0.50% or less, W: 0.50% or less, Co: 0.50% or less, B: 0.0100% or less It can further contain one or two or more.
- Cu 0.010% or more and 1.000% or less
- Cu is an element that has the effect of increasing the hardenability of steel and improving the strength of the base material of the steel sheet, and can be optionally added.
- the Cu content is preferably 0.010% or more in order to obtain the above effect.
- the Cu content exceeds 1.000%, deterioration of toughness and an increase in alloy cost are caused. Therefore, when Cu is added, the Cu content is set to 1.000% or less.
- Cu content is more preferably 0.750% or less, and further preferably 0.500% or less.
- Ni 0.010% or more and 1.000% or less
- Ni is an element that has the effect of improving the strength of the base metal of the steel sheet, and can be optionally added.
- the Ni content is preferably 0.010% or more in order to obtain the above effect.
- the Ni content exceeds 1.000%, the weldability deteriorates and the alloy cost increases. Therefore, when Ni is added, the Ni content is made 1.00% or less. Note that the Ni content is more preferably 0.750% or less, and even more preferably 0.500% or less.
- Cr 0.010% or more and 0.500% or less Cr, like Cu, is an element that has the effect of improving the strength of the base material of the steel sheet, and can be optionally added.
- the Cr content is preferably 0.010% or more.
- the Cr content exceeds 0.500%, the weldability deteriorates and the alloy cost increases. Therefore, when Cr is added, the Cr content is made 0.500% or less.
- the Cr content is more preferably 0.050% or more, and more preferably 0.250% or less.
- Mo 0.010% or more and 0.500% or less
- Mo is an element that has the effect of improving the strength of the base material of the steel sheet, like Cu, and can be optionally added.
- the Mo content is preferably 0.010% or more.
- Mo content shall be 0.500% or less. Note that the Mo content is more preferably 0.050% or more, and more preferably 0.250% or less.
- V 0.010% or more and 0.500% or less
- V is an element having the effect of improving the strength of the base material of the steel sheet, like Cu, and can be optionally added.
- the V content is preferably 0.010% or more.
- the V content exceeds 0.500%, the weldability deteriorates and the alloy cost increases. Therefore, when V is added, the V content is made 0.500% or less.
- the V content is more preferably 0.050% or more, and more preferably 0.250% or less.
- W 0.01% or more and 0.50% or less W is an element having the effect of improving the strength of the base material of the steel sheet, like Cu, and can be optionally added.
- the W content is preferably 0.01% or more.
- the W content is more preferably 0.05% or more, and more preferably 0.25% or less.
- Co 0.01% or more and 0.50% or less
- Co is an element that has the effect of improving the strength of the steel sheet like Cu, and can be optionally added.
- the Co content is preferably 0.01% or more.
- the Co content is more preferably 0.05% or more, and more preferably 0.25% or less.
- Nb 0.005% or more and 0.050% or less
- Nb is an element that has the effect of reducing the grain size of prior austenite by precipitating as carbonitrides and improving the toughness of steel.
- the Nb content is made 0.005% or more to obtain the above effect.
- the Nb content is more preferably 0.007% or more.
- the Nb content exceeds 0.050%, a large amount of NbC precipitates, resulting in a decrease in toughness. Therefore, when Nb is added, the Nb content is made 0.050% or less.
- the Nb content is more preferably 0.040% or less, even more preferably 0.030% or less, and even more preferably 0.020% or less.
- B 0.0001% or more and 0.0100% or less B is an element that has the effect of significantly improving the hardenability of steel even when added in a very small amount. Therefore, the strength of the base material of the steel plate can be improved.
- the B content is preferably 0.0001% or more.
- coarse Fe—B-based carbides are formed. Such coarse Fe—B-based carbides act as starting points for fracture and significantly lower the toughness of the base metal and HAZ. Therefore, when B is added, the B content is made 0.0100% or less.
- the B content is more preferably 0.0050% or less, more preferably 0.0030% or less.
- Ca 0.0100% or less
- Mg 0.0100% or less
- REM 0.010% or less. 1 or 2 or more selected from 0200% or less can be further contained.
- Ca 0.0005% or more and 0.0100% or less
- Ca is an element that binds to S and has the effect of suppressing the formation of MnS or the like that elongates in the rolling direction of the steel sheet. Therefore, by adding Ca, it is possible to control the morphology of the sulfide-based inclusions so that they exhibit a spherical shape, and improve the toughness of welded joints and the like.
- the Ca content is preferably 0.0005% or more, more preferably 0.0020% or more.
- the Ca content exceeds 0.0100%, the cleanliness of the steel is lowered and the HAZ toughness is lowered. Therefore, when Ca is added, the Ca content is set to 0.0100% or less. Also, the Ca content is more preferably 0.0075% or less, and even more preferably 0.0050% or less.
- Mg 0.0005% to 0.0100%
- Mg is an element that binds to S and has the effect of suppressing the formation of MnS or the like that elongates in the rolling direction of the steel sheet. Therefore, by adding Mg, the morphology of the sulfide-based inclusions can be controlled so as to exhibit a spherical shape, and the toughness of welded joints and the like can be improved.
- the Mg content is preferably 0.0005% or more, more preferably 0.0020% or more.
- the Mg content exceeds 0.0100%, the cleanliness of the steel is lowered, and the HAZ toughness is lowered. Therefore, when Mg is added, the Mg content is made 0.0100% or less.
- the Mg content is more preferably 0.0075% or less, and even more preferably 0.0050% or less.
- REM 0.0005% or more and 0.0200% or less REM (rare earth metal), like Ca and Mg, is an element that binds to S and has the effect of suppressing the formation of MnS or the like that elongates in the rolling direction of the steel sheet. . Therefore, by adding REM, it is possible to control the morphology of the sulfide-based inclusions so as to exhibit a spherical shape and improve the toughness of welded joints and the like. In order to obtain the above effect, when REM is added, the REM content is preferably 0.0005% or more, more preferably 0.0015% or more.
- the REM content exceeds 0.0200%, the cleanliness of the steel is lowered and the HAZ toughness is lowered. Therefore, when REM is added, the REM content is made 0.0200% or less.
- the REM content is more preferably 0.0100% or less, even more preferably 0.0080% or less, and even more preferably 0.0050% or less.
- REM is scandium (Sc) with atomic number 21, yttrium (Y) with atomic number 39, and lanthanide elements from lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71. refers to
- the REM content is the total content of one or more elements selected from the above REMs.
- the steel sheet of the present invention has a total volume fraction of 90% or more of ferrite and pearlite at a quarter position in the plate thickness direction, and the grain size of the ferrite is 5 ⁇ m or more. It has a microstructure that is 20 ⁇ m or less. The reason for limiting the microstructure of steel as described above will be explained below.
- the total volume fraction of ferrite and pearlite at a position 1/4 of the plate thickness from the steel plate surface is 90% or more]
- the structure at the position of 1/4 of the thickness which represents the structure of the steel plate, is the yield strength (YS) of bainite, martensite, etc. become a high-ranking organization.
- hot rolling is controlled, and air cooling (radiation cooling) is performed without cooling after hot rolling, as in the steel sheet manufacturing method described later.
- the steel sheet satisfies predetermined strength characteristics and has improved low-temperature toughness.
- the total volume fraction of ferrite and pearlite is 90% or more in the structure at the position of 1/4 of the plate thickness.
- the ferrite is deformed and the yield strength (YS) is increased.
- Ferrites that have not been subjected (hereinafter ferrites) are clearly distinguished in the present invention. That is, ferrite as used in the present invention excludes processed ferrite.
- the steel material was mirror-polished, nital-etched to expose the structure, and observed with an SEM at a magnification of 500 to 3000 times.
- Ferrite is a structure that is isotropically grown and does not contain carbide, and the inside of the grain looks black.
- Pearlite is observed as a structure in which ferrite (white) and carbide (black) look like striped patterns (stripes).
- Bainite was defined as a structure having a lath-like ferrite structure grown elongated and containing carbides having an equivalent circle diameter of 0.05 ⁇ m or more.
- Martensite was defined as a structure having an elongated lath-like structure similar to bainite and containing carbides having an equivalent circle diameter of 0.05 ⁇ m or less. Note that the carbide looks like black dots.
- Austenite is defined as a non-carbide structure with an equivalent circle diameter of 0.50 ⁇ m or more, which exists between bainite or martensite structures.
- EBSD electron beam reflection diffraction
- the ferrite in the present invention has an average grain size of 20 ⁇ m or less in order to improve toughness at low temperatures.
- the average grain size of the ferrite is preferably 15 ⁇ m or less, more preferably 10 ⁇ m or less.
- the type is not particularly limited, but structures such as deformed ferrite, austenite, bainite, and martensite may be mixed, but the total volume fraction thereof should be less than 10%.
- the fraction of each structure in the residual structure does not need to be particularly limited, but from the viewpoint of toughness, it is preferable to avoid martensite, which is a microstructure with a large hardness difference from ferrite and pearlite. Bainite is preferred.
- the threshold value of 15° which is the threshold value for large-angle grain boundaries that are generally recognized as grain boundaries, is used, and the region tightly surrounded by grain boundaries with a crystal misorientation of 15° or more is visualized.
- the area average (Area fraction average) of ferrite was calculated.
- OIM Analysis software manufactured by TSL was used for the calculation.
- the obtained area-average grain size of ferrite was used as the average grain size of ferrite.
- a steel material having the chemical composition described above is heated and hot-rolled to form a hot-rolled steel sheet, which is then cooled to a starting temperature equal to or higher than the Ar 3 transformation point to form a steel sheet.
- the manufacturing conditions are described in detail below.
- the manufacturing conditions of the steel material are not particularly limited, but the molten steel having the above-described chemical composition is melted by a known melting method such as a converter, and is subjected to a known casting method such as a continuous casting method. Therefore, it is preferable to use a steel material such as a slab having a predetermined size. It should be noted that there is no problem in making a steel material such as a slab having a predetermined size by the ingot casting-decomposition rolling method.
- the obtained steel material is directly hot rolled without cooling, or once heated and then hot rolled. Hot rolling is performed at a temperature equal to or higher than the Ar 3 transformation point, and then air cooling (standing to cool) is started at a temperature equal to or higher than the Ar 3 transformation point.
- Heating temperature of steel material 950° C. or higher and 1250° C. or lower
- the heating temperature of the steel material is not particularly limited. The load on the steel increases, and hot rolling becomes difficult. On the other hand, when the temperature exceeds 1250° C., the oxidation becomes significant, the oxidation loss increases, and the yield decreases. For this reason, the heating temperature is preferably 950° C. or higher and 1250° C. or lower. In addition, it is more preferably 1000° C. or higher and 1150° C. or lower.
- Hot rolling start temperature Ar 3 transformation point + 200°C or higher After heating to the above temperature, hot rolling is performed. If the temperature at which rolling is started is less than the Ar 3 transformation point +200°C, it becomes difficult to achieve the hot rolling end temperature: the Ar 3 transformation point or higher, which will be described later, in a steel sheet having a thickness of less than 13 mm as the final product. Desired strength characteristics cannot be obtained. Therefore, the rolling start temperature is set to Ar 3 transformation point +200°C or higher. From the viewpoint of securing the time for rolling in the non-recrystallization temperature range described later, the rolling start temperature is preferably set to the Ar 3 transformation point +250°C or higher.
- the upper limit of the rolling start temperature should generally follow the above-described heating temperature of the steel material.
- the Ar 3 transformation point can be obtained by, for example, the following equation.
- Ar 3 (° C.) 910-273 ⁇ C-74 ⁇ Mn-57 ⁇ Ni-16 ⁇ Cr-9 ⁇ Mo ⁇ 5 ⁇ Cu
- each element symbol represents the content (% by mass) of each component, and is set to 0 when not contained.
- the rolling reduction per pass (hereinafter also referred to as rolling reduction / pass) is less than 10%, or the cumulative rolling reduction is less than 65% , a sufficient working effect on austenite cannot be obtained. If the austenite is not worked sufficiently, the ferrite will not be sufficiently finely grained by air cooling (standing to cool), which will be described later, and the desired low temperature toughness will not be obtained. Therefore, in the non-recrystallization temperature range, the rolling reduction per pass is set to 10% or more and the cumulative rolling reduction is set to 65% or more.
- the rolling reduction per pass is defined as a value obtained by dividing the cumulative rolling reduction by the total number of passes.
- the cumulative reduction ratio/pass in the non-recrystallized region is set to 20% or less.
- the cumulative rolling reduction in the non-recrystallized region is preferably 70% or more, more preferably 75% or more, in order to further improve toughness at low temperatures.
- the cumulative rolling reduction in the non-recrystallized region exceeds 80%, the load on the rolling mill becomes too large, so the cumulative rolling reduction in the non-recrystallized region is preferably 80% or less.
- Cooling start temperature Ar 3 transformation point or higher
- the hot-rolled steel sheet is cooled from the Ar 3 transformation point or higher.
- the cooling start temperature should be the Ar 3 transformation point or higher.
- Cooling method air cooling After hot rolling, air cooling (standing to cool) to room temperature is performed. This produces a predetermined microstructure. At this time, if cooling such as water cooling is performed, a predetermined microstructure cannot be obtained, and the desired strength characteristics cannot be satisfied. It is not possible to obtain a steel plate with good flatness in which the maximum value of the gap between the steel plate surface and the long length is 14 mm or less when they are brought into contact with each other.
- the cooling rate is 1.0° C./s to 5.0° C./s at the position of 1/4 of the plate thickness. In addition, when water cooling is performed, it becomes 50 degrees C/s or more.
- a steel sheet having the above-described structure can be obtained by manufacturing a steel material having the above-described chemical composition according to the above-described manufacturing method. The steel plate thus obtained has excellent strength characteristics, toughness and flatness, and is suitable for high heat input welding.
- the cooling rate can be calculated by (700 (°C) - 500 (°C))/cooling time (s) from 700°C to 500°C.
- the cooling end temperature is room temperature (not particularly limited, but for example -5 to 50°C).
- the steel sheets obtained were evaluated for chemical composition, strength characteristics, microstructure, base material toughness and flatness. Further, the obtained steel sheets were subjected to submerged arc welding as described below, and HAZ toughness was evaluated.
- a yield strength of 440 MPa or less was evaluated as a steel sheet with excellent ammonia stress corrosion cracking resistance, and a steel sheet with a tensile strength of 490 MPa or more was evaluated as a steel sheet with excellent tensile strength.
- Yield strength YS is closely related to ammonia stress corrosion cracking resistance, and as a structural member of a liquefied gas bulk carrier, the risk of ammonia stress corrosion cracking resistance is minimized according to the IMO gas code and ship classification regulations. Therefore, the yield point is defined as 440 MPa or less, and steel sheets with YS of 440 MPa or less were judged to be excellent in ammonia stress corrosion cracking resistance.
- HAZ toughness A 1 mm depth from the surface of the joint obtained by high heat input welding is used as the surface layer of the test piece, and FL (fusion line, fusion line), which is the boundary between the weld metal and HAZ, is included in the notch position. took a piece.
- a Charpy impact test was performed on the sampled test pieces at a test temperature of -55 ° C., and the average value vE-55 ° C. (unit: J) of the absorbed energy of three test pieces performed under the same conditions was obtained as the HAZ toughness. .
- the evaluation results thus obtained are also shown in Table 2.
- all of the invention examples have a yield strength YS of 440 MPa or less and a tensile strength TS of 490 MPa or more, the absorbed energy of the steel plate base material and HAZ at -55 ° C. is 100 J or more, and the flat A steel sheet with a flatness of 14 mm/2000 mm or less, excellent low-temperature toughness and resistance to ammonia stress corrosion cracking, and high flatness was obtained.
- the steel plate No. corresponding to the comparative example. 3, 4, 5, 6, and 7 differ from the invention examples in the microstructure or plate thickness of 1/4 of the plate thickness, and the yield strength YS, tensile strength TS, toughness of the base material at low temperature, or flatness are different. It is inferior to the invention example.
- any of the amount of addition of various elements, the stipulations for Ti and N, and Ceq are outside the upper or lower limits stipulated in the present invention, and the strength characteristics of the base material, the toughness of the base material, or the HAZ Inferior to either toughness.
Landscapes
- Chemical & Material Sciences (AREA)
- Engineering & Computer Science (AREA)
- Mechanical Engineering (AREA)
- Materials Engineering (AREA)
- Metallurgy (AREA)
- Organic Chemistry (AREA)
- Physics & Mathematics (AREA)
- Thermal Sciences (AREA)
- Crystallography & Structural Chemistry (AREA)
- Heat Treatment Of Steel (AREA)
Priority Applications (3)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| KR1020247024057A KR20240128014A (ko) | 2022-03-03 | 2023-02-09 | 강판 및 강판의 제조 방법 |
| JP2023526870A JP7323090B1 (ja) | 2022-03-03 | 2023-02-09 | 鋼板および鋼板の製造方法 |
| CN202380017504.1A CN118541503A (zh) | 2022-03-03 | 2023-02-09 | 钢板和钢板的制造方法 |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2022-032655 | 2022-03-03 | ||
| JP2022032655 | 2022-03-03 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2023166935A1 true WO2023166935A1 (ja) | 2023-09-07 |
Family
ID=87883370
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2023/004276 Ceased WO2023166935A1 (ja) | 2022-03-03 | 2023-02-09 | 鋼板および鋼板の製造方法 |
Country Status (4)
| Country | Link |
|---|---|
| JP (1) | JP7323090B1 (cg-RX-API-DMAC7.html) |
| KR (1) | KR20240128014A (cg-RX-API-DMAC7.html) |
| CN (1) | CN118541503A (cg-RX-API-DMAC7.html) |
| WO (1) | WO2023166935A1 (cg-RX-API-DMAC7.html) |
Families Citing this family (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN118745555B (zh) * | 2024-07-31 | 2026-01-09 | 鞍钢股份有限公司 | 一种优异低温性能移动罐车用压力容器钢板及其制造方法 |
Citations (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH11131178A (ja) * | 1997-10-23 | 1999-05-18 | Kobe Steel Ltd | 耐アンモニア応力腐食割れ性および大入熱溶接における熱影響部の靱性に優れた低降伏比型低温用鋼板 |
| JP2011105963A (ja) * | 2009-11-12 | 2011-06-02 | Nippon Steel Corp | 低温靭性の優れた低降伏比高張力鋼板の製造方法 |
| JP2019214752A (ja) * | 2018-06-12 | 2019-12-19 | 日本製鉄株式会社 | 低降伏比厚鋼板 |
| JP2020509174A (ja) * | 2016-12-22 | 2020-03-26 | ポスコPosco | 高強度高靭性厚鋼板及びその製造方法 |
| WO2020184683A1 (ja) * | 2019-03-14 | 2020-09-17 | 日本製鉄株式会社 | 鋼板およびその製造方法 |
Family Cites Families (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP3802626B2 (ja) | 1996-11-12 | 2006-07-26 | 新日本製鐵株式会社 | 溶接性および低温靭性の優れた低降伏比高張力鋼の製造方法 |
| JP3848415B2 (ja) | 1996-12-11 | 2006-11-22 | 新日本製鐵株式会社 | 溶接性および低温靭性の優れた低降伏比高張力鋼の製造方法 |
| JP5076658B2 (ja) | 2006-12-06 | 2012-11-21 | Jfeスチール株式会社 | 大入熱溶接用鋼材 |
| JP4897126B2 (ja) | 2010-05-27 | 2012-03-14 | 新日本製鐵株式会社 | 厚鋼板の製造方法 |
| JP5713135B1 (ja) | 2013-11-19 | 2015-05-07 | 新日鐵住金株式会社 | 鋼板 |
-
2023
- 2023-02-09 KR KR1020247024057A patent/KR20240128014A/ko active Pending
- 2023-02-09 WO PCT/JP2023/004276 patent/WO2023166935A1/ja not_active Ceased
- 2023-02-09 JP JP2023526870A patent/JP7323090B1/ja active Active
- 2023-02-09 CN CN202380017504.1A patent/CN118541503A/zh active Pending
Patent Citations (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH11131178A (ja) * | 1997-10-23 | 1999-05-18 | Kobe Steel Ltd | 耐アンモニア応力腐食割れ性および大入熱溶接における熱影響部の靱性に優れた低降伏比型低温用鋼板 |
| JP2011105963A (ja) * | 2009-11-12 | 2011-06-02 | Nippon Steel Corp | 低温靭性の優れた低降伏比高張力鋼板の製造方法 |
| JP2020509174A (ja) * | 2016-12-22 | 2020-03-26 | ポスコPosco | 高強度高靭性厚鋼板及びその製造方法 |
| JP2019214752A (ja) * | 2018-06-12 | 2019-12-19 | 日本製鉄株式会社 | 低降伏比厚鋼板 |
| WO2020184683A1 (ja) * | 2019-03-14 | 2020-09-17 | 日本製鉄株式会社 | 鋼板およびその製造方法 |
Also Published As
| Publication number | Publication date |
|---|---|
| CN118541503A (zh) | 2024-08-23 |
| KR20240128014A (ko) | 2024-08-23 |
| JPWO2023166935A1 (cg-RX-API-DMAC7.html) | 2023-09-07 |
| JP7323090B1 (ja) | 2023-08-08 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| JP7147960B2 (ja) | 鋼板およびその製造方法 | |
| JP6631353B2 (ja) | 耐サワー鋼板及び耐サワー鋼管 | |
| JP7099653B1 (ja) | 鋼板およびその製造方法 | |
| JP7077801B2 (ja) | 低降伏比厚鋼板 | |
| JP2010202931A (ja) | 脆性亀裂伝播停止特性に優れた構造用高強度厚鋼板およびその製造方法 | |
| EP3378962B1 (en) | High heat input welded steel material | |
| WO2014175122A1 (ja) | H形鋼及びその製造方法 | |
| WO2021020220A1 (ja) | 耐サワーラインパイプ用高強度鋼板およびその製造方法並びに耐サワーラインパイプ用高強度鋼板を用いた高強度鋼管 | |
| EP3533891A1 (en) | Steel for high heat input welding | |
| KR102889835B1 (ko) | 고강도 강판 및 그 제조 방법 | |
| JP7323091B1 (ja) | 鋼板およびその製造方法 | |
| CN115210400B (zh) | 钢材及其制造方法、以及罐 | |
| JP2017110249A (ja) | 耐サワー鋼板 | |
| JP7323090B1 (ja) | 鋼板および鋼板の製造方法 | |
| KR20230125288A (ko) | 강재 및 그 제조 방법, 탱크 및 그 제조 방법 | |
| JP7444339B1 (ja) | 大入熱溶接用鋼板およびその製造方法 | |
| JP7243916B2 (ja) | 鋼板および鋼板の製造方法 | |
| WO2022045351A1 (ja) | 鋼板およびその製造方法 | |
| JP7700972B2 (ja) | 鋼板およびその製造方法 | |
| KR20160121712A (ko) | 초대입열 용접용 강판의 제조 방법과 이에 의해 제조된 초대입열 용접용 강판 | |
| JP7468814B1 (ja) | 高強度極厚鋼板およびその製造方法 | |
| JP7396322B2 (ja) | 鋼板 | |
| JP2025178632A (ja) | 鋼板およびその製造方法 | |
| JP2025031575A (ja) | 鋼板およびその製造方法 | |
| WO2025022587A1 (ja) | 鋼板およびその製造方法 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| WWE | Wipo information: entry into national phase |
Ref document number: 2023526870 Country of ref document: JP |
|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 23763197 Country of ref document: EP Kind code of ref document: A1 |
|
| ENP | Entry into the national phase |
Ref document number: 20247024057 Country of ref document: KR Kind code of ref document: A |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 202380017504.1 Country of ref document: CN |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| 122 | Ep: pct application non-entry in european phase |
Ref document number: 23763197 Country of ref document: EP Kind code of ref document: A1 |